Flame retardant nylon and preparation method thereof
By introducing phosphorus-nitrogen-silicon crosslinked polymers and transesterification reactions into nylon materials to form β-hydroxy ester bonds, and combining the flame-retardant mechanism of DOPO and silicon-oxygen-silicon structures, the problems of nylon's flammability and dripping are solved, achieving highly efficient flame retardancy and drip-free combustion performance.
Patent Information
- Application Number
- CN202310247143.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-03-10
AI Technical Summary
Nylon materials are flammable and drip molten material when burning, posing a fire hazard. They need to be modified to improve flame retardant properties and prevent dripping.
By introducing phosphorus-nitrogen-silicon crosslinked polymers into nylon, β-hydroxy ester bonds are formed through transesterification, which increases the matrix melt strength and prevents molten droplets from falling. Furthermore, the limiting oxygen index is improved through the gas-phase flame retardant effect of DOPO and the condensed-phase flame retardant effect of the silicon-oxygen-silicon structure.
It achieves highly efficient flame retardancy of nylon materials, with a limiting oxygen index greater than 30%, UL-94 V0 rating, and no molten dripping during combustion, significantly improving the safety of the material.
Smart Images

Figure CN116200027B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of flame retardant synthesis and application thereof, and in particular to a flame retardant nylon and a preparation method thereof. Background Art
[0002] Nylon (nylon 6), chemically known as polycaprolactam, is a polymer characterized by repeating amide groups in its main chain molecular structure. It is also one of the most common engineering plastics in our daily lives. It is a translucent or opaque milky white crystalline polymer with excellent electrical properties, heat resistance, wear resistance, electrical insulation, chemical resistance, and self-lubrication. Its low coefficient of friction and ease of processing make it widely used in various fields, including transportation, electronics, machinery, aerospace, and aviation. However, nylon's molecular structure contains large amounts of carbon and hydrogen, making it highly flammable in air. Its limiting oxygen index is only about 23%, and combustion is accompanied by large amounts of molten droplets. Vertical combustion cannot reach any level, and fires may occur during use, posing a significant threat to human life and property. Therefore, it must be flame-retardant modified.
[0003] In recent years, flame retardants (vitrimers) have become a hot topic of research. Vitrimers are materials with three-dimensional network structures based on covalent bonds. These bonds can undergo reversible breakage and reformation under external stimuli, while the degree of crosslinking remains virtually unchanged during this process. Therefore, vitrimers have excellent reproducibility and crosslink integrity. Types of reversible covalent reactions used in adaptive networks include ester exchange, transamination, and disulfide exchange. Among them, the ester exchange-type glass-like polymer developed by Leibler is based on the reaction of ester bonds with hydroxyl groups and is the most common of all bond exchange types. The basic characteristics of networks based on ester exchange are simple preparation, good thermal stability, and good chemical stability. Summary of the Invention
[0004] The technical problem to be solved by the technical solution of this application is to provide a flame-retardant nylon material with better performance, which has the characteristics of flame retardancy and no melting dripping when burning.
[0005] One aspect of the present application provides a flame-retardant nylon, comprising: nylon; a phosphorus-nitrogen-silicon cross-linked polymer, wherein the phosphorus-nitrogen-silicon cross-linked polymer is a reaction product of a phosphorus-nitrogen diacid monomer and a silicon-containing epoxy monomer in the presence of a catalyst, and comprises a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group; and a product of a melt-mixing reaction between the phosphorus-nitrogen-silicon cross-linked polymer and the nylon portion, wherein the product comprises an exchange product between the β-hydroxy ester bond and an amide bond in the nylon, and a chain extension product formed by the reaction of amino and carboxyl groups in the nylon, and hydroxyl groups in the phosphorus-nitrogen-silicon cross-linked polymer with epoxy groups.
[0006] In some embodiments of the present application, the phosphorus-nitrogen diacid monomer comprises:
[0007]
[0008] or
[0009]
[0010] In some embodiments of the present application, the silicon-containing epoxy monomer includes: or
[0011]
[0012] In some embodiments of the present application, the catalyst includes any one of zinc acetate, zinc acetylacetonate, triethanolamine, N-methylimidazole, 1-methylimidazole, 2-methylimidazole, 1,2-dimethylimidazole, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
[0013] In some embodiments of the present application, the mass percentage of the nylon is 40% to 60%, the mass percentage of the phosphorus-nitrogen-silicon cross-linked polymer is 5 to 10%, and the mass percentage of the product of the melt mixing reaction of the phosphorus-nitrogen-silicon cross-linked polymer and the nylon portion is 20 to 30%.
[0014] Another aspect of the present application provides a method for preparing flame-retardant nylon, comprising: allowing a carboxyl-containing aldehyde compound to chemically react with a polyamino compound to generate a carboxyl-containing Schiff base intermediate, then allowing the Schiff base intermediate to react with DOPO to generate a phosphorus-nitrogen diacid monomer; allowing a disiloxane derivative to chemically react with glycidol and an acid-binding agent to generate a silicon-containing epoxy monomer; allowing the phosphorus-nitrogen diacid monomer and the silicon-containing epoxy monomer to react under the action of a catalyst to generate a phosphorus-nitrogen-silicon cross-linked polymer, wherein the phosphorus-nitrogen-silicon cross-linked polymer includes a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group; and melt-mixing the dried phosphorus-nitrogen-silicon cross-linked polymer with dried nylon to form the flame-retardant nylon.
[0015] In some embodiments of the present application, the carboxyl-containing aldehyde compound includes any one or a combination of 4-formylbenzoic acid, 4-formyl-3-hydroxybenzoic acid, 4-formyl-3-nitrobenzoic acid, 5-formyl-2-thiophenecarboxylic acid, 5-formyl-2-furancarboxylic acid and 2,4-dimethyl-5-formyl-1H-pyrrole-3-carboxylic acid.
[0016] In some embodiments of the present application, the polyamino compound includes any one or a combination of hexamethylenediamine, 1,4-cyclohexanediamine, p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 2,5-bis(aminomethyl)furan, 2,4-diaminopyrimidine, 2,2'-diaminodiphenyl disulfide, 2,6-diaminoanthraquinone and 2,6-diaminopyridine.
[0017] In some embodiments of the present application, the disiloxane derivative includes any one or a combination of 1,3-dichlorotetramethyldisiloxane, 1,3-bis(chloromethyl)tetramethyldisiloxane, hexachlorodisiloxane and 1,3-dichloro-1,3-diphenyl-1,3-dimethyldisiloxane.
[0018] In some embodiments of the present application, the acid binding agent includes one or more of triethylamine, pyridine, N,N-diisopropylethylamine (DIEA), sodium hydroxide, potassium carbonate and sodium carbonate.
[0019] In some embodiments of the present application, the molar ratio of the phosphorus-nitrogen diacid monomer, the silicon-containing epoxy monomer, and the catalyst is 1:(1-1.5):(0.03-0.12).
[0020] In some embodiments of the present application, the phosphorus-nitrogen-containing diacid monomer and the silicon-containing epoxy monomer react under a catalyst to form a phosphorus-nitrogen-silicon cross-linked polymer under the following reaction conditions: curing at 100-200° C. for 5-12 hours.
[0021] In some embodiments of the present application, the catalyst includes any one of zinc acetate, zinc acetylacetonate, triethanolamine, N-methylimidazole, 1-methylimidazole, 2-methylimidazole, 1,2-2-methylimidazole, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
[0022] In some embodiments of the present application, the molar ratio of the carboxyl-containing aldehyde compound to the polyamino compound is in the range of 2:1 to 4:1, and the molar ratio of the Schiff base intermediate to DOPO is in the range of 1:1 to 1:1.1.
[0023] In some embodiments of the present application, the molar ratio of the disiloxane derivative, glycidol, and acid binding agent is in a range of 1:2:2 to 1:4:4.
[0024] Compared with the existing technology, the technical solution of this application has the following beneficial effects:
[0025] The phosphorus-nitrogen-silicon cross-linked polymer flame-retardant nylon described in the present application has a limiting oxygen index greater than 30%, a UL-94 V0 rating, and no molten droplets fall during combustion. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is the phosphorus-nitrogen diacid monomer product 1 in Example 1 1 H NMR spectrum.
[0027] Figure 2 is the phosphorus-nitrogen diacid monomer product 1 in Example 1 31 P NMR spectrum. DETAILED DESCRIPTION
[0028] The following description provides specific application scenarios and requirements of the present application, with the purpose of enabling those skilled in the art to make and use the content of this application. Various local modifications to the disclosed embodiments will be apparent to those skilled in the art, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of this application. Therefore, this application is not limited to the embodiments shown, but is intended to be of the widest scope consistent with the claims.
[0029] On the one hand, the present application provides a flame-retardant nylon, comprising: nylon; a phosphorus-nitrogen-silicon cross-linked polymer, wherein the phosphorus-nitrogen-silicon cross-linked polymer is a reaction product of a phosphorus-nitrogen-containing diacid monomer and a silicon-containing epoxy monomer in the presence of a catalyst, and comprises a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group; and a product of a melt-kneading reaction between the phosphorus-nitrogen-silicon cross-linked polymer and the nylon portion, wherein the product comprises an exchange product between the β-hydroxy ester bond and the amide bond in the nylon.
[0030] In some embodiments of the present application, the phosphorus-nitrogen diacid monomer includes two or more carboxyl groups and a DOPO structure added by a Schiff base, wherein the DOPO is 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and the structural formula is
[0031] In some embodiments of the present application, the phosphorus-nitrogen diacid monomer comprises
[0032]
[0033] or
[0034]
[0035] In some embodiments of the present application, the silicon-containing epoxy monomer includes: or
[0036]
[0037] In some embodiments of the present application, the catalyst includes any one of zinc acetate, zinc acetylacetonate, triethanolamine, N-methylimidazole, 1-methylimidazole, 2-methylimidazole, 1,2-dimethylimidazole, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
[0038] In some embodiments of the present application, the mass percentage of the nylon is 40% to 60%, for example, 45%, 50%, 55%, etc.; the mass percentage of the phosphorus-nitrogen-silicon cross-linked polymer is 5 to 10%, for example, 6%, 8%, 9%, etc., and the mass percentage of the product of the melt-mixing reaction of the phosphorus-nitrogen-silicon cross-linked polymer and the nylon portion is 20 to 30%, for example, 25%, 28%, etc.
[0039] In the embodiment of the present application, the phosphorus-nitrogen-silicon cross-linked polymer may include a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group, and may further include multiple DOPO and silicon-oxygen-silicon structures added by a Schiff base, for example:
[0040]
[0041] The DOPO therein exerts a gas phase flame retardant effect during the combustion process of the flame retardant nylon, releasing PO to interrupt the chain reaction, and the silicon-oxygen-silicon structure exerts a condensed phase flame retardant effect to isolate heat and combustible gases.
[0042] During the melt mixing process, the phosphorus-nitrogen-silicon crosslinked polymer and the nylon portion undergo a melt mixing reaction, wherein the reaction product includes an exchange product between the β-hydroxy ester bond and the amide bond in the nylon. The exchange product between the β-hydroxy ester bond and the amide bond in the nylon increases the melt strength of the matrix and prevents dripping.
[0043] Furthermore, during the melt mixing process, the nylon's end groups (amino and carboxyl groups) and the hydroxyl groups in the phosphorus-nitrogen-silicon crosslinked polymer can react with epoxy groups to form chain extension products. These chain extension products can increase the matrix melt strength and prevent dripping. The flame-retardant nylon has a limiting oxygen index greater than 30%, a UL-94 V0 rating, and exhibits zero dripping during combustion.
[0044] On the other hand, the present application provides a method for preparing flame-retardant nylon, comprising:
[0045] Step S1, preparing a phosphorus-nitrogen diacid monomer: chemically reacting a carboxyl-containing aldehyde compound with a polyamino compound to generate a carboxyl-containing Schiff base intermediate, and then reacting the Schiff base intermediate with DOPO to generate a phosphorus-containing diacid monomer;
[0046] Step S2, preparing a silicon-containing epoxy monomer: chemically reacting a disiloxane derivative with glycidol and an acid-binding agent to generate a silicon-containing epoxy monomer;
[0047] Step S3, reacting a phosphorus-nitrogen diacid monomer and a silicon-containing epoxy monomer in the presence of a catalyst to generate a phosphorus-nitrogen-silicon crosslinked polymer, wherein the phosphorus-nitrogen-silicon crosslinked polymer includes a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group;
[0048] Step S4: vacuum-drying and grinding the phosphorus-nitrogen-silicon cross-linked polymer, and then melt-mixing it with dried nylon to form the flame-retardant nylon.
[0049] The preparation method of the flame retardant nylon is further described in detail below.
[0050] In step S1, the carboxyl-containing aldehyde compound includes any one or more combinations of 4-formylbenzoic acid, 4-formyl-3-hydroxybenzoic acid, 4-formyl-3-nitrobenzoic acid, 5-formyl-2-thiophenecarboxylic acid, 5-formyl-2-furancarboxylic acid and 2,4-dimethyl-5-formyl-1H-pyrrole-3-carboxylic acid.
[0051] The polyamino compound includes one or more of hexamethylenediamine, 1,4-cyclohexanediamine, p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 2,5-bis(aminomethyl)furan, 2,4-diaminopyrimidine, 2,2'-diaminodiphenyl disulfide, 2,6-diaminoanthraquinone and 2,6-diaminopyridine.
[0052] The molar ratio of the carboxyl-containing aldehyde compound and the polyamino compound is in the range of 2:1 to 4:1. Optionally, the molar ratio of the carboxyl-containing aldehyde compound and the polyamino compound is in the range of 2:1 to 3:1, for example, the molar ratio of the carboxyl-containing aldehyde compound and the polyamino compound is 2:1.
[0053] In one embodiment of the present application, 2 molar equivalents of a carboxyl-containing aldehyde compound in a solvent are added dropwise to 1 molar equivalent of a polyamino compound in a solvent, and the reaction is carried out at 25-110°C for 1-8 hours to obtain a carboxyl-containing Schiff base intermediate. Schiff bases, also known as azomethines, are relatively stable imines with an alkyl or aryl group attached to the nitrogen atom.
[0054] The reaction temperature of the carboxyl-containing aldehyde compound and the polyamino compound is preferably 40 to 80° C., and the reaction time is preferably 2 to 8 hours.
[0055] Subsequently, DOPO and the Schiff base intermediate are reacted at a temperature of 60 to 150° C. for 4 to 12 hours to prepare a phosphorus-nitrogen diacid monomer. The molar ratio of DOPO to the Schiff base intermediate is in the range of 1:1 to 1:1.3. Alternatively, the molar ratio of DOPO to the Schiff base intermediate is in the range of 1:1 to 1:1.1.
[0056] The DOPO is 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and its structural formula is
[0057]
[0058] The phosphorus-nitrogen diacid monomer includes two or more carboxyl groups and a DOPO structure added by a Schiff base, for example:
[0059]
[0060]
[0061] or
[0062] wait.
[0063] In step S2, the disiloxane derivative includes any one or more of 1,3-dichlorotetramethyldisiloxane, 1,3-bis(chloromethyl)tetramethyldisiloxane, hexachlorodisiloxane, 1,3-dichloro-1,1,3,3-tetraisopropyldisiloxane and 1,3-dichloro-1,3-diphenyl-1,3-dimethyldisiloxane.
[0064] The acid binding agent includes any one or more of triethylamine, pyridine, N,N-diisopropylethylamine (DIEA), sodium hydroxide, potassium carbonate and sodium carbonate.
[0065] The molar ratio of the disiloxane derivative to glycidol and the acid binding agent is in the range of 1:2:2 to 1:4:4. Alternatively, the molar ratio of the disiloxane derivative to glycidol and the acid binding agent is in the range of 1:2:2 to 1:3:3. For example, the molar ratio of the disiloxane derivative to glycidol and the acid binding agent is 1:2:2.
[0066] In one embodiment of the present application, 1 molar equivalent of a disiloxane derivative containing a solvent is added dropwise to 2 molar equivalents of glycidol, 2 molar equivalents of an acid-binding agent are added, and the reaction is carried out in an ice-water bath for 1 to 4 hours. The temperature is then raised to 40 to 80°C (preferably 40 to 60°C) and the reaction is continued for 4 to 8 hours (preferably 4 to 6 hours) to produce a silicon-containing epoxy monomer. The reaction in an ice-water bath for 1 to 4 hours prevents the volatilization of toxic gases generated during the reaction. After all toxic gases generated during the reaction are consumed by the reaction, the temperature is raised to 40 to 80°C and the reaction is continued.
[0067] In another embodiment of the present application, 1 molar equivalent of the disiloxane derivative is added dropwise to 2.5 molar equivalents of glycidol, 2.5 molar equivalents of an acid binding agent are added, and the mixture is reacted for 1 to 4 hours in an ice-water bath atmosphere, then the temperature is raised to 40 to 60° C. and the reaction is continued for 4 to 6 hours to prepare a silicon-containing epoxy monomer.
[0068] Wherein, the generated silicon-containing epoxy monomer includes:
[0069] or
[0070]
[0071] In step S3, a phosphorus-nitrogen diacid monomer and a silicon-containing epoxy monomer are reacted under the action of a catalyst to generate a phosphorus-nitrogen-silicon cross-linked polymer, wherein the phosphorus-nitrogen-silicon cross-linked polymer includes a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group; the catalyst includes any one of zinc acetate, zinc acetylacetonate, triethanolamine, N-methylimidazole, 1-methylimidazole, 2-methylimidazole, 1,2-2-methylimidazole, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
[0072] The molar ratio of the phosphorus-nitrogen diacid monomer, the silicon-containing epoxy monomer, and the catalyst is 1:(1-1.5):(0.03-0.12). Alternatively, the molar ratio of the phosphorus-nitrogen diacid monomer, the silicon-containing epoxy monomer, and the catalyst is 1:(1-1.2):(0.05-0.10). For example, the molar ratio of the phosphorus-nitrogen diacid monomer, the silicon-containing epoxy monomer, and the catalyst is 1:1:0.05.
[0073] In one embodiment of the present application, a phosphorus-nitrogen diacid monomer, a silicon-containing epoxy monomer, and a catalyst in a molar ratio of 1:1:0.05 are stirred and mixed by a solvent, and cured at 100-200°C (preferably 130-170°C) for 5-12 hours (preferably 6-8 hours). The carboxyl group reacts with the epoxy group to form an ester exchange reaction to form a β-hydroxy ester bond. The β-hydroxy ester bond can be reversibly broken and reorganized at high temperature to prepare a phosphorus-nitrogen-silicon cross-linked polymer.
[0074] Optionally, the process of curing the phosphorus-nitrogen diacid monomer and the silicon-containing epoxy monomer may include: pre-curing at a temperature of 100-140°C for 1-4 hours to ensure complete evaporation of the solvent, and then heating to 160-200°C for curing for 4-8 hours to ensure complete curing of the raw materials.
[0075] In step S1, step S2, and step S3 of the present application, the solvent is one or a mixture of methanol, ethanol, acetone, chloroform, dimethyl sulfoxide, 1,4-dioxane, toluene, and N,N-dimethylformamide.
[0076] The molecular structure of the phosphorus-nitrogen-silicon cross-linked polymer prepared in the examples of the present application includes a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group, and further includes multiple DOPO and silicon-oxygen-silicon structures added by a Schiff base, for example:
[0077]
[0078] The DOPO in it exerts a gas-phase flame retardant effect during the combustion process, releasing PO to interrupt the chain reaction, and the silicon-oxygen-silicon structure exerts a condensed-phase flame retardant effect, isolating heat and combustible gases.
[0079] Step S4: vacuum-drying and grinding the phosphorus-nitrogen-silicon cross-linked polymer, and melt-mixing it with the vacuum-dried nylon to form the flame-retardant nylon. The nylon may be nylon 6.
[0080] In some embodiments of the present application, the mass percentage of the phosphorus-nitrogen-silicon crosslinked polymer before melt-mixing with the nylon portion is 6 to 12%, and after melt-mixing with the nylon portion, the mass percentage of the phosphorus-nitrogen-silicon crosslinked polymer in the flame-retardant nylon described herein is 5 to 10%. The melt-mixing temperature range is 240 to 260°C.
[0081] In other embodiments of the present application, the phosphorus-nitrogen-silicon cross-linked polymer is vacuum dried at 80-100°C for 4-8 hours and ground for 5-10 minutes. Nylon 6 is vacuum dried at 80-110°C for 4-8 hours, and the phosphorus-nitrogen-silicon cross-linked polymer is melt-mixed with nylon 6 at a mass fraction of 8-10 to form a flame-retardant nylon with a limiting oxygen index greater than 30%, a UL-94 V0 rating, and no molten droplets during combustion. The improvement in flame retardancy is mainly attributed to the decomposition of DOPO during combustion to produce PO· free radicals, which can capture H· and OH· free radicals produced by nylon combustion, interrupting the chain reaction and achieving a gas-phase flame retardant effect. The combustion of the silicon-oxygen-silicon structure will form a physical barrier that covers the surface of the nylon matrix, isolating heat and combustible gases, and achieving a condensed-phase flame retardant effect.
[0082] During the melt mixing process, the phosphorus-nitrogen-silicon crosslinked polymer and the nylon portion undergo a melt mixing reaction, wherein the reaction product includes an exchange product between the β-hydroxy ester bond and the amide bond in the nylon. The exchange product between the β-hydroxy ester bond and the amide bond in the nylon increases the melt strength of the matrix and prevents dripping.
[0083] Furthermore, during the melt mixing process, the terminal groups (amino and carboxyl groups) of the nylon and the hydroxyl groups in the phosphorus-nitrogen-silicon cross-linked polymer can react with epoxy groups to form chain extension products. The chain extension products can increase the melt strength of the matrix and prevent molten dripping.
[0084] The following further describes the implementation of the present application in detail through Examples 1 to 10.
[0085] Example 1:
[0086] Under nitrogen protection, 15.13 g of 4-formylbenzoic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 9.92 g of 4,4-diaminodiphenylmethane (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. After that, a light yellow solid was obtained by filtration, washed three times with anhydrous ethanol, and dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 1, whose structure is shown below:
[0087]
[0088] From the attached Figure 1 It can be seen that 6.5-8.5 ppm is the proton absorption peak of the benzene ring, 5.0-6.0 is the proton peak on CH after DOPO addition, and 2.0-4.0 is the alkane proton peak on the aliphatic chain. These data indicate that the phosphorus-nitrogen diacid monomer product 1 was successfully synthesized.
[0089] From the attached Figure 2 It can be seen that the phosphorus absorption peaks at 28.0 and 30.2 ppm are caused by the addition of DOPO in the phosphorus-nitrogen diacid product 1, indicating that the phosphorus-nitrogen diacid monomer product 1 was successfully synthesized.
[0090] Under nitrogen protection, 14.82 g (0.2 mol) of glycidol and 20.24 g of triethylamine (0.2 mol) were placed in a 500 mL three-necked flask, 150 mL of tetrahydrofuran was added, and magnetic stirring was performed under ice-water bath conditions. A tetrahydrofuran solution containing 23.12 g of 1,3-bis(chloromethyl)tetramethyldisiloxane (0.1 mol) was added dropwise to the flask, and the reaction was continued for 2 h. The temperature was then raised to 50° C. and the reaction was continued for 6 h. The mixture was then extracted with dichloromethane / deionized water, and the organic phase was collected, dried over anhydrous magnesium sulfate, and the solvent was removed by rotary evaporation to obtain a disiloxane-containing epoxy monomer product 1, the structure of which is shown below:
[0091]
[0092] 1 mol equivalent of phosphorus-nitrogen diacid monomer product 1, 1.1 mol equivalent of disiloxane-containing epoxy monomer product 1 and 0.03 mol of zinc acetate were dissolved in chloroform, and cured at 120°C for 2 hours and at 170°C for 6 hours to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0093] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 92g of nylon 6 and 8g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 30.8%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0094] Example 2:
[0095] Under nitrogen protection, 15.13 g of 4-formylbenzoic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.51 g of 2,4-diaminopyrimidine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. Then, a white solid was obtained by filtration, washed three times with anhydrous ethanol, and dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 2, whose structure is shown below:
[0096]
[0097] 1 mol equivalent of phosphorus-nitrogen diacid monomer product 2, 1.2 mol equivalent of disiloxane-containing epoxy monomer product 1 and 0.05 mol of zinc acetate were dissolved in chloroform, and cured at 120°C for 2 hours and at 160°C for 6 hours to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0098] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 90g of nylon 6 and 10g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 31.0%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0099] Example 3:
[0100] Under nitrogen protection, 15.62 g of 5-formyl-2-thiophenecarboxylic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.41 g of p-phenylenediamine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. The white solid was then filtered off and washed three times with anhydrous ethanol. It was then dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 3, whose structure is shown below:
[0101]
[0102] Under nitrogen protection, 14.82 g (0.2 mol) of glycidol and 20.24 g of triethylamine (0.2 mol) were placed in a 500 mL three-necked flask, 150 mL of tetrahydrofuran was added, and magnetic stirring was performed under ice-water bath conditions. A tetrahydrofuran solution containing 20.32 g of 1,3-dichlorotetramethyldisiloxane (0.1 mol) was added dropwise to the flask, and the reaction was continued for 2 h. The temperature was then raised to 50° C. and the reaction was continued for 6 h. The mixture was then extracted with dichloromethane / deionized water, and the organic phase was collected, dried over anhydrous magnesium sulfate, and the solvent was removed by rotary evaporation to obtain a disiloxane-containing epoxy monomer product 2, the structure of which is shown below:
[0103]
[0104] 1 mol equivalent of phosphorus-nitrogen diacid monomer product 3, 1.2 mol equivalent of disiloxane-containing epoxy monomer product 2 and 0.10 mol of zinc acetate acetonate were dissolved in chloroform, and cured at 130°C for 2 hours and at 160°C for 5 hours to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0105] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 91g of nylon 6 and 9g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 30.6%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0106] Example 4:
[0107] Under nitrogen protection, 15.62 g of 5-formyl-2-thiophenecarboxylic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.51 g of 2,4-diaminopyrimidine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. The white solid was then filtered off and washed three times with anhydrous ethanol. It was then dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 4, whose structure is shown below:
[0108]
[0109] 1 mol equivalent of phosphorus-nitrogen diacid monomer product 4, 1.2 mol equivalent of disiloxane-containing epoxy monomer product 2 and 0.06 mol of zinc acetylacetonate were dissolved in chloroform and cured at 130°C for 2 hours and at 170°C for 5 hours to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0110] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 92g of nylon 6 and 8g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 31.4%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0111] Example 5:
[0112] Under nitrogen protection, 16.72 g of 2,4-dimethyl-5-formyl-1H-pyrrole-3-carboxylic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.41 g of p-phenylenediamine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. The white solid was then filtered off and washed three times with anhydrous ethanol. It was then dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 5, whose structure is shown below:
[0113]
[0114] Under nitrogen protection, 14.82 g (0.2 mol) of glycidol and 20.24 g of triethylamine (0.2 mol) were placed in a 500 mL three-necked flask, 150 mL of tetrahydrofuran was added, and magnetic stirring was performed under ice-water bath conditions. A tetrahydrofuran solution containing 32.73 g of 1,3-dichloro-13-diphenyl-13-dimethyldisiloxane (0.1 mol) was added dropwise to the flask. The reaction was continued for 2 h, and then the temperature was raised to 50° C. and the reaction was continued for 6 h. The mixture was then extracted with dichloromethane / deionized water and the solvent was removed by rotary evaporation to obtain a disiloxane-containing epoxy monomer product 3, the structure of which is shown below:
[0115]
[0116] 1 mol equivalent of phosphorus-nitrogen dicarboxylic acid monomer product 5, 1.1 mol equivalent of disiloxane-containing epoxy monomer product 3, and 0.05 mol of 1,5,7-triazabicyclo[4.4.0]dec-5-ene were dissolved in chloroform, and cured at 120°C for 2 h and at 170°C for 4 h to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0117] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 90g of nylon 6 and 10g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 30.2%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0118] Example 6:
[0119] Under nitrogen protection, 15.13 g of 4-formylbenzoic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.82 g of hexamethylenediamine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. After filtration, a light yellow solid was obtained, which was washed three times with anhydrous ethanol and dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 6, whose structure is shown below:
[0120]
[0121] 1 mol equivalent of phosphorus-nitrogen diacid monomer product 1, 1.2 mol equivalent of disiloxane-containing epoxy monomer product 3 and 0.08 mol of zinc acetate were dissolved in chloroform, cured at 130°C for 2 hours and at 170°C for 5 hours to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0122] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 90g of nylon 6 and 10g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 31.2%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0123] Example 7:
[0124] Under nitrogen protection, 15.62 g of 5-formyl-2-thiophenecarboxylic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.82 g of hexamethylenediamine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. The white solid was then filtered off and washed three times with anhydrous ethanol. It was then dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 7, whose structure is shown below:
[0125]
[0126] Under nitrogen protection, 14.82 g (0.2 mol) of glycidol and 20.24 g of triethylamine (0.2 mol) were placed in a 500 mL three-necked flask, 150 mL of tetrahydrofuran was added, and magnetic stirring was performed under ice-water bath conditions. A tetrahydrofuran solution containing 28.48 g of hexachlorodisiloxane (0.1 mol) was added dropwise to the flask, and the reaction was continued for 2 h. The temperature was then raised to 50° C. and the reaction was continued for 6 h. The mixture was then extracted with dichloromethane / deionized water, and the organic phase was collected, dried over anhydrous magnesium sulfate, and the solvent was removed by rotary evaporation to obtain epoxy monomer product 4 containing disiloxane, the structure of which is shown below:
[0127]
[0128] 1 mol equivalent of phosphorus-nitrogen diacid monomer product 7, 1.1 mol equivalent of disiloxane-containing epoxy monomer product 4 and 0.06 mol of zinc acetylacetonate were dissolved in chloroform, and cured at 120°C for 2 h and at 170°C for 6 h to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0129] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 91g of nylon 6 and 9g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 31.4%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0130] Example 8:
[0131] Under nitrogen protection, 16.72 g of 2,4-dimethyl-5-formyl-1H-pyrrole-3-carboxylic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.82 g of hexamethylenediamine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. The white solid was then filtered off and washed three times with anhydrous ethanol. It was then dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 8, whose structure is shown below:
[0132]
[0133] 1 mol equivalent of phosphorus-nitrogen diacid monomer product 8, 1.1 mol equivalent of disiloxane-containing epoxy monomer product 4 and 0.05 mol of zinc acetylacetonate were dissolved in chloroform, cured at 130°C for 2 hours and at 170°C for 4 hours to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0134] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 90g of nylon 6 and 10g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 31.0%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0135] Example 9:
[0136] Under nitrogen protection, 15.13 g of 4-formylbenzoic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.71 g of cis-1,4-cycloethylenediamine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. After filtration, a light yellow solid was obtained, which was washed three times with anhydrous ethanol and dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 9, whose structure is shown below:
[0137]
[0138] Under nitrogen protection, 14.82 g (0.2 mol) of glycidol and 20.24 g of triethylamine (0.2 mol) were placed in a 500 mL three-necked flask, 150 mL of tetrahydrofuran was added, and magnetic stirring was performed under ice-water bath conditions. A tetrahydrofuran solution containing 31.54 g of 1,3-dichloro-1,1,3,3-tetraisopropyldisiloxane (0.1 mol) was added dropwise to the flask. The reaction was continued for 2 h, and then the temperature was raised to 50° C. and the reaction was continued for 6 h. The mixture was then extracted with dichloromethane / deionized water, and the organic phase was collected, dried over anhydrous magnesium sulfate, and the solvent was removed by rotary evaporation to obtain a disiloxane-containing epoxy monomer product 5, the structure of which is shown below:
[0139]
[0140] 1 mol equivalent of phosphorus-nitrogen dicarboxylic acid monomer product 9, 1.3 mol equivalent of disiloxane-containing epoxy monomer product 5, and 0.06 mol of 1,5,7-triazabicyclo[4.4.0]dec-5-ene were dissolved in chloroform and cured at 130°C for 2 h and at 170°C for 4 h to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0141] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours, and the phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 90g of nylon 6 and 10g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 31.2%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0142] Example 10:
[0143] Under nitrogen protection, 15.62 g of 5-formyl-2-thiophenecarboxylic acid (0.1 mol) was placed in a 500 mL three-necked flask, 250 mL of anhydrous ethanol was added, and the temperature was raised to 30°C with magnetic stirring. An anhydrous ethanol solution containing 5.71 g of cis-1,4-cycloethylenediamine (0.05 mol) was added dropwise to the flask, and the reaction was continued for 4 h. Then, 21.61 g of DOPO (0.1 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 8 h. The white solid was then filtered off and washed three times with anhydrous ethanol. It was then dried in vacuo at 80°C for 4 h to obtain the phosphorus-nitrogen diacid monomer product 10, whose structure is shown below:
[0144]
[0145] 1 mol equivalent of phosphorus-nitrogen diacid monomer product 10, 1.2 mol equivalent of disiloxane-containing epoxy monomer product 5, and 0.05 mol of 1,5,7-triazabicyclo[4.4.0]dec-5-ene were dissolved in chloroform and cured at 120°C for 2 h and at 170°C for 4 h to obtain a phosphorus-nitrogen-silicon cross-linked polymer.
[0146] Nylon 6 was dried in a forced-air drying oven at 100°C for 5 hours. The phosphorus-nitrogen-silicon crosslinked polymer was dried in a vacuum oven at 80°C for 6 hours. 91g of nylon 6 and 9g of the phosphorus-nitrogen-silicon crosslinked polymer were blended in an internal mixer and mixed at 240°C for 5 minutes to produce nylon 6. The resulting nylon 6 had a limiting oxygen index of 30.8%, achieved a UL-94 V0 rating, and exhibited no dripping during combustion.
[0147] Finally, it should be understood that the embodiments of the application disclosed herein are illustrations of the principles of the embodiments of the present application. Other modified embodiments are also within the scope of the present application. Therefore, the embodiments disclosed in the present application are merely examples and not limitations. Those skilled in the art can adopt alternative configurations based on the embodiments in the present application to implement the applications in the present application. Therefore, the embodiments of the present application are not limited to those embodiments that have been precisely described in the application.
Claims
1. A flame retardant nylon, characterized in that: include: nylon; A phosphorus-nitrogen-silicon crosslinked polymer, wherein the phosphorus-nitrogen-silicon crosslinked polymer is a reaction product of a phosphorus-nitrogen-containing diacid monomer and a silicon-containing epoxy monomer under the action of a catalyst, and includes a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group; and a product of a melt-kneading reaction between the phosphorus-nitrogen-silicon crosslinked polymer and the nylon portion, wherein the product includes an exchange product between the β-hydroxy ester bond and the amide bond in the nylon, and a chain extension product of an amino group and a carboxyl group in the nylon, a hydroxyl group in the phosphorus-nitrogen-silicon crosslinked polymer, and an epoxy group, the mass percentage of the nylon is 40% to 60%, the mass percentage of the phosphorus-nitrogen-silicon crosslinked polymer is 5 to 10%, and the mass percentage of the product of a melt-kneading reaction between the phosphorus-nitrogen-silicon crosslinked polymer and the nylon portion is 20 to 30%, wherein the phosphorus-nitrogen-containing diacid monomer includes: or The silicon-containing epoxy monomer comprises: or 2. The flame retardant nylon according to claim 1, characterized in that: The catalyst includes any one of zinc acetate, zinc acetylacetonate, triethanolamine, N-methylimidazole, 1-methylimidazole, 2-methylimidazole, 1,2-dimethylimidazole, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
3. A method for preparing flame retardant nylon, characterized in that: include: A carboxyl-containing aldehyde compound is chemically reacted with a polyamino compound to generate a carboxyl-containing Schiff base intermediate, and then the Schiff base intermediate is reacted with DOPO to generate a phosphorus-nitrogen-containing diacid monomer, wherein the carboxyl-containing aldehyde compound includes any one or a combination of 4-formylbenzoic acid, 4-formyl-3-hydroxybenzoic acid, 4-formyl-3-nitrobenzoic acid, 5-formyl-2-thiophenecarboxylic acid, 5-formyl-2-furancarboxylic acid and 2,4-dimethyl-5-formyl-1H-pyrrole-3-carboxylic acid; the polyamino compound includes Any one or a combination of hexamethylenediamine, 1,4-cyclohexanediamine, p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 2,5-bis(aminomethyl)furan, 2,4-diaminopyrimidine, 2,2'-diaminodiphenyl disulfide, 2,6-diaminoanthraquinone and 2,6-diaminopyridine; the molar ratio of the carboxyl-containing aldehyde compound to the polyamino compound is in the range of 2:1 to 4:1, and the molar ratio of the Schiff base intermediate to DOPO is in the range of 1:1 to 1:1.1; A disiloxane derivative, glycidol and an acid-binding agent are chemically reacted to generate a silicon-containing epoxy monomer, wherein the molar ratio of the disiloxane derivative, glycidol and the acid-binding agent is in the range of 1:2:2 to 1:4:4, and the disiloxane derivative includes any one of 1,3-dichlorotetramethyldisiloxane, 1,3-bis(chloromethyl)tetramethyldisiloxane, hexachlorodisiloxane and 1,3-dichloro-1,3-diphenyl-1,3-dimethyldisiloxane or a combination of more than one thereof; The phosphorus-nitrogen diacid monomer and the silicon-containing epoxy monomer are reacted under the action of a catalyst to generate a phosphorus-nitrogen-silicon crosslinked polymer, wherein the phosphorus-nitrogen-silicon crosslinked polymer includes a β-hydroxy ester bond formed by an ester exchange reaction between an epoxy group and a carboxyl group, and the molar ratio of the phosphorus-nitrogen diacid monomer, the silicon-containing epoxy monomer and the catalyst is 1:(1-1.5):(0.03-0.12); The dried phosphorus-nitrogen-silicon cross-linked polymer is melt-mixed with dried nylon to form the flame-retardant nylon, wherein the mass percentage of the nylon is 40% to 60%, the mass percentage of the phosphorus-nitrogen-silicon cross-linked polymer is 5 to 10%, and the mass percentage of the product of the melt-mixing reaction between the phosphorus-nitrogen-silicon cross-linked polymer and the nylon portion is 20 to 30%.
4. The method for preparing flame-retardant nylon according to claim 3, characterized in that: The acid binding agent includes one or a combination of triethylamine, pyridine, N,N-diisopropylethylamine, sodium hydroxide, potassium carbonate and sodium carbonate.
5. The method for preparing flame-retardant nylon according to claim 3, characterized in that: The catalyst includes any one of zinc acetate, zinc acetylacetonate, triethanolamine, N-methylimidazole, 1-methylimidazole, 2-methylimidazole, 1,2-dimethylimidazole, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
Citation Information
Patent Citations
Phosphor-nitrogen containing silane A, phosphite ester halogen-free flame retardant containing nitrogen phosphor silicon and preparation method of phosphite ester halogen-free flame retardant
CN103387589A
Phosphaphenanthrene-structure reactive fire retardant and application thereof
CN106554483A
Phosphaphenanthrene / phenylsiloxane double-base macromolecule and preparation method thereof
CN109438515A
NH2-POSS-bisDOPO flame retardant as well as preparation method and application thereof
CN112961359A
DOPO group-based compound containing silicon, phosphorus and nitrogen as well as preparation method and application of DOPO group-based compound
CN115073522A