Ultra-high fluidity thermoplastic elastomer for automotive parts and preparation method thereof
The ultra-high fluidity thermoplastic elastomer prepared through a specific proportion and a two-step extrusion process solves the problem of poor fluidity of existing thermoplastic elastomers in automotive interior parts and achieves high fluidity, weather resistance and improved strength. , suitable for industrial production of auto parts.
Patent Information
- Application Number
- CN202211705349.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-29
AI Technical Summary
Existing thermoplastic elastomers have poor fluidity in automotive interior parts, are difficult to replace raw materials with high carbon emissions, and have insufficient mechanical properties and weather resistance.
Specific materials using EPDM rubber, polyolefin resin, thermoplastic elastomer, plasticizer, filler, anti-scratch agent, cross-linking agent, co-cross-linking agent, lubricant, antioxidant, light stabilizer and other materials The proportion and two-step extrusion process are used to prepare ultra-high fluidity thermoplastic elastomer to improve its fluidity, weather resistance and strength.
The ultra-high fluidity thermoplastic elastomer used in automobile parts has been realized. It has excellent weather resistance and strength, has stable process and low cost, and is suitable for large-scale industrial production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermoplastic elastomer materials, in particular to an ultra-high fluidity thermoplastic elastomer for automobile parts and a preparation method thereof. Background Art
[0002] Thermoplastic elastomers are a type of high-performance composite material with physical properties between plastic and rubber. They are easy to process and have the elasticity of rubber, and are known as the "third generation of rubber". This material has the functionality of vulcanized rubber at room temperature, and the plasticity and repeated processability of thermoplastics at high temperatures. Compared with traditional thermosetting rubbers, thermoplastic elastomers have the advantages of simple molding, energy-saving processing equipment, high cost performance, and recyclable materials and nozzle materials. While meeting the functions, appearance, and touch, they also have significant advantages in energy saving and environmental protection. With the widespread application of thermoplastic elastomers in the automotive industry, building materials and home furnishings, electronic appliances, medical and health care, and consumer products, rubber products other than pneumatic tires are seeking to use thermoplastic elastomers as substitutes.
[0003] At the same time, the requirements for the application scope of thermoplastic elastomers to replace traditional automotive interior materials are gradually increasing. At present, there are a large number of cases where thermoplastic elastomer materials are used in automotive interior products. However, most thermoplastic elastomer materials have poor fluidity, and a very small amount of thermoplastic elastomers with slightly higher fluidity have poor mechanical properties or poor weather resistance. In order to apply thermoplastic elastomers in some thin-walled, large-area automotive interior parts with higher fluidity, weather resistance and strength requirements, they are usually limited by fluidity and difficult to replace existing high-carbon emission raw materials.
[0004] Therefore, an ultra-high fluidity thermoplastic elastomer applied to automotive parts is proposed to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide an ultra-high fluidity thermoplastic elastomer for automotive parts; the thermoplastic elastomer has ultra-high fluidity as well as excellent weather resistance and strength, so as to solve the requirements of the existing central thermoplastic elastomer for ultra-high fluidity, weather resistance and high strength.
[0006] Another object of the present invention is to provide a method for preparing an ultra-high fluidity thermoplastic elastomer for automotive parts, which has stable process, low cost, easy control and continuous production.
[0007] The present invention achieves the purpose of the invention by adopting the following technical solutions to solve the above problems:
[0008] A super-high fluidity thermoplastic elastomer for automobile parts comprises the following raw materials in parts by weight: 100 parts of EPDM rubber, 80-200 parts of polyolefin resin, 80-200 parts of thermoplastic elastomer, 80-200 parts of plasticizer, 0-120 parts of filler, 5-20 parts of scratch resistant agent, 2-20 parts of cross-linking agent, 2-20 parts of auxiliary cross-linking agent, 1-20 parts of lubricant, 1-20 parts of antioxidant and 1-20 parts of light stabilizer.
[0009] Preferably, the polyolefin resin provided by the present invention is one or more of homopolypropylene, copolymer polypropylene, metallocene polypropylene and polyethylene.
[0010] Furthermore, the polyolefin resin is one or more of homopolypropylene, copolymer polypropylene, metallocene polypropylene and polyethylene. When the polyolefin resin contains homopolypropylene, the content of homopolypropylene is ≥10wt%, and the melting index at 230℃ / 2.16kg is 20-120g / 10min; when the polyolefin resin contains copolymer polypropylene, the content of copolymer polypropylene is ≥15wt%, and the melting index at 230℃ / 2.16kg is 10-100g / 10min; when the polyolefin resin contains metallocene polypropylene, the content of metallocene polypropylene is ≥10wt%, and the melting index at 230℃ / 2.16kg is 80-3000g / 10min; when the polyolefin resin contains polyethylene, the content of polyethylene is ≥10wt%, and the melting index at 230℃ / 2.16kg is 2-100g / 10min; further, the polymerization unit of the copolymer polypropylene includes one or more of ethylene, propylene, butene, hexene, and octene; and the polyethylene includes at least one of low-density polyethylene, linear low-density polyethylene, high-density polyethylene, and metallocene polyethylene.
[0011] Preferably, the thermoplastic elastomer provided by the present invention is a blend of one or more of styrene-butadiene-styrene block copolymer, styrene-ethylene-butylene-styrene block copolymer, and styrene-ethylene-propylene-styrene block copolymer.
[0012] Preferably, the plasticizer provided by the present invention has a flash point greater than 200°C and a kinematic viscosity greater than 100 mm at 40°C. 2 / s of one or more blends of paraffin oil, cycloparaffin oil, aromatic oil, and straight-chain paraffin oil.
[0013] Preferably, the filler provided by the present invention is at least one of calcium carbonate, talc, kaolin, mica, wollastonite, barium sulfate, carbon black, white carbon black, and titanium dioxide. Further, the filler has a particle size of 3000-6000 mesh.
[0014] Preferably, the anti-scratch agent provided by the present invention is one or more of siloxane, polysiloxane, silicone masterbatch, and dimethyl silicone oil.
[0015] Furthermore, the viscosity of the dimethyl silicone oil is 10000-300000 cSt.
[0016] Preferably, the lubricant provided by the present invention is one or more of erucamide, oleamide, zinc stearate, magnesium stearate, silicone, and polyethylene wax.
[0017] Preferably, the cross-linking agent provided by the present invention is one or more of tert-butyl peroxyisopropyl carbonate, odorless diisopropyl peroxide, phenolic resin, and modified methyltriacetoxysilane.
[0018] Preferably, the auxiliary cross-linking agent provided by the present invention is one or more of bismaleimide, trimethylolpropane trimethacrylate, triallylmethyl triisocyanurate, 3-triethoxysilyl-1-propylamine, triallyl isocyanurate, N,N'-m-phenylene bismaleimide and triallyl cyanurate.
[0019] Another object of the present invention is to provide a method for preparing the above-mentioned thermoplastic elastomer, comprising the following steps:
[0020] (1) putting a thermoplastic elastomer and 20-40 wt% of a plasticizer into a high-speed mixer in sequence, stirring at a speed of 100-500 r / min for 10-30 minutes, standing for 1-4 hours, and then putting EPDM rubber, polyolefin resin, filler, anti-scratch agent, lubricant, antioxidant, and light stabilizer into the high-speed mixer together, stirring at a speed of 100-300 r / min for 5-10 minutes to obtain a premix A;
[0021] (2) adding premix A to an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, continuously and quantitatively adding premix A to the first section of the solid conveying zone of the extruder by using a metering pump, adding 20-40 wt % of a plasticizer to the front section of the extruder by using a metering pump, and performing vacuum treatment at the rear section of the extruder by using a vacuum pump. The premix is melted, extruded, and granulated in the extruder to obtain an intermediate B;
[0022] (3) adding the intermediate B into the extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the intermediate B, the cross-linking agent, the auxiliary cross-linking agent and the remaining plasticizer in the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder. After melting, extruding and granulating in the extruder, an ultra-high fluidity thermoplastic elastomer is obtained.
[0023] Preferably, the extruders in steps (2) and (3) are both co-rotating twin-screw extruders, with a feed speed of 60-300 r / min, a screw speed of 200-500 r / min, and a screw aspect ratio of 52-64.
[0024] Preferably, in steps (2) and (3), the temperature of the first section of the solid conveying zone of the extruder does not exceed 120°C, and the temperature of the remaining sections is 150-240°C.
[0025] Beneficial effects:
[0026] The ultra-high fluidity thermoplastic elastomer prepared by the present invention uses EPDM rubber as a main material to obtain a high-fluidity dynamically vulcanized EPDM rubber / polypropylene resin mixture, and introduces ultra-high fluidity polypropylene resin. Through reasonable proportioning and processing technology, the mixture system has excellent dispersibility and compatibility, and has the characteristics of ultra-high fluidity while having excellent weather resistance and a wide range of applications.
[0027] The thermoplastic elastomer material prepared by the present invention using EPDM rubber, polyolefin resin, thermoplastic elastomer, plasticizer, filler, scratch resistant agent, crosslinking agent, co-crosslinking agent, lubricant, antioxidant and light stabilizer in a certain proportion and under certain technical conditions can adjust different hardness and touch according to customer needs, has good mechanical properties, processing properties, resistance to high and low temperatures and environmental changes, and safety for human contact, and can be used for interior parts in automotive parts that come into contact with the human body.
[0028] At the same time, the present invention optimizes the production steps through reasonable production process design, and only needs two steps of extrusion to complete the production of ultra-high fluidity thermoplastic elastomer. The production process is simple, stable, easy to control, environmentally friendly, and has low equipment requirements, which is beneficial to large-scale industrial production.
[0029] The batch addition of the plasticizer in the present invention can effectively improve the heat resistance of the material, reduce the risk of precipitation, and at the same time increase production capacity and reduce energy consumption. In addition, by integrating the production scheme of styrene thermoplastic elastomer and thermoplastic dynamic vulcanizate, in the optimized process, the two-step extrusion method can complete the production of the final product. In the product obtained by this method, the styrene elastomer and the EPDM rubber can be well dispersed in the polyolefin continuous phase. DETAILED DESCRIPTION
[0030] The present invention is further explained below by means of specific examples.
[0031] The percentages (%) in the following examples are all mass percentages.
[0032] Example 1
[0033] A super-high fluidity thermoplastic elastomer used for automobile parts comprises the following raw materials in parts by weight: 100 parts of EPDM rubber, 100 parts of polyolefin resin, 80 parts of thermoplastic elastomer, 160 parts of plasticizer, 50 parts of filler, 10 parts of scratch resistant agent, 5 parts of cross-linking agent, 5 parts of auxiliary cross-linking agent, 10 parts of lubricant, 2 parts of antioxidant and 2 parts of light stabilizer.
[0034] In this embodiment: the polyolefin resin is a mixture of 30% homopolypropylene, 40% copolymer polypropylene and 30% metallocene polypropylene in a mass ratio;
[0035] The thermoplastic elastomer is a styrene-ethylene-propylene-styrene block copolymer with a styrene content of 40 wt%;
[0036] Plasticizers have a flash point greater than 200°C and a kinematic viscosity greater than 100 mm at 40°C. 2 / s of a blend of 40wt% paraffin oil and 60wt% cycloparaffin oil;
[0037] The filler is 6000 mesh calcium carbonate;
[0038] The scratch resistant agent is a mixture of 30wt% polysiloxane and 70wt% silicone masterbatch;
[0039] The crosslinking agent is tert-butyl peroxyisopropyl carbonate, and the auxiliary crosslinking agent is 50wt% bismaleimide and 50wt% trimethylolpropane trimethacrylate;
[0040] The lubricant is a mixture of 30 wt% erucamide and 70 wt% zinc stearate.
[0041] The preparation method of the ultra-high fluidity thermoplastic elastomer specifically comprises the following steps:
[0042] (1) A thermoplastic elastomer and 30 wt% of a plasticizer are sequentially placed in a high-speed mixer, stirred at a speed of 300 r / min for 10 minutes, and allowed to stand for 4 hours. Then, EPDM rubber, polyolefin resin, filler, anti-scratch agent, lubricant, antioxidant, and light stabilizer are placed in the high-speed mixer together, and stirred at a speed of 300 r / min for 10 minutes to obtain a premix A;
[0043] (2) adding premix A to an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, continuously and quantitatively adding premix A to the first section of the solid conveying zone of the extruder by using a metering pump, adding 30 wt% of a plasticizer to the front section of the extruder by using a metering pump, and performing a vacuum treatment at the rear section of the extruder by using a vacuum pump, with a vacuum pressure lower than 0.1 MPa. The premix is melted, extruded, and granulated in the extruder to obtain an intermediate B;
[0044] (3) adding the intermediate B into the extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the intermediate B, the cross-linking agent, the auxiliary cross-linking agent and the remaining plasticizer in the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder, with the vacuum pressure being lower than 0.1 MPa. After melting, extruding and granulating in the extruder, an ultra-high fluidity thermoplastic elastomer is obtained.
[0045] In the above steps (2) and (3), the extruder is a co-rotating twin-screw extruder with a feed speed of 180 r / min, a screw speed of 400 r / min, a screw aspect ratio of 64, and a processing temperature of the extruder: the first section temperature is 80°C, and the remaining section temperature is 210°C.
[0046] Example 2
[0047] A super-high fluidity thermoplastic elastomer used for automobile parts comprises the following raw materials in parts by weight: 100 parts of EPDM rubber, 120 parts of polyolefin resin, 150 parts of thermoplastic elastomer, 150 parts of plasticizer, 100 parts of filler, 6 parts of scratch resistant agent, 2 parts of cross-linking agent, 2 parts of auxiliary cross-linking agent, 8 parts of lubricant, 3 parts of antioxidant and 6 parts of light stabilizer.
[0048] The polyolefin resin is 60% copolymerized polypropylene and 40% metallocene polypropylene, the thermoplastic elastomer is a styrene-ethylene-butylene-styrene block copolymer with a styrene content of 30%, the plasticizer is a blend of 40% paraffin oil, 30% cycloalkane oil and 30% aromatic oil, the filler is a mixture of 30% carbon black and 70% white carbon black, the scratch-resistant agent is a mixture of 30% silicone masterbatch and 70% dimethyl silicone oil, the cross-linking agent is a phenolic resin, the auxiliary cross-linking agent is 50% N, N'-m-phenylene bismaleimide and 50% trimethylolpropane trimethacrylate, and the lubricant is a mixture of 70% zinc stearate and 30% silicone.
[0049] The preparation method of the ultra-high fluidity thermoplastic elastomer specifically comprises the following steps:
[0050] (1) A thermoplastic elastomer and 20% of a plasticizer are sequentially placed in a high-speed mixer and stirred at a speed of 500 r / min for 30 minutes. After standing for 4 hours, EPDM rubber, polyolefin resin, filler, anti-scratch agent, lubricant, antioxidant, and light stabilizer are placed in the high-speed mixer and stirred at a speed of 500 r / min for 5 minutes to obtain a premix A;
[0051] (2) adding premix A to an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, continuously and quantitatively adding premix A to the first section of the solid conveying zone of the extruder by using a metering pump, adding 40% of a plasticizer to the front section of the extruder by using a metering pump, and performing a vacuum treatment at the rear section of the extruder by using a vacuum pump, with a vacuum pressure of less than 0.1 MPa. The premix is melted, extruded, and granulated in the extruder to obtain an intermediate B;
[0052] (3) adding the intermediate B into the extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the intermediate B, the cross-linking agent, the auxiliary cross-linking agent and the remaining plasticizer in the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder, with the vacuum pressure being lower than 0.1 MPa. After melting, extruding and granulating in the extruder, an ultra-high fluidity thermoplastic elastomer is obtained.
[0053] In steps (2) and (3), the extruder is a co-rotating twin-screw extruder with a feed speed of 200 r / min, a screw speed of 450 r / min, a screw aspect ratio of 60, a first section temperature of 90°C, and a remaining section temperature of 190°C.
[0054] Example 3
[0055] A super-high fluidity thermoplastic elastomer used for automobile parts comprises the following raw materials in parts by weight: 100 parts of EPDM rubber, 140 parts of polyolefin resin, 200 parts of thermoplastic elastomer, 200 parts of plasticizer, 80 parts of filler, 5 parts of scratch resistant agent, 2 parts of cross-linking agent, 2 parts of auxiliary cross-linking agent, 20 parts of lubricant, 4 parts of antioxidant and 4 parts of light stabilizer.
[0056] The polyolefin resin is a mixture of 30% homopolypropylene, 30% copolymer polypropylene and 40% metallocene polypropylene, the thermoplastic elastomer is a blend of 80% styrene-ethylene-butylene-styrene block copolymer and 20% styrene-ethylene-propylene-styrene block copolymer, the plasticizer is a blend of 20% cycloalkane oil, 30% aromatic oil and 50% straight-chain alkane oil, the filler is a mixture of 70% calcium carbonate and 30% carbon black, the scratch-resistant agent is a mixture of 40% polysiloxane, 30% silicone masterbatch and 30% dimethyl silicone oil, the crosslinking agent is tert-butyl peroxy isopropyl carbonate, the co-crosslinking agent is 50% N, N'-m-phenylene bismaleimide and 50% triallyl cyanurate, and the lubricant is a mixture of 30% zinc stearate, 40% oleic acid amide and 30% polyethylene wax.
[0057] The preparation method of the ultra-high fluidity thermoplastic elastomer specifically comprises the following steps:
[0058] (1) A thermoplastic elastomer and 20% of a plasticizer are sequentially placed in a high-speed mixer and stirred at a speed of 200 r / min for 10 minutes. After standing for 1 hour, EPDM rubber, polyolefin resin, filler, anti-scratch agent, lubricant, antioxidant, and light stabilizer are placed in the high-speed mixer and stirred at a speed of 200 r / min for 5 minutes to obtain a premix A;
[0059] (2) adding premix A to an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, continuously and quantitatively adding premix A to the first section of the solid conveying zone of the extruder by using a metering pump, adding 40% of a plasticizer to the front section of the extruder by using a metering pump, and performing a vacuum treatment at the rear section of the extruder by using a vacuum pump, with a vacuum pressure of less than 0.1 MPa. The premix is melted, extruded, and granulated in the extruder to obtain an intermediate B;
[0060] (3) adding the intermediate B into the extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the intermediate B, the cross-linking agent, the auxiliary cross-linking agent and the remaining plasticizer in the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder, with the vacuum pressure being lower than 0.1 MPa. After melting, extruding and granulating in the extruder, an ultra-high fluidity thermoplastic elastomer is obtained.
[0061] In steps (2) and (3), the extruder is a co-rotating twin-screw extruder with a feed speed of 120 r / min, a screw speed of 350 r / min, a screw aspect ratio of 56, a first section temperature of 70°C, and a remaining section temperature of 180°C.
[0062] Comparative Example 1:
[0063] A super-high fluidity thermoplastic elastomer used for automobile parts comprises the following raw materials in parts by weight: 100 parts of EPDM rubber, 120 parts of polyolefin resin, 150 parts of thermoplastic elastomer, 150 parts of plasticizer, 100 parts of filler, 6 parts of scratch resistant agent, 2 parts of cross-linking agent, 2 parts of auxiliary cross-linking agent, 8 parts of lubricant, 3 parts of antioxidant and 6 parts of light stabilizer.
[0064] The polyolefin resin is 60% copolymerized polypropylene and 40% metallocene polypropylene, the thermoplastic elastomer is a styrene-ethylene-butylene-styrene block copolymer with a styrene content of 30%, the plasticizer is a blend of 40% paraffin oil, 30% cycloalkane oil and 30% aromatic oil, the filler is a mixture of 30% carbon black and 70% white carbon black, the scratch-resistant agent is a mixture of 30% silicone masterbatch and 70% dimethyl silicone oil, the cross-linking agent is a phenolic resin, the auxiliary cross-linking agent is 50% N, N'-m-phenylene bismaleimide and 50% trimethylolpropane trimethacrylate, and the lubricant is a mixture of 70% zinc stearate and 30% silicone.
[0065] The preparation method of the ultra-high fluidity thermoplastic elastomer specifically comprises the following steps:
[0066] (1) adding EPDM rubber, 50% polyolefin resin, filler, lubricant and antioxidant into a high-speed mixer, maintaining the stirring speed at 200 r / min for 10 min, and obtaining a premix A;
[0067] (2) adding premix A to an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add premix A to the first section of the solid conveying zone of the extruder, using a metering pump to add a plasticizer to the front section of the extruder, and using a vacuum pump to evacuate the rear section of the extruder, with the vacuum pressure being lower than 0.1 MPa. The premix is melted, extruded, and granulated in the extruder to obtain a mixture B;
[0068] (3) adding the mixture B into an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the mixture B, the crosslinking agent, and the auxiliary crosslinking agent to the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder, with the vacuum pressure being lower than 0.1 MPa, and after melting, extruding, and granulating in the extruder, a mixture C is obtained;
[0069] (4) Adding mixture C, thermoplastic elastomer, remaining polyolefin resin, scratch resistant agent, and light stabilizer into a high-speed stirrer at 200 r / min, stirring for 20 minutes, and standing for 2 hours to obtain mixture D;
[0070] (5) Adding the mixture D into the extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the mixture D in the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder, with the vacuum pressure being lower than 0.1 MPa. After melting, extruding, and granulating in the extruder, the target product is obtained.
[0071] In steps (2), (3) and (5), the extruder is a co-rotating twin-screw extruder with a feed speed of 120 r / min, a screw speed of 350 r / min, a screw aspect ratio of 56, a first section temperature of 70°C, and a remaining section temperature of 180°C.
[0072] Comparative Example 2:
[0073] A super-high fluidity thermoplastic elastomer used for automobile parts comprises the following raw materials in parts by weight: 100 parts of EPDM rubber, 120 parts of polyolefin resin, 150 parts of thermoplastic elastomer, 100 parts of plasticizer, 80 parts of filler, 10 parts of scratch resistant agent, 10 parts of cross-linking agent, 10 parts of auxiliary cross-linking agent, 10 parts of lubricant, 5 parts of antioxidant and 5 parts of light stabilizer.
[0074] The polyolefin resin is selected from 50% homopolymer polypropylene and 50% copolymer polypropylene, the thermoplastic elastomer is 50% styrene-ethylene-butylene-styrene block copolymer and 50% styrene-butadiene-styrene block copolymer, the plasticizer is a blend of 50% paraffin oil, 30% cycloalkane oil and 20% aromatic oil, the filler is a mixture of 60% mica powder and 40% white carbon black, the scratch-resistant agent is a mixture of 50% silicone masterbatch and 50% dimethyl silicone oil, the cross-linking agent is tert-butyl peroxy isopropyl carbonate, the auxiliary cross-linking agent is 50% N, N'-m-phenylene bismaleimide and 50% triallyl cyanurate, and the lubricant is a mixture of 50% magnesium stearate and 50% silicone.
[0075] The preparation method of the ultra-high fluidity thermoplastic elastomer specifically comprises the following steps:
[0076] (1) adding EPDM rubber, 50% polyolefin resin, filler, lubricant and antioxidant into a high-speed mixer, maintaining the stirring speed at 400 r / min for 10 min, and obtaining a premix A;
[0077] (2) adding premix A to an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add premix A to the first section of the solid conveying zone of the extruder, using a metering pump to add a plasticizer to the front section of the extruder, and using a vacuum pump to evacuate the rear section of the extruder, with the vacuum pressure being lower than 0.1 MPa. The premix is melted, extruded, and granulated in the extruder to obtain a mixture B;
[0078] (3) adding the mixture B into an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the mixture B, the crosslinking agent, and the auxiliary crosslinking agent to the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder, with the vacuum pressure being lower than 0.1 MPa, and after melting, extruding, and granulating in the extruder, a mixture C is obtained;
[0079] (4) Adding mixture C, thermoplastic elastomer, remaining polyolefin resin, scratch resistant agent, and light stabilizer into a high-speed stirrer at 200 r / min, stirring for 20 minutes, and standing for 2 hours to obtain mixture D;
[0080] (5) Adding the mixture D into the extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the mixture D in the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder, with the vacuum pressure being lower than 0.1 MPa. After melting, extruding, and granulating in the extruder, the target product is obtained.
[0081] In steps (2), (3) and (5), the extruder is a co-rotating twin-screw extruder with a feed speed of 120 r / min, a screw speed of 350 r / min, a screw aspect ratio of 56, a first section temperature of 90°C, and a remaining section temperature of 200°C.
[0082] Test results
[0083] Test method: Hardness, measured according to ISO 7619-1, type A;
[0084] Tensile strength: the test standard is ISO 37-1, and the tensile test rate is 500 mm / min;
[0085] Tear strength, test standard is ISO 34-1, method B, use uncut rectangular specimen, test rate is 500mm / min;
[0086] Melt flow rate, test standard is ISO 1133-1, method A, 190℃, 2.16kg;
[0087] Hot air aging is carried out according to the method specified in GB / T 3512. The sample is placed in a constant heat aging box at a specified temperature of (130±2)℃ for 168h. The sample is taken out and stored in a standard environment for at least 16h before the tensile strength is measured and the change rate of tensile strength is calculated:
[0088]
[0089] The scratch resistance was tested by a 100-grid cross scratch test according to the method specified in GB / T 9286, and ΔE was measured using a colorimeter before and after the test.
[0090] Table 1 Measurement results
[0091]
[0092] It can be seen from the above table that the thermoplastic elastomer prepared in the present application has a high melt flow rate and strong mechanical strength. Compared with the comparative example, the embodiment has higher fluidity, mechanical strength, better heat resistance and scratch resistance.
[0093] In Example 1, the styrene content of the thermoplastic elastomer is high, the addition amount of the crosslinking agent and the auxiliary crosslinking agent is high, the overall strength is high, and the fluidity is good; compared with Example 1, in Example 2, there is a higher addition amount of polyolefin and thermoplastic elastomer, and the content of metallocene polypropylene is higher, homopolymer polypropylene is not added, and the addition amount of the scratch resistant agent, crosslinking agent and crosslinking auxiliary agent is low, so the mechanical strength of the product is slightly poor, but the fluidity performance is good; compared with Example 2, in Example 3, a certain amount of homopolymer polypropylene is replaced, and the content of thermoplastic elastomer and plasticizer is high, so the fluidity performance is excellent, and at the same time a certain mechanical strength, heat aging resistance and scratch resistance are guaranteed; compared with Example Compared with Comparative Example 2, the same material formula is used in Comparative Example 1, but the processing process is according to the traditional method, firstly the TPV finished product is produced as the homemade raw material according to dynamic vulcanization, and then it is produced according to the process of thermoplastic elastomer, the production process is more complicated, and the dispersion of EPDM and SEBS in the substrate is poor, the mechanical properties are low, and the fluidity is significantly low; compared with Comparative Example 1, the same production process is used in Comparative Example 2, and the addition of metallocene polypropylene is reduced in the formula design, and the amount of polypropylene resin, thermoplastic elastomer, and plasticizer is also reduced, and the amount of cross-linking agent and cross-linking aid is increased, and the product performance is manifested as worse fluidity and relatively high mechanical properties.
[0094] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the foregoing description, and it is intended that all changes that fall within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0095] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An ultra-high fluidity thermoplastic elastomer for automotive parts, characterized in that: The invention is prepared from the following components by weight: 100 parts of EPDM rubber, 80-200 parts of polyolefin resin, 80-200 parts of thermoplastic elastomer, 80-200 parts of plasticizer, 0-120 parts of filler, 5-20 parts of scratch resistant agent, 2-20 parts of crosslinking agent, 2-20 parts of auxiliary crosslinking agent, 1-20 parts of lubricant, 1-20 parts of antioxidant and 1-20 parts of light stabilizer. The preparation method comprises the following steps: (1) Putting a thermoplastic elastomer and 20-40 wt% of a plasticizer into a high-speed mixer in sequence, stirring at a speed of 100-500 r / min for 10-30 minutes, and standing for 1-4 hours; then putting EPDM rubber, polyolefin resin, filler, scratch resistant agent, lubricant, antioxidant, and light stabilizer into the high-speed mixer together, stirring at a speed of 100-500 r / min for 5-10 minutes, to obtain a premix A; (2) adding premix A into an extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add premix A into the first section of the solid conveying zone of the extruder, adding 20-40 wt% of a plasticizer into the front section of the extruder using a metering pump, and performing vacuum treatment at the rear section of the extruder using a vacuum pump. The premix is melted, extruded, and granulated in the extruder to obtain an intermediate B; (3) adding the intermediate B into the extruder, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, using a metering pump to continuously and quantitatively add the intermediate B, the cross-linking agent, the auxiliary cross-linking agent and the remaining plasticizer in the first section of the solid conveying zone of the extruder, and using a vacuum pump to evacuate the tail end of the extruder. After melting, extruding and granulating in the extruder, an ultra-high fluidity thermoplastic elastomer is obtained; The extruders in steps (2) and (3) are both co-rotating twin-screw extruders, with a feed speed of 60-300 r / min, a screw speed of 200-500 r / min, and a screw aspect ratio of 52-64; the temperature of the first section of the solid conveying zone of the extruder does not exceed 120°C, and the temperature of the remaining sections is 150-240°C.
2. The ultra-high fluidity thermoplastic elastomer according to claim 1, characterized in that: The polyolefin resin is one or more of homopolypropylene, copolymer polypropylene, metallocene polypropylene and polyethylene.
3. The ultra-high fluidity thermoplastic elastomer according to claim 1, characterized in that: The thermoplastic elastomer is one or more blends of styrene-butadiene-styrene block copolymer, styrene-ethylene-butylene-styrene block copolymer, and styrene-ethylene-propylene-styrene block copolymer.
4. The ultra-high fluidity thermoplastic elastomer according to claim 1, characterized in that: The plasticizer has a flash point greater than 200°C and a kinematic viscosity greater than 100 mm at 40°C. 2 / s of one or more blends of paraffin oil, cycloparaffin oil, aromatic oil, and straight-chain paraffin oil.
5. The ultra-high fluidity thermoplastic elastomer according to claim 1, characterized in that: The filler is at least one of calcium carbonate, talc, kaolin, mica, wollastonite, barium sulfate, carbon black, white carbon black, and titanium dioxide; The scratch-resistant agent is one or more of siloxane, polysiloxane, silicone masterbatch and dimethyl silicone oil.
6. The ultra-high fluidity thermoplastic elastomer according to claim 1, characterized in that: The lubricant is one or more of erucamide, oleamide, zinc stearate, magnesium stearate, silicone and polyethylene wax.
7. The ultra-high fluidity thermoplastic elastomer according to claim 1, characterized in that: The crosslinking agent is one or more of tert-butyl peroxyisopropyl carbonate, odorless diisopropyl peroxide, phenolic resin, and modified methyl triacetoxy silane.
8. The ultra-high fluidity thermoplastic elastomer according to claim 1, characterized in that: The auxiliary crosslinking agent is one or more of bismaleimide, trimethylolpropane trimethacrylate, triallylmethyl triisocyanurate, 3-triethoxysilyl-1-propylamine, triallyl isocyanurate, N,N'-m-phenylene bismaleimide and triallyl cyanurate.