Buffer block for ship hatch cover and preparation method thereof

By designing thermoplastic composite cushion blocks with a continuous non-layered structure, the problems of insufficient compressive strength and environmental pollution of cushion blocks in the existing technology are solved, achieving high cost performance and improved performance, and are suitable for use in ship hatch covers.

CN116118084BActive Publication Date: 2024-10-22CSSC HUAHAI MARINE EQUIP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310189534.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-02
Publication Date
2024-10-22
Estimated Expiration
2043-03-02

AI Technical Summary

Technical Problem

The existing buffer pads used for ship hatch covers have problems such as insufficient compressive strength and modulus, easy deformation, low processing efficiency, high cost and environmental pollution. In particular, the thermosetting composite buffer pads have insufficient lateral pressure bearing capacity and Hazardous gas emissions during chemical preparation processes.

Method used

Design a continuous non-layered thermoplastic composite cushion block including a bottom section, a lower buffer section, a high-strength section and a surface section. It is formed by hot pressing and melting to improve the bending strength and lateral compression strength, and to achieve self-lubricating on the surface and bottom. Self-balancing, using physical preparation process and green technology, optimizing material composition to overcome the shortcomings of traditional cushion blocks.

Benefits of technology

It achieves higher load-bearing capacity and performance uniformity, improves bending strength and lateral compression strength, is highly cost-effective, and reduces environmental pollution through green processes, making it suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a buffer pad for a ship hatch cover and a preparation method thereof, wherein the buffer pad comprises a pad body, wherein the pad body comprises a bottom section, a lower buffer section, a high-strength section, an upper buffer section and a surface section, and the bottom section, the lower buffer section, the high-strength section, the upper buffer section and the surface section are a continuous non-layered combination. In the present invention, the provided buffer pad realizes self-lubrication on the surface of the buffer pad and self-balancing at the bottom through the provision of the bottom section, the lower buffer section, the upper buffer section, the high-strength section and the surface section, so that the buffer pad has a higher overall bearing capacity, and the performance is uniformly transitioned, with high cost performance, and is suitable for wide promotion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of design of buffer pads for ships, and relates to a buffer pad for a ship hatch cover and a preparation method thereof. Background Art

[0002] Buffer pads are an important component of the deck of large ships, especially large container ships. They are located between the ship's hatch coaming and hatch cover, and play the role of bearing the weight of the hatch cover itself and even the weight of several layers of large containers to protect the hatch coaming. When the ship shakes, the hatch cover can produce a certain displacement on its surface to stabilize and buffer the container layer or even the ship itself.

[0003] Traditional metal buffer blocks, such as the classic tin bronze buffer blocks, are expensive, highly corrosive to seawater, and are often easily lost. Most of them have been replaced by non-metal buffer blocks, because thermoplastic engineering plastic buffer blocks and thermosetting composite buffer blocks can well overcome the defects of metal buffer blocks and achieve better results. However, non-metal buffer blocks still show some insurmountable performance defects. For example, although thermoplastic engineering plastic buffer blocks have high manufacturing efficiency and low cost, their compression strength and modulus are not high enough, they are easy to deform, have a short service life, and need to be replaced frequently. The compressive strength and modulus of thermosetting composite buffer pads are several times higher than those of thermoplastic engineering plastic buffer pads, but the layered structure of the reinforced fabric results in the lateral pressure bearing capacity being only one-third of that in the forward direction. The buffer pad is installed in a buffer pad box with the upper part exposed to the box surface, and there will also be high lateral pressure and shear force, especially shear force parallel to the box surface, which is very unfavorable for the layered structure of the reinforced fabric of the buffer pad, and the processing efficiency is low and the cost is high. In particular, the chemical preparation process will release harmful gases and pollute the environment.

[0004] Therefore, it is urgent to design and develop a buffer pad for ship hatch covers to overcome the defects of the existing technology and meet the needs of actual industrial applications. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a buffer pad block for ship hatch covers and a preparation method thereof. In the present invention, the provided buffer pad block has a designed bottom section, a lower buffer section, a high-strength section, an upper buffer section and a surface section, so that the surface of the buffer pad block is self-lubricating and the bottom is self-balancing, and has a higher bearing capacity, and the performance is uniformly transitioned, with high cost performance, and is suitable for wide promotion.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a buffer pad for a ship hatch cover, the buffer pad comprising a pad body, the pad body comprising a bottom layer section, a lower buffer section, a high-strength section, an upper buffer section and a surface layer section, and the bottom layer section, the lower buffer section, the high-strength section, the upper buffer section and the surface layer section are a continuous non-layered combination.

[0008] In the present invention, the buffer pad block provided has self-lubricating surface and self-balancing bottom through the designed bottom layer section, lower buffer section, high-strength section, upper buffer section and surface layer section, has higher bearing capacity, uniform performance transition, high cost performance, and is suitable for wide promotion.

[0009] It should be noted that the "continuous non-layered combination" in the present invention means that the bottom layer segment, lower buffer segment, high-strength segment, upper buffer segment and surface layer segment are obtained by a preparation method of a large number of thin sheet raw materials of different compositions through hot pressing and melting, cooling and solidification molding. The buffer pad is a thermoplastic composite buffer pad with a complete and continuous structure and multiple functions in one, and has a complete structure and different composition distribution, thereby forming different functions to adapt to different working environments; further, the buffer pad of the present invention has a bending strength of 300% relative to the fabric reinforced buffer pad, and a lateral compression strength of 200% relative to the fabric reinforced buffer pad, which overcomes the insurmountable defects of the fabric layered reinforced buffer pad; and realizes the self-balancing adjustment function.

[0010] As a preferred technical solution of the present invention, the material of the bottom layer segment is a mixture of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp.

[0011] Preferably, the mass ratio of the polypropylene, polyethylene-octene co-elastomer, continuous long glass fiber and aramid pulp is (7-8):1:(11-12):1, for example, it can be 7:1:12:1, 7:1:11:1, 7:1:11.5:1, 8:1:12:1, 8:1:11:1, 8:1:11.5:1, 7.5:1:12:1, 7.5:1:11:1, 8.5:1:12:1, 7.5:1:11:1, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; more preferably, it is 7:1:12:1.

[0012] The present invention limits the mass ratio of the polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp in the bottom layer segment to (7-8):1:(11-12):1, because within this numerical range, the bottom layer segment can have a certain degree of property deformation under heavy load in the working environment and achieve self-balancing. If it is not within the limited range of the present invention, the buffer pad will lose its self-balancing performance.

[0013] As a preferred technical solution of the present invention, the material of the lower buffer section is a mixture of polypropylene, continuous long glass fibers and aramid pulp.

[0014] Preferably, the mass ratio of the polypropylene, continuous long glass fiber and aramid pulp is (7-8):(11-12):1, for example, it can be 7:12:1, 7:11:1, 7:11.5:1, 8:11:1, 8:12:1, 7:11.5:1, 7.5:12:1, 8.5:12:1, 7.5:11:1, 8.5:11:1, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; more preferably, it is 7:12:1.

[0015] The present invention limits the mass ratio of the polypropylene, continuous long glass fiber and aramid pulp in the lower buffer section to (7-8):(11-12):1, because within this numerical range, the structure and performance of the high-strength section and the bottom section can be smoothly transitioned. If it is not within the limited range of the present invention, it will lead to a sudden change in the structure and performance of the surface section and the high-strength section, forming a layered structure.

[0016] As a preferred technical solution of the present invention, the material of the high-strength section is a mixture of polypropylene, continuous long glass fibers and aramid pulp.

[0017] Preferably, the mass ratio of the polypropylene, continuous long glass fiber and aramid pulp is (6-7):(13-14):1, for example, it can be 6:13:1, 6:14:1, 6:13.5:1, 7:13:1, 7:14:1, 7:13.5:1, 6.5:13:1, 7.5:13:1, 6.5:13.5:1, 7.5:13.5:1, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; more preferably, it is 6:13:1.

[0018] The present invention limits the mass ratio of the polypropylene, continuous long glass fiber and aramid pulp in the high-strength section to (6-7):(13-14):1, because within this numerical range the buffer block can have the designed supporting capacity. If it is not within the limited range of the present invention, it will cause damage to the buffer block.

[0019] As a preferred technical solution of the present invention, the material of the upper buffer section is a mixture of polypropylene, continuous long glass fibers and aramid pulp.

[0020] Preferably, the mass ratio of the polypropylene, continuous long glass fiber and aramid pulp is (7-8):(11-12):1, for example, it can be 7:12:1, 7:11:1, 7:11.5:1, 8:11:1, 8:12:1, 7:11.5:1, 7.5:12:1, 8.5:12:1, 7.5:11:1, 8.5:11:1, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; more preferably, it is 7:12:1.

[0021] The present invention limits the mass ratio of the polypropylene, continuous long glass fiber and aramid pulp in the upper buffer section to (7-8):(11-12):1, because within this numerical range, the structure and performance of the surface section and the high-strength section can be smoothly transitioned. If it is not within the limited range of the present invention, it will lead to a sudden change in the structure and performance of the surface section and the high-strength section, forming a layered structure.

[0022] As a preferred technical solution of the present invention, the material of the surface layer section is a mixture of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp.

[0023] Preferably, the mass ratio of the polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp is (6-7):(10-11):(3-4):1, for example, it can be 6:10:3:1, 6:11:3:1, 6:10:4:1, 6:11:4:1, 7:10:3:1, 7:11:3:1, 7:10:4:1, 7:11:4:1, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; more preferably, it is 6:10:3:1.

[0024] The present invention limits the mass ratio of the polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp in the surface layer segment to (6-7):(10-11):(3-4):1. This is because within this numerical range, the surface layer segment can have self-lubricating properties under heavy loads in the working environment and play a buffering role as a pad. If it is not within the limited range of the present invention, the buffer pad will lose its buffering function.

[0025] As a preferred technical solution of the present invention, the thickness of the pad body is 28 to 30 mm, for example, it can be 28 mm, 28.2 mm, 28.4 mm, 28.6 mm, 28.8 mm, 29 mm, 29.2 mm, 29.4 mm, 29.6 mm, 29.8 mm, 30 mm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the width of the pad body is 70-80 mm, for example, it can be 70 mm, 71 mm, 72 mm, 73 mm, 74 mm, 75 mm, 76 mm, 77 mm, 78 mm, 79 mm, 80 mm, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the length of the pad body is 200-220 mm, for example, it can be 200 mm, 202 mm, 204 mm, 206 mm, 208 mm, 210 mm, 212 mm, 214 mm, 216 mm, 218 mm, 220 mm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] The present invention limits the thickness of the cushion block body to 28-30 mm, the width to 70-80 mm and the length to 200-220 mm, because within this numerical range the buffer cushion block can achieve the designed bearing capacity and has a certain degree of installation adjustability.

[0029] As a preferred technical solution of the present invention, the positive compression strength of the buffer pad is 280-360MPa, for example, it can be 280MPa, 300MPa, 320MPa, 340MPa, 360MPa, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the side compression strength of the buffer pad is 200-250 MPa, for example, it can be 200 MPa, 210 MPa, 220 MPa, 230 MPa, 240 MPa, 250 MPa, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the bending strength of the buffer pad is 280-300 MPa, for example, it may be 280 MPa, 282 MPa, 284 MPa, 286 MPa, 288 MPa, 290 MPa, 292 MPa, 294 MPa, 296 MPa, 298 MPa, 300 MPa, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the friction coefficient of the buffer pad is less than 0.04, for example, it can be 0.039, 0.035, 0.03, 0.028, 0.02, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] It should be noted that the friction coefficient detection method in the present invention adopts the Ever / East method, which is well known to those skilled in the art. The test shows that the friction coefficient of the buffer pad is less than 0.04, and the maximum tilt deformation of the bottom layer under a load of 70MPa is 1.5mm.

[0034] In a second aspect, the present invention provides a method for preparing the buffer pad according to the first aspect, the preparation method comprising:

[0035] The bottom layer segment, the lower buffer segment, the high-strength segment and the surface layer segment are stacked in sequence in a mold, hot-pressed and melted, and solidified to obtain the buffer pad.

[0036] It should be noted that the preparation method in the present invention can be: polypropylene composite sheet with different compositions, the sheet thickness is 0.5-0.7mm, stacked in a mold in sequence, hot pressed and melted, solidified to obtain the buffer pad, and the buffer pad is a complete but non-layered structure. For the preparation method of the buffer pad, when the raw material sheets of the bottom layer section, the lower buffer section, the high-strength section, the upper buffer section and the surface layer section are stacked in sequence in the mold, the superposition of each structure is layered, but the buffer pad obtained after the hot pressing and melting and solidification treatment method is a non-layered structure, a thermoplastic composite buffer pad with a complete and continuous structure and multiple functions, and its functions include surface self-lubrication, bottom self-balancing, high load-bearing, uniform performance transition, high cost performance, and a green preparation process (the preparation method is a physical process throughout, green, environmentally friendly, and overcomes the preparation defects of thermosetting reinforced buffer pads); wherein the low-priced general-purpose plastic polypropylene is used as the matrix and the above composite modification is used to obtain mechanical properties similar to those of aluminum alloy materials, reflecting the high cost performance of the product.

[0037] As a preferred technical solution of the present invention, the temperature of the hot pressing melting is 220-230°C, for example, it can be 220°C, 221°C, 222°C, 223°C, 224°C, 225°C, 226°C, 227°C, 228°C, 229°C, 230°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] The present invention limits the temperature of hot pressing melting to 220-230°C because within this numerical range, the material matrix can be completely melted, but the components of each layer do not change. If it is not within the limited range of the present invention, it will cause incomplete melting of the material matrix or flow between components.

[0039] Preferably, the solidification molding temperature is 30-40°C, for example, it can be 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 50°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] It should be noted that in the present invention, the hot pressing and melting adopts a plastic press device, and the solidification molding adopts a plastic press device, which are all well-known contents to those skilled in the art.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] In the present invention, the buffer block provided has a bottom section, a lower buffer section, a high-strength upper buffer layer and a surface section, so that the surface of the buffer block is self-lubricating and the bottom is self-balanced, and has a higher bearing capacity, and the performance is uniformly transitioned, with high cost performance, and is suitable for wide promotion. DETAILED DESCRIPTION

[0043] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0044] In a specific embodiment, the present invention provides a buffer pad for a ship hatch cover, wherein the buffer pad includes a pad body, the pad body includes a bottom layer section, a lower buffer section, a high-strength section, an upper buffer section and a surface layer section, and the bottom layer section, the lower buffer section, the high-strength section, the upper buffer section and the surface layer section are a continuous non-layered combination.

[0045] In the present invention, the buffer pad block provided has a bottom layer section, a lower buffer section, a high-strength section, an upper buffer section and a surface layer section, so that the surface of the buffer pad block is self-lubricating and the bottom is self-balanced, and has a higher bearing capacity, and the performance is uniformly transitioned, with high cost performance, and is suitable for wide promotion.

[0046] It should be noted that the "continuous non-layered combination" in the present invention refers to the raw material sheets of the bottom layer segment, the lower buffer segment, the high-strength segment, the upper buffer layer and the surface layer segment stacked in layers, but the buffer pad obtained after the hot pressing melting and solidification molding process is a non-layered structure, a complete and continuous structure, and a multifunctional thermoplastic composite buffer pad; further, the buffer pad of the present invention has a bending strength of 300% relative to the fabric reinforced buffer pad, and a lateral compression strength of 200% relative to the fabric reinforced buffer pad, which overcomes the insurmountable defects of the fabric layered reinforced buffer pad; and realizes the self-balancing adjustment function.

[0047] The material of the bottom layer section is a mixture of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp. The mass ratio of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp is (7-8):1:(11-12):1, for example, it can be 7:1:12:1, 7:1:11:1, 7:1:11.5:1, 8:1:12:1, 8:1:11:1, 8:1:11.5:1, 7.5:1:12:1, 7.5:1:11:1, 8.5:1:12:1, 7.5:1:11:1, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, it is 7:1:12:1. The material of the lower buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is (7-8):(11-12):1, for example, it can be 7:12:1, 7:11:1, 7:11.5:1, 8:11:1, 8:12:1, 7:11.5:1, 7.5:12:1, 8.5:12:1, 7.5:11:1, 8.5:11:1, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, it is 7:12:1.

[0048] The material of the high-strength section is a mixture of polypropylene, continuous long glass fiber and aramid pulp. The mass ratio of polypropylene, continuous long glass fiber and aramid pulp is (6-7):(13-14):1, for example, it can be 6:13:1, 6:14:1, 6:13.5:1, 7:13:1, 7:14:1, 7:13.5:1, 6.5:13:1, 7.5:13:1, 6.5:13.5:1, 7.5:13.5:1, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, it is 6:13:1.

[0049] The material of the upper buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is (7-8):(11-12):1, for example, it can be 7:12:1, 7:11:1, 7:11.5:1, 8:11:1, 8:12:1, 7:11.5:1, 7.5:12:1, 8.5:12:1, 7.5:11:1, 8.5:11:1, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, it is 7:12:1.

[0050] The material of the surface layer section is a mixture of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp. The mass ratio of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp is (6-7): (10-11): (3-4): 1, for example, it can be 6:10:3:1, 6:11:3:1, 6:10:4:1, 6:11:4:1, 7:10:3:1, 7:11:3:1, 7:10:4:1, 7:11:4:1, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; further, it is 6:10:3:1.

[0051] The thickness of the pad body is 28-30 mm, for example, it can be 28 mm, 28.2 mm, 28.4 mm, 28.6 mm, 28.8 mm, 29 mm, 29.2 mm, 29.4 mm, 29.6 mm, 29.8 mm, 30 mm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] The width of the pad body is 70-80mm, for example, it can be 70mm, 71mm, 72mm, 73mm, 74mm, 75mm, 76mm, 77mm, 78mm, 79mm, 80mm, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] The length of the pad body is 200-220mm, for example, it can be 200mm, 202mm, 204mm, 206mm, 208mm, 210mm, 212mm, 214mm, 216mm, 218mm, 220mm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] The positive compression strength of the buffer pad is 260-280 MPa, for example, it can be 260 MPa, 262 MPa, 264 MPa, 266 MPa, 268 MPa, 270 MPa, 272 MPa, 274 MPa, 276 MPa, 278 MPa, 280 MPa, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] The side compression strength of the buffer pad is 180-200 MPa, for example, it can be 180 MPa, 182 MPa, 184 MPa, 186 MPa, 188 MPa, 190 MPa, 192 MPa, 194 MPa, 196 MPa, 198 MPa, 200 MPa, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0056] The bending strength of the buffer pad is 280-300 MPa, for example, it can be 280 MPa, 282 MPa, 284 MPa, 286 MPa, 288 MPa, 290 MPa, 292 MPa, 294 MPa, 296 MPa, 298 MPa, 300 MPa, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] The friction coefficient of the buffer pad is less than 0.04, for example, it can be 0.039, 0.035, 0.03, 0.028, 0.02, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] It should be noted that the friction coefficient detection method in the present invention adopts the Ever / East method, which is well known to those skilled in the art. The test shows that the friction coefficient of the buffer pad is less than 0.04, and the maximum tilt deformation of the bottom layer under a load of 70MPa is 1.5mm.

[0059] In another specific embodiment, the present invention provides a method for preparing the buffer pad, the method comprising:

[0060] The raw material sheets of the bottom layer section, the lower buffer section, the high-strength section, the upper buffer section and the surface layer section are stacked in sequence in a mold, hot-pressed and melted, and solidified to obtain a buffer pad, and the buffer pad is a complete rather than layered structure.

[0061] It should be noted that, in the preparation method of the buffer pad in the present invention, when the raw material sheets of the bottom layer section, the lower buffer section, the high-strength section, the upper buffer section and the surface layer section are stacked in sequence in a mold, the superposition of each structure presents a layered shape, but the buffer pad obtained after the hot pressing melting and solidification molding treatment method is a non-layered structure, a complete and continuous structure, and a multifunctional thermoplastic composite buffer pad. Its functions include bottom self-balancing, higher load-bearing, uniform performance transition, high cost performance, and a green preparation process (the preparation method is a physical process throughout, which is green and environmentally friendly, and overcomes the preparation defects of thermosetting reinforced buffer pads); wherein the low-cost general-purpose plastic polypropylene is used as the matrix and the above composite modification is performed to obtain mechanical properties similar to those of aluminum alloy materials, reflecting the high cost performance of the product.

[0062] The temperature of hot pressing and melting is 220-230°C, for example, it can be 220, 221, 222, 223, 224, 225, 226, 227, 228, 229, 230, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; the temperature of solidification molding is 30-40°C.

[0063] Example 1

[0064] This embodiment provides a buffer pad for a ship hatch cover and a preparation method thereof, wherein:

[0065] The buffer block comprises a block body, which comprises a bottom layer section, a lower buffer section, a high-strength section, an upper buffer section and a surface layer section, and the bottom layer section, the lower buffer section, the high-strength section, the upper buffer section and the surface layer section are a continuous non-layered combination.

[0066] The material of the bottom section is a mixture of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp is 7:1:11:1. The material of the lower buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 7:11:1. The material of the high-strength section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 6:13:1. The material of the upper buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 7:11:1.

[0067] The material of the surface layer is a mixture of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp. The mass ratio of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp is 6:10:3:1. The thickness of the pad body is 28mm; the width of the pad body is 70mm; the length of the pad body is 200mm. The positive compression strength of the buffer pad is 260MPa, the side compression strength of the buffer pad is 180MPa, the bending strength of the buffer pad is 280MPa, and the friction coefficient of the buffer pad is 0.035.

[0068] The preparation method comprises: placing the raw material sheets of the bottom layer section, the lower buffer section, the high-strength upper buffer section and the surface layer section in a mold in sequence, hot pressing and melting, and solidifying and forming to obtain a buffer pad, and the buffer pad is a continuous non-layered structure. The temperature of hot pressing and melting is 220°C; the temperature of solidification and forming is 30°C.

[0069] Example 2

[0070] This embodiment provides a buffer pad for a ship hatch cover and a preparation method thereof, wherein:

[0071] The buffer pad comprises a pad body, which comprises a bottom layer section, a lower buffer section, a high-strength section and a surface layer section, and the bottom layer section, the lower buffer section, the high-strength section and the surface layer section are a continuous non-layered combination.

[0072] The material of the bottom section is a mixture of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp is 7.5:1:11:1. The material of the lower buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 7.5:11:1. The material of the high-strength section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 6.5:13:1. The material of the upper buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 7.5:12:1.

[0073] The material of the surface layer is a mixture of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp. The mass ratio of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp is 6.5:10.5:3:1. The thickness of the pad body is 29mm; the width of the pad body is 75mm; the length of the pad body is 210mm. The positive compression strength of the buffer pad is 300MPa, the side compression strength of the buffer pad is 190MPa, the bending strength of the buffer pad is 290MPa, and the friction coefficient of the buffer pad is 0.032.

[0074] The preparation method comprises: placing the raw material sheets of the bottom layer section, the lower buffer section, the high-strength section and the surface layer section in a mold in sequence, hot pressing and melting, and solidifying and forming to obtain a buffer pad, and the buffer pad is a continuous non-layered structure. The temperature of hot pressing and melting is 225°C; the temperature of solidification and forming is 35°C.

[0075] Example 3

[0076] This embodiment provides a buffer pad for a ship hatch cover and a preparation method thereof, wherein:

[0077] The buffer pad comprises a pad body, which comprises a bottom layer section, a lower buffer section, a high-strength section and a surface layer section, and the bottom layer section, the lower buffer section, the high-strength section and the surface layer section are a non-layered combination.

[0078] The material of the bottom section is a mixture of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp is 8:1:12:1. The material of the lower buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 8:12:1. The material of the high-strength section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 7:14:1. The material of the upper buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber and aramid pulp is 8:12:2.

[0079] The material of the surface layer section is a mixture of polypropylene, continuous long glass fiber, needle-shaped wollastonite and aramid pulp, and the mass ratio of polypropylene, continuous long glass fiber, needle-shaped wollastonite and aramid pulp is 7:11:8:1.

[0080] The thickness of the pad body is 28mm, the width of the pad body is 70mm, and the length of the pad body is 200mm. The positive compression strength of the buffer pad is 360MPa, the side compression strength of the buffer pad is 250MPa, and the bending strength of the buffer pad is 300MPa.

[0081] The preparation method comprises: placing the raw material sheets of the bottom layer section, the lower buffer section, the high-strength section, the upper buffer section and the surface layer section in a mold in sequence, hot pressing and melting, and solidifying and forming to obtain a buffer pad, and the buffer pad is a continuous non-layered structure. The temperature of hot pressing and melting is 230°C; the temperature of solidification and forming is 40°C.

[0082] Compared with the thermosetting buffer blocks that are currently in widespread use, the buffer blocks of Examples 1-3 are transformed from thermosetting materials to thermoplastic materials, and the structure is transformed from layered reinforcement to continuous reinforcement, and the overall structure is non-layered and continuous. The preparation method is transformed from chemical process to physical process, realizing green production and multi-functions. A breakthrough in performance is achieved, with the maximum front compressive strength increased from 280 MPa to 360 MPa, the maximum side compressive strength increased from 90 MPa to 250 MPa, and the bending strength increased from 100 MPa to 300 MPa, reaching the level of aluminum alloy.

[0083] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A buffer pad for a ship hatch cover, characterized in that: The buffer block comprises a block body, and the block body comprises a bottom layer section, a lower buffer section, a high-strength section, an upper buffer section and a surface layer section, and the bottom layer section, the lower buffer section, the high-strength section, the upper buffer section and the surface layer section are a continuous non-layered combination; The continuous non-layered combination refers to a layered structure formed by stacking the raw material sheets of the bottom layer section, the lower buffer section, the high-strength section, the upper buffer layer and the surface layer section, but the buffer pad obtained by the hot pressing, melting and solidification molding method is a non-layered, complete and continuous structure of a thermoplastic composite buffer pad with multiple functions. The material of the bottom layer section is a mixture of polypropylene, polyethylene octene copolymer elastomer, continuous long glass fiber and aramid pulp; The mass ratio of the polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp is (7-8):1:(11-12):1; The material of the lower buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp; The mass ratio of the polypropylene, the continuous long glass fiber and the aramid pulp is (7-8):(11-12):1; The material of the high-strength section is a mixture of polypropylene, continuous long glass fiber and aramid pulp; The mass ratio of the polypropylene, the continuous long glass fiber and the aramid pulp is (6-7):(13-14):1; The material of the upper buffer section is a mixture of polypropylene, continuous long glass fiber and aramid pulp; The mass ratio of the polypropylene, the continuous long glass fiber and the aramid pulp is (7-8):(11-12):1; The material of the surface layer section is a mixture of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp; The mass ratio of the polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp is (6-7):(10-11):(3-4):

1.

2. The buffer pad according to claim 1, characterized in that: The mass ratio of polypropylene, polyethylene octene co-elastomer, continuous long glass fiber and aramid pulp in the bottom layer section is 7:1:12:

1.

3. The buffer pad according to claim 1, characterized in that: The mass ratio of polypropylene, continuous long glass fiber and aramid pulp in the lower buffer section is 7:12:

1.

4. The buffer pad according to claim 1, characterized in that: The mass ratio of polypropylene, continuous long glass fiber and aramid pulp in the high-strength section is 6:13:

1.

5. The buffer pad according to claim 1, characterized in that: The mass ratio of polypropylene, continuous long glass fiber and aramid pulp in the upper buffer section is 7:12:

1.

6. The buffer pad according to claim 1, characterized in that: The mass ratio of polypropylene, continuous long glass fiber, polytetrafluoroethylene and aramid pulp in the surface layer section is 6:10:3:

1.

7. The buffer pad according to claim 1, characterized in that: The thickness of the pad body is 28-30 mm.

8. The buffer pad according to claim 1, characterized in that: The width of the pad body is 70-80 mm.

9. The buffer pad according to claim 1, characterized in that: The length of the cushion block body is 200-220 mm.

10. The buffer pad according to claim 1, characterized in that: The positive compression strength of the buffer pad is 280~360MPa.

11. The buffer pad according to claim 1, characterized in that: The side compression strength of the buffer pad is 200-250 MPa.

12. The buffer pad according to claim 1, characterized in that: The bending strength of the buffer pad is 280-300 MPa.

13. The buffer pad according to claim 1, characterized in that: The friction coefficient of the buffer pad is less than 0.

04.

14. A method for preparing a buffer pad according to any one of claims 1 to 13, characterized in that: The preparation method comprises: The bottom layer segment, the lower buffer segment, the high-strength segment, the upper buffer segment and the surface layer segment are stacked in sequence in a mold, hot-pressed and melted, and solidified to obtain the buffer pad, which has a non-layered structure.

15. The preparation method according to claim 14, characterized in that: The temperature of the hot pressing and melting is 220-230°C.

16. The preparation method according to claim 14, characterized in that: The solidification temperature is 30-40°C.

Citation Information