Multiple exposure method for fabricating semiconductor devices
Self-aligned triple patterning (SATP) simplifies the process flow in semiconductor device fabrication, reduces the number of steps and material requirements, lowers costs, and improves pattern density and yield, solving the problems of complexity and high cost of traditional SAQP processes.
Patent Information
- Application Number
- CN202111417086.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-11-26
AI Technical Summary
In existing semiconductor device fabrication, the self-aligned quadruple patterning (SAQP) process is complex and costly, requiring 16 sub-steps, including multiple deposition and etching processes.
The self-aligned triple patterning process (SATP) is adopted. By forming a predetermined photoresist pattern on the semiconductor substrate, depositing an insulating layer stepwise and performing four etching processes, it is simplified to 11 sub-steps, including 4 deposition layer processes, 1 photomask setting and 2 insulating layer deposition processes, for a total of 11 sub-steps. Multiple deposition processes are eliminated and only continuous etching is performed.
The process was simplified, the manufacturing cost was reduced, and the target pitch was reduced to 1/3, which improved the pattern density and integration, and increased the yield.
Smart Images

Figure CN116190213B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor device fabrication technology, and in particular to a multiple exposure method for fabricating semiconductor devices. Background Technology
[0002] In existing semiconductor device fabrication, self-aligned quadruple patterning (SAQP) is commonly used, such as... Figure 2 As shown, this process involves 16 sub-steps. In the figure: the effect of the first sub-image requires 6 deposition process sub-steps and 1 photomask setting sub-step; the effect of the second sub-image requires 1 etching sub-step and 1 deposition process sub-step based on the previous sub-image; the effect of the third sub-image requires 1 etching sub-step and 1 core removal sub-step based on the previous sub-image; the effect of the fourth sub-image requires 1 etching sub-step based on the previous sub-image; the effect of the sixth sub-image requires 1 core removal sub-step and 1 etching sub-step based on the previous sub-image; that is, a total of 16 sub-steps are involved.
[0003] The main preparation process in the existing technology is to first perform a deposition process (dep spacer), then an etching process (etch), then perform another deposition process (dep spacer), and then an etching process (etch) to form the SAQP effect. Such process steps are complex and too costly. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a multiple exposure method for fabricating semiconductor devices, comprising the following steps:
[0005] On a semiconductor substrate with multiple deposited layers, a predetermined photoresist pattern is formed by a patterning process, and the predetermined photoresist pattern is used as a first photomask.
[0006] Two insulating layers are deposited stepwise on the first photolithography mask to form the first insulating layer and the second insulating layer in sequence.
[0007] The first etching process removes a layer of the second insulating layer vertically downwards, exposing a portion of the first insulating layer.
[0008] The first insulating layer is removed vertically downwards through a second etching process, and the remaining first insulating layer and second insulating layer form a predetermined insulating layer pattern, which is then used as a second photomask.
[0009] Through a third etching process, the patterns of the first photomask and the second photomask are transferred to at least one deposition layer adjacent to the first photomask and the second photomask in the multilayer deposition layer;
[0010] Through a fourth etching process, the pattern of at least one deposited layer adjacent to the first and second photomasks is transferred to at least one deposited layer in the multilayer deposition layers that is far away from the first and second photomasks.
[0011] Optionally, the semiconductor substrate pre-deposited with multiple deposition layers is a semiconductor substrate pre-deposited with four deposition layers.
[0012] Optionally, the patterns of the first and second photomasks are transferred to the two deposition layers adjacent to the first and second photomasks in the four deposition layers through a third etching process.
[0013] Optionally, a fourth etching process is used to transfer the pattern of the two deposited layers adjacent to the first and second photomasks to two deposited layers away from the first and second photomasks.
[0014] Optionally, the width of the first photolithographic mask is half the target midpoint; the spacing between the first photolithographic masks is at least twice the target midpoint.
[0015] Optionally, the spacing between the first photolithographic masks is two and a half times the target center distance.
[0016] Optionally, the etching selectivity ratio of the first photomask, the first insulating layer, and the second insulating layer is in the range of 5 to ∞: 1: 5 to ∞.
[0017] Optionally, the material composition of both the first insulating layer and the second insulating layer includes silicides.
[0018] Optionally, the four pre-deposited layers are, in order from the distance away from the first photomask and the second photomask to the distance from the distance to the distance to the distance to the first photomask and the second photomask, the first deposition layer, the second deposition layer, the third deposition layer, and the fourth deposition layer;
[0019] The material of the first deposited layer includes silicon dioxide;
[0020] The material of the second deposited layer includes polycrystalline silicon;
[0021] The material of the third deposition layer includes carbon;
[0022] The material of the fourth deposition layer includes silicon oxynitride.
[0023] Optionally, the thickness of the second deposition layer is equal to the sum of the thickness of the third deposition layer and the thickness of the fourth deposition layer.
[0024] Optionally, in the third etching process, a fluorocarbon compound is used to adjust the etching selectivity range of the first photomask, the first insulating layer, and the second insulating layer to 5~∞:1:5~∞.
[0025] The multi-exposure method for fabricating semiconductor devices of the present invention replaces the traditional self-aligned quadruple patterning process (SAQP) with a self-aligned triple patterning process (SATP). Step S100 includes four deposition layer process steps, one photomask setting process step, and two insulating layer deposition process steps. Steps S200-500 each include one etching process step, for a total of 11 steps. Based on step S100, starting from step S200, there is no need to interleave deposition processes; instead, four consecutive etching steps are performed to achieve the target effect. Traditional SAQP interleaves deposition processes between multiple etching steps and requires more etching cycles. The present invention reduces the 16 steps of traditional SAQP to the 11 steps of SATP, which can reduce the target pitch to 1 / 3, simplifying the process and saving fabrication costs.
[0026] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other advantages of the invention may be realized and obtained by means of the structures particularly pointed out in the written description, claims, and drawings.
[0027] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0028] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings:
[0029] Figure 1 This is a flowchart of a multiple exposure method for fabricating semiconductor devices according to an embodiment of the present invention;
[0030] Figure 2 This is a schematic diagram illustrating the effect of the traditional Self-Aligned Quadruple Patterning (SAQP) process.
[0031] Figure 3 This is a schematic diagram showing the effect formed after steps S100 and S200 in an embodiment of the multiple exposure method for preparing semiconductor devices according to the present invention;
[0032] Figure 4This is a schematic diagram of the effect formed after step S300 in an embodiment of the multiple exposure method for fabricating semiconductor devices of the present invention;
[0033] Figure 5 This is a schematic diagram showing the effect formed after step S400 in an embodiment of the multiple exposure method for fabricating semiconductor devices according to the present invention.
[0034] Figure 6 This is a schematic diagram of the effect formed after step S500 in an embodiment of the multiple exposure method for preparing semiconductor devices according to the present invention;
[0035] Figure 7 This is a schematic diagram of the effect formed after step S600 in an embodiment of the multiple exposure method for preparing semiconductor devices according to the present invention;
[0036] Figure 8 This diagram illustrates the optimal application range of the multiple exposure method for fabricating semiconductor devices according to the present invention, replacing SAQP. Detailed Implementation
[0037] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0038] like Figure 1 and Figure 3-7 As shown, this embodiment of the invention provides a multiple exposure method for fabricating semiconductor devices, comprising the following steps:
[0039] S100 On a semiconductor substrate 1 pre-deposited with multiple layers of deposition, a predetermined photoresist pattern is formed by a patterning process, and the predetermined photoresist pattern is used as a first photomask 6.
[0040] S200 deposits two insulating layers in stages on the first photolithography mask, sequentially forming the first insulating layer 7 and the second insulating layer 8; the effect is as follows: Figure 3 As shown;
[0041] S300 uses a first etching process to vertically remove a layer of the second insulating layer 8 at a thickness not less than one layer of the second insulating layer 8, exposing a portion of the first insulating layer 7; the resulting effect is as follows: Figure 4 As shown;
[0042] S400 removes the exposed first insulating layer vertically downwards through a second etching process. The remaining first and second insulating layers form a predetermined insulating layer pattern, which is then used as a second photolithography mask. The resulting effect is as follows: Figure 5 As shown;
[0043] S500 uses a third etching process to transfer the patterns of the first and second photomasks to at least one deposition layer adjacent to the first and second photomasks in the multilayer deposition layers; as... Figure 6 The image shows the transfer to two adjacent sedimentary layers among the four sedimentary layers, namely the third and fourth sedimentary layers;
[0044] S600 uses a fourth etching process to transfer the pattern of at least one deposited layer adjacent to the first and second photomasks to at least one deposited layer in the multilayer deposition layers that is far from the first and second photomasks; as Figure 7 The image shows the deposition layer being transferred downwards to a second deposition layer.
[0045] The working principle and beneficial effects of the above technical solution are as follows: This solution differs from the traditional self-aligned quadruple patterning process (SAQP) and adopts a self-aligned triple patterning process (SATP). Taking a four-layer deposition layer as an example, it only requires 11 sub-steps to achieve the effect of the traditional self-aligned quadruple patterning process (SAQP). Step S100 includes 4 deposition layer process sub-steps and 1 photolithography mask setting process sub-step. Step S200 includes 2 insulating layer deposition process sub-steps. Steps S300-600... Each step in SATP includes one etching process sub-step, for a total of 11 sub-steps. Based on steps S100 and S200, starting from step S300, there is no need to intersperse deposition processes; instead, four consecutive etching steps are performed to achieve the target effect. Traditional SAQP intersperses deposition processes between multiple etching steps and requires more etching steps. This solution reduces the 16 sub-steps of traditional SAQP to 11 sub-steps of SATP, which can reduce the target pitch to 1 / 3. This simplifies the process and saves on preparation costs.
[0046] In one embodiment, such as Figure 3-5 As shown, four deposition layers are pre-deposited on semiconductor substrate 1;
[0047] like Figure 6 As shown, through the third etching process, the patterns of the first photomask and the second photomask are transferred to the two deposition layers adjacent to the first photomask and the second photomask in the four deposition layers;
[0048] like Figure 7 As shown, through the fourth etching process, the pattern of the two deposited layers adjacent to the first photomask and the second photomask is transferred to the two deposited layers away from the first photomask and the second photomask.
[0049] The working principle and beneficial effects of the above technical solution are as follows: This solution pre-deposits four deposition layers on the semiconductor substrate. During the third etching process, the first and second photomasks are removed, and the two deposition layers adjacent to the first and second photomasks that are not blocked by them are also removed, thus realizing the transfer of the pattern formed by the first and second photomasks. During the fourth etching process, the two deposition layers that were originally blocked by the first and second photomasks but were not removed during the third etching form a new etching mask. The fourth etching removes the remaining two upper deposition layers and removes the two unblocked deposition layers adjacent to the upper layers, thus realizing the pattern transfer once again. Finally, the required pattern density is formed.
[0050] In one embodiment, such as Figure 3 As shown, in step S100, the width of the first photomask is half of the target midpoint; the spacing between the first photomasks is at least twice the target midpoint, preferably, the spacing between the first photomasks is two and a half times the target midpoint.
[0051] The working principle and beneficial effects of the above technical solution are as follows: This solution limits the width and spacing of the photolithography mask, where spacing refers to the gap width between two objects; this solution uses the target pitch as a reference for setting, where pitch refers to the center distance between two objects, and the target pitch is the target pattern formed after the S600 step (i.e., Figure 7 The distance between the centers of adjacent units remaining in the second deposition layer is the sum of the spacing between adjacent units and the width of one unit; the target pitch is determined according to the design, and the target pitch data can be different for different products, that is, it can be flexibly controlled as needed; this limitation intuitively reflects the relationship between the photolithography mask setting and the influence on pattern design and fabrication in SATP. This invention can reduce the pitch of the final pattern to one-third of the pitch of the first photolithography mask, thereby increasing the pattern density and improving the integration.
[0052] In one embodiment, the first insulating layer and the second insulating layer are made of SiO2 and SiN materials, respectively, and the first photomask is made of PR material.
[0053] The working principle and beneficial effects of the above technical solution are as follows: This solution limits the material types of the first photomask, the first insulating layer and the second insulating layer, thereby determining the etching selectivity of the three, thus ensuring the completion quality of the S300 and S400 steps, and further ensuring the final effect after the 600 steps, which can improve the yield of the prepared products.
[0054] In one embodiment, in step S100, four deposition layers may be used, as shown in the example where the four deposition layers are formed sequentially through four deposition processes; such as Figure 3-6 As shown, the four deposition layers on the upper surface of wafer 1 are, from the distance away from the first photomask and the second photomask to the distance to the distance to the first photomask and the second photomask (i.e. from bottom to top in the figure), the first deposition layer 2, the second deposition layer 3, the third deposition layer 4 and the fourth deposition layer 5.
[0055] The material of the first deposited layer 2 includes silicon dioxide (SiO2);
[0056] The material of the second deposited layer 3 includes polycrystalline silicon;
[0057] The material of the third deposition layer 4 includes carbon.
[0058] The material of the fourth deposition layer 5 includes silicon oxynitride (SiON);
[0059] Preferably, the thickness of the second deposition layer 3 is equal to the sum of the thickness of the third deposition layer 4 and the thickness of the fourth deposition layer 5.
[0060] The working principle and beneficial effects of the above technical solution are as follows: In the early stages of the process, compared with the traditional SAQP process, this solution can reduce two deposition layers on the upper surface of the wafer, requiring only four deposition layers, thereby reducing material requirements and lowering the manufacturing cost; by setting the thickness of the second deposition layer to be equal to the sum of the thicknesses of the third and fourth deposition layers, it can be ensured that the first deposition layer will not be damaged during the fourth etching step of the 600 steps, and all residual parts of the third and fourth deposition layers can be removed, thus ensuring process quality and effect.
[0061] In one embodiment, in the third etching process, a fluorocarbon compound is used to adjust the etching selectivity range of the first photomask, the first insulating layer, and the second insulating layer to 5 to ∞: 1: 5 to ∞.
[0062] The working principle and beneficial effects of the above technical solution are as follows: The fluorocarbon compound in this solution can be trifluoromethane (CHF3) gas. The fluorocarbon compound is used to adjust the polymer used for etching, so that the etching selectivity range of the first photomask, the first insulating layer and the second insulating layer is adjusted to 5~∞:1:5~∞, so that the surface of the etched product is smooth, thereby ensuring product performance, improving product yield, reducing production costs and ensuring process quality and effect.
[0063] The multi-exposure process (SATP) for semiconductor device fabrication of the present invention simplifies the process flow, such as... Figure 8As shown, the present invention is most effective in replacing the traditional SAQP process in the 26nm to 38nm range.
[0064] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.
Claims
1. A multiple exposure method for fabricating semiconductor devices, characterized in that, Includes the following steps: On a semiconductor substrate pre-deposited with four deposition layers, a predetermined photoresist pattern is formed by a patterning process, and the predetermined photoresist pattern is used as a first photomask; the width of the first photomask is half of the target center distance; The first photolithographic mask spacing is at least twice the target center distance; the target center distance is the distance between the centers of each adjacent unit remaining in the deposition layer of the target pattern formed after the fourth etching process; Two insulating layers are deposited stepwise on the first photolithography mask to form the first insulating layer and the second insulating layer in sequence. The first etching process removes a layer of the second insulating layer vertically downwards, exposing a portion of the first insulating layer. The first insulating layer is removed vertically downwards through a second etching process, and the remaining first insulating layer and second insulating layer form a predetermined insulating layer pattern, which is then used as a second photomask. The four pre-deposited layers are, in order from the distance away from the first and second photomasks to the distance from the first and second photomasks, the first, second, third, and fourth deposition layers; the thickness of the second deposition layer is equal to the sum of the thicknesses of the third and fourth deposition layers; Through a third etching process, the patterns of the first photomask and the second photomask are transferred to the third and fourth deposition layers adjacent to the first and second photomasks in the four deposition layers. Through the fourth etching process, the pattern of at least one deposition layer adjacent to the first and second photomasks is transferred to the second deposition layer in the four deposition layers that is far away from the first and second photomasks.
2. The multiple exposure method for fabricating semiconductor devices according to claim 1, characterized in that, The pattern of the two deposition layers adjacent to the first and second photomasks is transferred to the two deposition layers away from the first and second photomasks through the fourth etching process.
3. The multiple exposure method for fabricating semiconductor devices according to claim 1, characterized in that, The spacing between the first photolithographic masks is two and a half times the center distance of the target.
4. The multiple exposure method for fabricating semiconductor devices according to claim 1, characterized in that, The etching selectivity ratio of the first photomask, the first insulating layer, and the second insulating layer is in the range of 5 to ∞: 1: 5 to ∞.
5. The multiple exposure method for fabricating semiconductor devices according to claim 1, characterized in that, Both the first insulating layer and the second insulating layer contain silicides in their material composition.
6. The multiple exposure method for fabricating semiconductor devices according to claim 1, characterized in that, The material of the first deposited layer includes silicon dioxide; The material of the second deposited layer includes polycrystalline silicon; The material of the third deposition layer includes carbon; The material of the fourth deposition layer includes silicon oxynitride.
7. The multiple exposure method for fabricating semiconductor devices according to claim 6, characterized in that, In the third etching process, a fluorocarbon compound is used to adjust the etching selectivity range of the first photomask, the first insulating layer, and the second insulating layer to 5~∞:1:5~∞.
Citation Information
Patent Citations
Method for forming semiconductor device
CN113380704A
Semiconductor patterning process
US20210351036A1