Aluminosilicate materials for water mineralization and their preparation methods
By subjecting aluminosilicate minerals to multi-step soaking and calcination, aluminosilicate materials for water mineralization were prepared, solving the problem of high aluminum leaching from natural aluminosilicate minerals and improving the safety of mineralized water.
Patent Information
- Application Number
- CN202111413933.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-11-25
AI Technical Summary
Existing natural aluminosilicate minerals used for water mineralization have a high aluminum leaching rate in water, which affects the safety of the mineralized water.
A silicate material for water mineralization was prepared by subjecting aluminosilicate minerals to a multi-step soaking and calcination process using hydrochloric acid, hydrogen peroxide solution, calcium chloride solution, and citric acid, while maintaining its layered structure and reducing aluminum leaching.
While ensuring the effective dissolution of macro and micro elements, it significantly reduces the amount of aluminum leaching and improves the safety of mineralized water.
Smart Images

Figure CN116159535B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of water treatment materials technology, for example to an aluminosilicate material for water mineralization and a method for preparing the same. Background Technology
[0002] Natural aluminosilicate minerals are widely distributed in nature and are abundant in variety, such as quartz monzonite, zeolite, mica, illite, and montmorillonite. These natural aluminosilicate minerals are not only important non-metallic mineral raw materials and resources, but also play a crucial role in water mineralization. For example, using quartz monzonite to treat water can transform it into water with a higher concentration of positively and negatively charged atomic groups, enabling it to adsorb free ions in the water. When quartz monzonite dissolves in water, it can release essential macroelements such as K, Ca, and Mg, as well as trace elements such as Si, Fe, Zn, Cu, Mo, Se, Mn, Sr, Ni, V, Li, Co, Cr, I, Ge, and Ti, which are beneficial to the human body and organisms. Quartz monzonite can also release essential amino acids in aqueous solutions. However, natural aluminosilicate minerals such as quartz monzonite can exhibit excessive aluminum levels during the leaching process.
[0003] Aluminum is a silvery-white, lightweight metal. In nature, it exists in the form of complex aluminosilicates and is the most abundant metal in the Earth's crust, accounting for 7.45% of its total mass. Aluminum is a non-essential trace element for the human body, generally entering the body through food, drinking water, medications, and the use of aluminum cookware. Long-term excessive intake can damage bones, the brain, and the nervous system, potentially leading to anemia, osteoporosis, and even Alzheimer's disease. Excessive intake by pregnant women can affect fetal development. Excessive aluminum has an even greater impact on children, affecting bone growth, causing developmental delays, and impairing neurological development in infants and young children, leading to intellectual disabilities.
[0004] In the process of implementing the embodiments of this disclosure, at least the following problems were found in the related art:
[0005] Existing natural aluminosilicate minerals used for water mineralization have a high aluminum leaching rate in water, which affects the safety of the resulting mineralized water. Summary of the Invention
[0006] To provide a basic understanding of some aspects of the disclosed embodiments, a brief summary is given below. This summary is not intended as a general commentary, nor is it intended to identify key / important components or describe the scope of protection of these embodiments, but rather as a prelude to the detailed description that follows.
[0007] This disclosure provides a method for preparing aluminosilicate materials for water mineralization, which, while ensuring the effective dissolution of essential macro- and micro-elements, reduces the amount of aluminum leached from water and improves the safety of mineralized water obtained using aluminosilicate materials.
[0008] In some embodiments, the method for preparing the aluminosilicate material for water mineralization includes: Step 1: pulverizing the aluminosilicate mineral to be treated to obtain a powder to be treated, and soaking the powder to be treated in hydrochloric acid and hydrogen peroxide solution to obtain a first pretreated product; Step 2: soaking the first pretreated product in hydrochloric acid for a second time, drying it, calcining it for a first time, soaking it in calcium chloride solution for a third time, drying it, and calcining it for a second time to obtain a second pretreated product; Step 3: mixing the second pretreated product with citric acid to obtain a mixture, calcining the mixture for a third time, and cooling it to obtain a third pretreated product; Step 4: washing the third pretreated product with hydrochloric acid, drying it, and obtaining the aluminosilicate material for water mineralization.
[0009] Optionally, the concentration of hydrochloric acid in the first soaking is 0.05-0.2 mol / L.
[0010] Optionally, the soaking time of hydrochloric acid in the first soaking is 3-4 hours.
[0011] Optionally, the soaking time of hydrogen peroxide in the first soaking is 3-4 hours.
[0012] Optionally, in the second soaking, the solid-liquid mass ratio of the solid-liquid mixture obtained after mixing the first pretreated material with hydrochloric acid is 1:15-1:25.
[0013] Optionally, the first calcination is carried out in a muffle furnace at a temperature of 380℃-430℃ for a duration of 1.5-2.5 hours.
[0014] Optionally, the second calcination is carried out in a muffle furnace at a temperature of 310°C-360°C for a duration of 0.8-1.2 hours.
[0015] Optionally, the third roasting is carried out in a tube furnace. First, the tube of the tube furnace is evacuated to a vacuum, and then steam is introduced into the tube. The roasting temperature is 400℃-500℃, and the roasting time is 2-4 hours.
[0016] Optionally, the aluminosilicate minerals include quartz diorite, zeolite, mica, illite, or montmorillonite.
[0017] In some embodiments, the aluminosilicate material for water mineralization is prepared by the aforementioned preparation method.
[0018] The aluminosilicate materials and their preparation methods for water mineralization provided in this disclosure can achieve the following technical effects:
[0019] The aluminosilicate material for water mineralization obtained by the method provided in this disclosure maintains the layered structure of the aluminosilicate material without destroying its overall structure. When using this aluminosilicate material for water mineralization, while ensuring the effective dissolution of macroelements such as K, Ca, and Mg, as well as trace elements such as Si, Fe, Zn, Cu, Mo, Se, Mn, Sr, Ni, V, Li, Co, Cr, I, Ge, and Ti from the resulting mineralized water, the amount of aluminum leached is reduced, thus improving the safety of the resulting mineralized water.
[0020] The above general description and the description below are exemplary and illustrative only and are not intended to limit this application. Attached Figure Description
[0021] One or more embodiments are illustrated by way of example with reference to the accompanying drawings. These illustrations and drawings do not constitute a limitation on the embodiments. Elements having the same reference numerals in the drawings are shown as similar elements. The drawings are not to be scaled. And wherein:
[0022] Figure 1 These are scanning electron microscope (SEM) images of quartz diorite before and after treatment using the preparation method provided in the embodiments of this disclosure;
[0023] Figure 2 The images show X-ray energy dispersive spectroscopy (EDS) spectra of quartz diorite before and after treatment using the preparation method provided in this embodiment of the present disclosure.
[0024] Figure 3 The images are X-ray diffraction (XRD) patterns of quartz diorite before and after treatment using the preparation method provided in the embodiments of this disclosure.
[0025] Figure 4 The diagram shows the pore size distribution of quartz diorite before and after treatment using the preparation method provided in this embodiment. Detailed Implementation
[0026] To provide a more detailed understanding of the features and technical content of the embodiments of this disclosure, the implementation of the embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. The accompanying drawings are for illustrative purposes only and are not intended to limit the embodiments of this disclosure. In the following technical description, for ease of explanation, several details are used to provide a full understanding of the disclosed embodiments. However, one or more embodiments may still be implemented without these details.
[0027] The terms "first," "second," etc., used in the specification, claims, and accompanying drawings of this disclosure are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence, unless a specific order is explicitly stated in the particular embodiment. It should be understood that such data can be interchanged where appropriate for the embodiments of this disclosure described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion.
[0028] Unless otherwise stated, the term "multiple" means two or more.
[0029] In this embodiment of the disclosure, the character " / " indicates that the objects before and after it are in an "or" relationship. For example, A / B means: A or B.
[0030] The term "and / or" describes an association between objects, indicating that three relationships can exist. For example, A and / or B means: A or B, or A and B.
[0031] It should be noted that, unless otherwise specified, the embodiments and features described in the present disclosure can be combined with each other.
[0032] Aluminosilicate minerals are silicate minerals formed by the isomorphous substitution of some silicon in silicate groups by aluminum, and they are widely distributed in nature. This disclosure provides a method for preparing aluminosilicate materials from natural aluminosilicate minerals that can be used for water mineralization.
[0033] In some alternative embodiments, the method for preparing the aluminosilicate material for water mineralization includes:
[0034] Step 1: Crush the aluminosilicate minerals to be treated to obtain the powder to be treated. Soak the powder to be treated in hydrochloric acid and hydrogen peroxide solution respectively to obtain the first pretreated product.
[0035] Optionally, the silicate mineral to be treated is washed with pure water and then ultrasonically treated in an ultrasonic cleaner until the ultrasonic solution is substantially clear. The cleaned silicate mineral is then dried and pulverized to obtain the powder to be treated. Optionally, the particle size of the powder to be treated is 60-80 mesh.
[0036] Optionally, the first soaking process of the powder to be treated includes: soaking in a dilute hydrochloric acid solution for a preset time, stirring several times during the soaking process to improve the efficiency of impurity removal. After removing it from the dilute hydrochloric acid, rinsing with pure water until the pH of the solution is neutral. Then, soaking in hydrogen peroxide solution for a preset time, stirring several times during the soaking process to improve the efficiency of impurity removal. Afterwards, rinsing repeatedly with pure water and drying, the first pretreated material is obtained. This step can effectively remove impurities from the surface of the powder to be treated.
[0037] Step 2: The first pretreated material is soaked in hydrochloric acid for a second time, dried, and then calcined for a first time. After completion, it is soaked in calcium chloride solution for a third time, dried, and then calcined for a second time to obtain the second pretreated material.
[0038] Optionally, the first pretreated material obtained after step one is first soaked in hydrochloric acid solution, filtered, and then repeatedly washed with pure water. The second soaking in hydrochloric acid solution can remove some of the aluminum and internal impurities from the crystal framework of the first pretreated material.
[0039] Optionally, the minerals after the second soaking are dried and then subjected to a first roasting. This removes moisture from the surface of the minerals and further removes internal organic matter.
[0040] Optionally, the minerals after the first roasting are subjected to a third soaking in a calcium chloride solution. Soaking in a calcium chloride solution ensures the proper dissolution of elements when the minerals are soaked in water.
[0041] Step 3: Mix the second pretreatment material with citric acid to obtain a mixture, then calcine the mixture for the third time, and after cooling, obtain the third pretreatment material.
[0042] The third roasting can further remove aluminum from the mineral crystal framework, further reducing the amount of aluminum dissolved in the resulting aluminosilicate material used for water mineralization.
[0043] Step 4: The third pretreatment material is washed with hydrochloric acid and dried to obtain aluminosilicate material for water mineralization.
[0044] The third pretreatment material is cleaned with dilute hydrochloric acid, which can remove substances such as alumina adhering to the surface of the third pretreatment material, and further reduce the aluminum content in the obtained aluminosilicate material.
[0045] The aluminosilicate material for water mineralization prepared by the method provided in this disclosure significantly reduces the amount of aluminum leached from the solution, while maintaining the layered structure of natural aluminosilicate minerals and ensuring the leaching of other essential macro- and micro-elements. Therefore, when the aluminosilicate material prepared by the method provided in this disclosure is used for water mineralization, it ensures the effective leaching of macro-elements such as K, Ca, and Mg, as well as micro-elements such as Si, Fe, Zn, Cu, Mo, Se, Mn, Sr, Ni, V, Li, Co, Cr, I, Ge, and Ti, while reducing the amount of aluminum leached and improving the safety of the resulting mineralized water.
[0046] Optionally, the concentration of hydrochloric acid in the first soaking is 0.05-0.2 mol / L.
[0047] The powder to be treated is first soaked in dilute hydrochloric acid to remove impurities from its surface. Optionally, the hydrochloric acid can be a dilute hydrochloric acid solution with concentrations of 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.12 mol / L, 0.15 mol / L, or 0.2 mol / L. Optionally, during the first soaking process, the solid-liquid mixture of hydrochloric acid and the powder to be treated is stirred to improve the removal effect of impurities from the powder surface.
[0048] Optionally, the soaking time in hydrochloric acid during the first soaking is 3-4 hours.
[0049] The initial soaking of the powder to be treated with dilute hydrochloric acid can last for 3, 3.5, or 4 hours to improve the removal of impurities from the powder surface. After soaking, the powder is repeatedly rinsed with pure water until the pH of the resulting cleaning solution is neutral.
[0050] Optionally, the soaking time of hydrogen peroxide in the first soaking is 3-4 hours.
[0051] After soaking in dilute hydrochloric acid, the powder is further soaked in hydrogen peroxide solution to remove impurities from its surface. Optionally, the hydrogen peroxide solution has a mass percentage of 5%, and the soaking time is 3-4 hours. Stirring can be performed several times during the soaking process to further improve the removal of impurities from the powder's surface.
[0052] Optionally, in the second soaking, the solid-liquid mass ratio of the solid-liquid mixture obtained after mixing the first pretreated material with hydrochloric acid is 1:15-1:25.
[0053] The first pretreated material obtained in step one is placed in a hydrochloric acid solution for a second soaking. During the second soaking, the concentration of the hydrochloric acid solution can be 1-2 mol / L, for example, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, or 2 mol / L. The mass ratio of the first pretreated material to the hydrochloric acid solution is 1:15-1:25, for example, 1:15, 1:20, or 1:25. Using hydrochloric acid solution for the second soaking can effectively remove aluminum and internal impurities from the mineral crystal framework in the first pretreated material. Optionally, the soaking time for the second soaking is 2 hours. Optionally, after the second soaking, the filtered mineral is repeatedly rinsed with pure water and dried.
[0054] Optionally, the first roasting is carried out in a muffle furnace at a temperature of 380℃-430℃ for a duration of 1.5-2.5 hours.
[0055] The minerals soaked in hydrochloric acid are first roasted in a muffle furnace at temperatures of 380℃, 390℃, 400℃, 410℃, 420℃, or 430℃. The roasting time can be 1.5 hours, 2 hours, or 2.5 hours. This first roasting in the muffle furnace removes moisture from the mineral surface and organic matter from its interior.
[0056] Optionally, after the minerals have cooled to room temperature after the first roasting, they are soaked in a 2 mol / L CaCl2 solution for 24 hours to ensure the normal dissolution of macroelements such as K, Ca, and Mg, and microelements such as Si, Fe, Zn, Cu, Mo, Se, Mn, Sr, Ni, V, Li, Co, Cr, I, Ge, and Ti when the aluminosilicate minerals are soaked in water.
[0057] Optionally, the second roasting is carried out in a muffle furnace at a temperature of 310℃-360℃ for a duration of 0.8-1.2 hours.
[0058] The second roasting temperature can be 310℃, 320℃, 330℃, 340℃, 350℃, or 360℃, and the roasting time can be 0.8 hours, 1 hour, or 1.2 hours. The second roasting further removes moisture from the mineral surface and organic matter from its interior. During the formation of mineral rocks, some organic matter is contained within them. The preparation method provided in this embodiment can remove the organic matter inside the aluminosilicate mineral, improving the purity of the obtained aluminosilicate material.
[0059] Optionally, the third roasting is carried out in a tube furnace. First, the tubes of the tube furnace are evacuated to a vacuum, and then steam is introduced into the tubes. The roasting temperature is 400℃-500℃, and the roasting time is 2-4 hours.
[0060] In step three, the mixture obtained by mixing the second pretreated material with citric acid has a mass ratio of 1:10. The mixture is then placed in a tube furnace for a third roasting to further remove aluminum from the mineral crystal framework. Optionally, the roasting temperature for the third roasting is 400℃, 420℃, 440℃, 450℃, 470℃, 480℃, or 500℃, and the roasting time is 2 hours, 3 hours, or 4 hours. Optionally, the third roasting temperature should not exceed 600℃, and the roasting time should not exceed 4 hours; otherwise, the crystal structure of the mineral will be damaged, affecting the normal dissolution of the aforementioned macro- and micro-elements when the mineral is soaked in water.
[0061] Alternatively, aluminosilicate minerals include quartz diorite, zeolite, mica, illite, or montmorillonite.
[0062] This disclosure provides an aluminosilicate material for water mineralization.
[0063] In some embodiments, the aluminosilicate material for water mineralization is prepared by the aforementioned method.
[0064] The aluminosilicate material obtained by the aforementioned method retains its original layered structure, preserving the original overall structure of the mineral. This facilitates the proper dissolution of macroelements such as K, Ca, and Mg, and trace elements such as Si, Fe, Zn, Cu, Mo, Se, Mn, Sr, Ni, V, Li, Co, Cr, I, Ge, and Ti from the resulting mineralized water during water mineralization.
[0065] The mass percentage of silicon and aluminum in the aluminosilicate material obtained by the aforementioned method is significantly increased, indicating that the aforementioned method for preparing aluminosilicate materials for water mineralization effectively removes aluminum from natural aluminosilicate minerals.
[0066] The aluminosilicate material obtained by the aforementioned method has a slightly increased specific surface area, and the number of micropores with a pore size of less than 2 nm is relatively reduced, while the number of mesopores with a pore size of 2 nm-50 nm is relatively increased. The increased specific surface area enhances the adsorption of heavy metals such as chromium in water.
[0067] The following uses quartz diorite as an example to further illustrate the preparation method of the aluminosilicate material for water mineralization provided in the embodiments of this disclosure.
[0068] Step one: After washing the quartz monzonite blocks with pure water, they are ultrasonically treated in an ultrasonic cleaner until the cleaning solution is basically clear. After drying, they are pulverized to obtain 60-80 mesh powder. Then, they are soaked in 0.1 mol / L dilute hydrochloric acid for 3 hours, stirring several times during the soaking process. After soaking, the powder is removed and repeatedly rinsed with pure water until the pH of the rinsing solution is neutral. Next, it is soaked in a 5% hydrogen peroxide solution for 4 hours, stirring several times during the soaking process. This step is used to remove impurities from the surface of the quartz monzonite mineral powder. Finally, it is repeatedly rinsed with pure water and dried to obtain the first pretreated quartz monzonite.
[0069] Step two: First, soak the quartz monzonite treated in Step one in 1.5 mol / L hydrochloric acid for 2 hours, at which point the solid-liquid volume ratio is 1:20. Then, filter out the quartz monzonite minerals and rinse repeatedly with pure water. After drying, calcine it in a muffle furnace at 400℃ for 2 hours. After the quartz monzonite cools to room temperature, soak it in 2 mol / L CaCl2 solution for 24 hours. After filtration, rinse the quartz monzonite several times with a small amount of deionized water, dry it at 120℃, and then calcine it in a muffle furnace at 340℃ for 1 hour. After removing it and cooling it to room temperature, pack it into a sealed bag to obtain the second pretreated quartz monzonite.
[0070] Step 3: Mix the quartz diorite treated in Step 2 with citric acid at a mass ratio of 1:10, place the mixture in a tube furnace, first evacuate the air from the tube to a vacuum state, then introduce water vapor into the tube, raise the temperature to 450°C, treat for 2 hours, and remove after cooling to obtain the third pretreated quartz diorite.
[0071] Step four: The minerals obtained in step three are first washed with 0.1 mol / L dilute hydrochloric acid, then rinsed with deionized water and dried to obtain quartz diorite material that can be used for water mineralization.
[0072] The quartz diorite before and after treatment was analyzed, and the results are as follows.
[0073] Figure 1 The left image in the image is a scanning electron microscope (SEM) image of the quartz diorite minerals before processing. Figure 1 The right image in the image is a scanning electron microscope (SEM) image of the processed quartz diorite material. From... Figure 1 As can be seen, after the aforementioned treatment, the structure of the quartz monzonite material did not change significantly and still exhibited a layered structure. Therefore, the preparation method provided in this embodiment does not damage the layered structure of the quartz monzonite, ensuring the normal dissolution of essential macro- and micro-elements required by the human body.
[0074] Figure 3 The upper image shows the X-ray diffraction (XRD) pattern of the processed quartz diorite material. From... Figure 3As can be seen from the above treatment, the intensity of the diffraction peaks of the obtained quartz diorite material at 2θ = 27°-29° increases, but from... Figure 3 As can be seen, the diffraction peak shape and diffraction angle remain unchanged, indicating that the overall structure of the quartz diorite was not destroyed after being treated by the preparation method provided in this embodiment.
[0075] Figure 2 The image above shows the X-ray energy dispersive spectroscopy (EDS) image of quartz diorite minerals before treatment. Figure 2 The image below shows the X-ray energy dispersive spectroscopy (EDS) image of the processed quartz diorite material. Figure 2 The mass percentages of each element in the X-ray energy dispersive spectroscopy (EDS) plot are shown in Table 1.
[0076] Table 1
[0077] element O Al Si Fe Ca Before processing 58.73 16.03 24.76 0.34 0.13 After processing 48.18 7.54 42.43 1.79 0.05
[0078] from Figure 2 As shown in Table 1, the Si / Al mass ratio of the quartz monzonite increased from 1.54 before treatment to 5.63 after treatment. This demonstrates that the method provided in this embodiment induces significant dealuminization in the quartz monzonite.
[0079] Pore size distribution of quartz diorite before and after treatment is as follows: Figure 4 As shown. Table 2 shows... Figure 4 The specific values of total pore volume, average pore diameter, and specific surface area before and after treatment of the quartz monzonite.
[0080] Table 2
[0081] Quartz diorite sample <![CDATA[Total pore volume (cm 3 / g)]]> Average pore size (nm) <![CDATA[Specific surface area (m 2 / g)]]> Before processing <![CDATA[9.989×10 -3 ]]> 18.39 2.173 After processing <![CDATA[1.031×10 -2 ]]> 18.57 2.221
[0082] from Figure 4 As can be seen from Table 2, the specific surface area of the quartz diorite increased slightly after treatment, the number of micropores with a pore size of less than 2 nm decreased relatively, while the number of mesopores with a pore size of 2 nm to 50 nm increased relatively.
[0083] Two 10g portions of raw quartz monzonite powder, the second pretreated quartz monzonite, and the fully treated quartz monzonite powder were weighed out and labeled as No. 1 and No. 2, respectively. They were placed in six 250mL Erlenmeyer flasks, and then 50mL of deionized water was added for soaking for 24±1h. The supernatant was poured into centrifuge tubes and centrifuged. The elemental content of the supernatant was tested, and the results are shown in Table 3.
[0084] Table 3
[0085]
[0086]
[0087] Note: "ND" means Not Detected.
[0088] As shown in Table 3, treated quartz monzonite can still leach macroelements such as K, Ca, and Mg, as well as trace elements such as Mn, Fe, and V, which are beneficial to the human body and organisms. However, after soaking untreated quartz monzonite for 24±1 hours, the aluminum content in the soaking solution was 0.3674 mg / L and 0.3777 mg / L. After soaking quartz monzonite with the second pretreatment for 24±1 hours, the aluminum content in the soaking solution was 0.1839 mg / L and 0.1671 mg / L, with the Al leaching amount decreasing by about 50%. After soaking quartz monzonite with full treatment for 24±1 hours, the aluminum content in the soaking solution was 0.0893 mg / L and 0.0961 mg / L, with the Al leaching amount decreasing by about 75%.
[0089] It is evident that when the quartz diorite material obtained by the method provided in this embodiment is subjected to water mineralization treatment, the amount of aluminum leaching in the resulting mineralized water is significantly reduced, while ensuring the normal leaching of macroelements such as K, Ca, and Mg, as well as microelements such as Mn, Fe, and V, thereby improving the safety of the mineralized water.
[0090] The foregoing description and accompanying drawings fully illustrate embodiments of the present disclosure to enable those skilled in the art to practice them. Parts and features of some embodiments may be included or substituted for parts and features of other embodiments. The embodiments of the present disclosure are not limited to the types of natural aluminosilicate materials, concentrations of the soaking solution, soaking times, calcination temperatures, calcination times, etc., as described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the present disclosure is limited only by the appended claims.
Claims
1. A method for preparing aluminosilicate materials for water mineralization, characterized in that, include: Step 1: Crush the aluminosilicate mineral to be treated to obtain the powder to be treated. Soak the powder to be treated in hydrochloric acid and hydrogen peroxide solution in sequence to obtain the first pretreated product. Step 2: The first pretreated material is soaked in hydrochloric acid for a second time, dried, and then calcined for a first time. After completion, it is soaked in calcium chloride solution for a third time, dried, and then calcined for a second time to obtain the second pretreated material. Step 3: Mix the second pretreated material with citric acid to obtain a mixture, calcine the mixture for the third time, and after cooling, obtain the third pretreated material; Step 4: The third pretreated material is washed with hydrochloric acid and dried to obtain the aluminosilicate material for water mineralization.
2. The preparation method according to claim 1, characterized in that, The concentration of hydrochloric acid in the first soaking is 0.05-0.2 mol / L.
3. The preparation method according to claim 2, characterized in that, The soaking time in hydrochloric acid in the first soaking is 3-4 hours.
4. The preparation method according to claim 1, characterized in that, The soaking time of the hydrogen peroxide solution in the first soaking is 3-4 hours.
5. The preparation method according to claim 1, characterized in that, In the second soaking, the solid-liquid mass ratio of the solid-liquid mixture obtained after mixing the first pretreated material with hydrochloric acid is 1:15-1:
25.
6. The preparation method according to claim 5, characterized in that, The first calcination is carried out in a muffle furnace at a temperature of 380℃-430℃ for 1.5-2.5 hours.
7. The preparation method according to claim 6, characterized in that, The second roasting is carried out in a muffle furnace at a temperature of 310℃-360℃ for a duration of 0.8-1.2 hours.
8. The preparation method according to claim 1, characterized in that, The third roasting is carried out in a tube furnace. First, the tubes of the tube furnace are evacuated to a vacuum, and then steam is introduced into the tubes. The roasting temperature is 400℃-500℃, and the roasting time is 2-4 hours.
9. The preparation method according to claim 1, characterized in that, The aluminosilicate minerals include quartz diorite, zeolite, mica, illite, or montmorillonite.
10. A silicate material for water mineralization, characterized in that, The aluminosilicate material for water mineralization is prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
Purified filtering agent for seawater desalination by using natural mineral
CN101049984A
Modification treatment method of Y-type zeolite
CN104628010A