A high performance die steel and a manufacturing method thereof

By adjusting the chemical composition and process flow of the mold steel, the problem of insufficient hardness and wear resistance of H13 steel under certain working conditions has been solved, the comprehensive performance of the mold steel has been improved, and its scope of use and life have been expanded.

CN116200660BActive Publication Date: 2024-10-22HEBEI UNIV OF ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211721319.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-22
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Traditional H13 steel has insufficient hardness, strength and wear resistance under certain working conditions, and cannot meet the needs of mold usage conditions and high production efficiency.

Method used

By adjusting the chemical composition, increasing the C, Ni, and W contents, reducing the Mn and Si contents, and adopting optimized smelting, forging, and heat treatment processes, the thermal conductivity, strength, and wear resistance of the mold steel are improved while maintaining toughness, forming a High performance mold steel.

Benefits of technology

It has improved the comprehensive performance of mold steel, expanded the scope of use and service life, has good thermal conductivity, strength, wear resistance and high temperature tempering stability, and is suitable for a variety of working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116200660B_ABST
    Figure CN116200660B_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance die steel and a manufacturing method thereof. The chemical composition of the high-performance die steel is as follows: C 0.45-0.54%, Si 0.02-0.15%, Mn 0.05-0.20%, Cr 2.2-3.0%, Mo 3.0-4.0%, V 0.32-0.55%, W 0.31-0.48%, Ni 0.34-0.55%, N≤0.015%, P≤0.020%, S≤0.003%, and the balance is Fe. The invention optimizes the production process according to the component design, so that the obtained die steel has good thermal conductivity and excellent strength, wear resistance and high-temperature tempering stability, high matrix purity, uniform structure, no large-particle primary carbide and good toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of die steel manufacturing, and in particular relates to a high-performance die steel and a manufacturing method thereof. Background Art

[0002] The mold is called the "mother of industry". The performance and quality of mold steel directly determine the service life of the mold and the production efficiency of the product. Mold steel is divided into plastic mold steel, cold work mold steel and hot work mold steel. Different types of mold steel have different performance requirements. For example, plastic mold steel requires higher thermal conductivity, polishability and hardness, cold work mold steel requires very high hardness and wear resistance, and hot work mold steel often requires high toughness and fatigue performance. In order to meet the needs of complex mold working conditions and reduce the problem of material selection for mold customers, mold steel with excellent comprehensive performance is very necessary. Taking H13 and H11 steel as examples, they have good comprehensive performance and can be used as hot work mold steel and plastic mold steel, but in some working conditions, the hardness, strength, wear resistance and other properties are low, which cannot meet the needs of mold use conditions and high production efficiency.

[0003] At present, the international community often adopts a low Si, high Mo and low V composition based on H13 steel. On this basis, the present invention increases the C content, reduces the Mn content, and increases the Ni and W contents. While improving the hardness and strength, the toughness and thermal conductivity of the mold steel are taken into consideration, so that the invented mold steel has more excellent comprehensive performance and improves the use range and service life of the mold steel. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a high-performance mold steel and a method for manufacturing the same, which solves the problems of insufficient strength, insufficient wear resistance and low thermal conductivity of traditional H13 steel, and improves the comprehensive performance and application range of the mold steel without significantly reducing toughness.

[0005] The purpose of the present invention is achieved by the following technical solutions:

[0006] A high-performance die steel, whose chemical composition is as follows by mass percentage:

[0007] C 0.45~0.54%, Si 0.02~0.15%, Mn 0.05~0.20%, Cr 2.2~3.0%, Mo 3.0~4.0%, V 0.32~0.55%, W 0.31~0.48%, Ni 0.34~0.55%, N≤0.015%, P≤0.020%, S≤0.003%, and the balance is Fe and inevitable impurity elements.

[0008] The manufacturing method of the high performance die steel as described above comprises the following steps:

[0009] S1. Smelting: First, iron, tungsten and nickel raw materials are added for smelting, oxygen is supplied or oxide scale is added to control Si≤0.12%, Mn≤0.16%; then a deoxidizer is added for deoxidation, and chromium, vanadium and molybdenum raw materials are added for further smelting. At the end of smelting, bottom blowing is performed, and then slag is removed, steel is tapped and a dephosphorizing agent is added to make P≤0.020%, and the tapping temperature is controlled to be 1600-1640°C;

[0010] S2. Refining outside the furnace: First, the molten steel after smelting in step S1 is further deoxidized by adding a deoxidizer in the LF furnace, desulfurized by making white slag, and refined for not less than 18min, controlling S≤0.005% in the steel, and the refining temperature ≥1600℃; then refined for not less than 15min in a VD furnace under vacuum ≤0.5tor, reducing the oxygen, hydrogen and nitrogen contents in the molten steel to 0.0025%, 0.0002% and 0.01% respectively, and then soft blowing and tapping, the tapping temperature is controlled to 1550~1590℃;

[0011] S3. Casting mother electrode: Use inert gas protection and pouring method to cast molten steel into mother electrode of the required specifications for electroslag remelting, the pouring temperature is not higher than 1570℃, the rising rate of molten steel during pouring is not higher than 10mm / s, after the pouring is completed, the mold is cooled for ≥2h, and then the stress relief annealing is carried out at 740~780℃ for more than 6h, and then it is taken out of the furnace;

[0012] S4. Electroslag remelting: The mother electrode is remelted and refined under atmosphere protection conditions. The CaO content in the selected refining slag is ≥10%, and the SiO2 content is ≤1%. The remelting voltage is 50-64V, the current is 8000-14000A, and the melting rate does not exceed 0.8DKg / h, where D is the diameter of the electroslag crystallizer. After the remelting is completed, the electroslag ingot is kept at 760-800℃ for more than 8h for annealing. After the insulation is completed, it is slowly cooled to ≤400℃ at ≤20℃ / h and then the heating is stopped;

[0013] S5. High temperature homogenization: The electroslag ingot after remelting annealing in step S4 is heated at a heating rate of ≤150°C / h, and then heated at 800-900°C for 2-4h and then heated to between 1250-1270°C for insulation, and the insulation time is not less than 8h;

[0014] S6. Forging: The electroslag ingot after high-temperature homogenization is blanked and forged into the required specifications by a punching method, and the heating temperature of each fire is not less than 1180°C and the total forging ratio is not less than 8 for multi-fire forging; the small-sized steel after forging is rapidly cooled by water cooling or mist cooling, and is placed in the air after cooling to a surface temperature of ≤400°C; the large-sized steel is directly processed by step S7 after forging; the small-sized steel is a steel with a thickness of ≤360mm or a diameter of ≤500mm, and the large-sized steel is a steel with a thickness of >360mm or a diameter of >500mm;

[0015] S7. High temperature refinement + annealing: heat to 1030-1045℃ and keep warm for more than 6h, then take out of the furnace and water cool. After cooling to the surface temperature within 400℃, annealing is carried out. The annealing temperature is 820-860℃ and the holding time is not less than 10h. After the holding is completed, slowly cool to ≤500℃ at ≤15℃ / h and stop heating.

[0016] Preferably, the smelting in step S1 is carried out in any one of the following three types of furnaces: an electric arc furnace, an induction furnace, or an induction furnace combined with an AOD furnace.

[0017] Preferably, the deoxidizer in step S1 is carbon powder, aluminum or aluminum calcium, and the dephosphorization agent is lime or pre-melted slag containing lime; and the deoxidizer in step S2 is aluminum wire, calcium wire or aluminum powder.

[0018] Preferably, the chromium, vanadium and molybdenum raw materials in step S1 are first preheated to 200-500°C before being added, and the smelting temperature after addition is greater than 1600°C, the bottom blowing gas is argon, the bottom blowing time is not less than 5 minutes, and the gas flow rate is not less than 500Nm 3 / h.

[0019] Preferably, the SiO2 content in the LF white slag in step S2 is ≤5%, the argon flow rate during VD soft blowing is not greater than 8 L / min, and the soft blowing time is ≥10 min.

[0020] Preferably, the upsetting reduction in step S6 is 30-50% of the height, and the temperature is kept at no less than 1250°C for more than 6 hours before upsetting; the single downsizing during drawing is ≥100mm, the last heating temperature is 1180-1220°C, and the final forging temperature is not less than 850°C.

[0021] Preferably, the water cooling method for the furnace in step S7 is: the single water entry time is between 0.5 and 5 minutes, and the water temperature is between 20 and 70°C.

[0022] Preferably, after the heating is stopped in step S7, the product is taken out of the furnace when the temperature is lower than 300°C.

[0023] Compared with the prior art, the advantages of the present invention are: the production process is optimized according to the composition design, so that the obtained mold steel has good thermal conductivity and excellent strength, wear resistance and high-temperature tempering stability, high matrix purity, uniform structure, no large particles of primary carbides and good toughness. It is a mold steel with excellent comprehensive performance and can be used in extrusion, hot forging, stamping and plastics and other working conditions that have high requirements on the comprehensive performance of mold steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is the annealing metallographic structure diagram of the high performance die steel of the present invention.

[0025] Figure 2 It is a comparison chart of the 600°C tempering stability of the high performance die steel of the present invention.

[0026] Figure 3 It is a comparison chart of the wear resistance of the high-performance die steel of the present invention.

[0027] Figure 4 It is a comparison chart of thermal conductivity of the high performance die steel of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail in conjunction with the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0029] The present invention provides a high-performance die steel, the chemical composition of which is as follows by mass percentage:

[0030] C 0.45~0.54%, Si 0.02~0.15%, Mn 0.05~0.20%, Cr 2.2~3.0%, Mo 3.0~4.0%, V 0.32~0.55%, W 0.31~0.48%, Ni 0.34~0.55%, N≤0.015%, P≤0.020%, S≤0.003%, and the balance is Fe and inevitable impurity elements.

[0031] The alloying elements and C element content in mold steel affect the microstructure and properties of mold steel. Mo, V, Cr, and W can combine with C elements to generate nano-scale secondary carbides, which improve the strength and wear resistance of mold steel, but may reduce the toughness of mold steel. In order to effectively play the beneficial role of alloying elements and inhibit their influence on toughness, the present invention reduces the Cr content in the alloy and increases Mo on the basis of H13 steel and Dievar steel. Adding W is beneficial to improving the anti-tempering stability and wear resistance, and at the same time makes up for the influence of the reduction of V content on strength and wear resistance; and reducing the content of Si and V elements can reduce element segregation and improve impact performance; increasing the Mo content and reducing the content of Si and Mn elements to improve the thermal conductivity of mold steel, and appropriately adding Ni content to reduce the influence of the reduction of Mn and Cr content on hardenability.

[0032] By optimizing the content of the above elements, high requirements are placed on the smelting, forging and heat treatment of die steel. Combined with equipment conditions and element content control, in order to obtain extremely low Si and Mn contents, strong oxygen supply is required during smelting (oxidants such as oxide scale are added when smelting in an induction furnace alone). In order to avoid the oxidation and burning of elements such as Cr, Mo, and V, which will increase costs, deoxidizers are first added before adding Cr, Mo, and V alloys in the later stage of smelting. This can not only avoid the oxidation and burning of the above alloys, but also absorb heat after the above alloys are added, resulting in excessive reduction in the temperature of the molten steel. The first addition of deoxidizers will also release heat, which will offset the heat absorbed after the addition of the alloy, thereby effectively controlling the smelting temperature. Then, bottom blowing is carried out at the end of smelting to even out the alloy composition and promote the floating of inclusions; dephosphorization agents are added during the steelmaking process to further reduce the P and S contents. The use of deoxidizers containing Si and Mn is prohibited in the LF process of refining outside the furnace, and the SiO2 content in the slag must meet certain content requirements to avoid Si increase; due to the high viscosity of the alloying elements and the high metal liquid, special requirements are placed on the VD bottom blowing (soft blowing is required) and vacuum refining process to meet the required gas content. When casting the mother electrode, due to the high content of Mo and C and a certain amount of V and W, coarse dendrites are easily formed, resulting in solidification defects such as segregation, so the pouring temperature and pouring rate are appropriately reduced. Electroslag remelting inhibits Si increase by controlling the SiO2 content in the slag, optimizes the slag system and the electrical system to promote the removal of inclusions and reduce solidification segregation. The purpose of high-temperature homogenization and forging is to evenly distribute elements such as Mo, W, and V in the alloy, eliminate large-particle carbides, and improve the toughness and isotropy of the mold. Different post-forging + high-temperature refinement + annealing treatment processes are formulated according to specifications, so that mold steels of different specifications in the present invention can obtain uniform and refined structures to meet the performance requirements.

[0033] In summary, combined with the control of impurity element content and inclusions by smelting process, optimization of forging process and improvement of matrix structure of mold steel by rapid cooling process, the high-performance mold steel produced has high purity, light element segregation, uniform structure and large-particle primary carbides. While improving the thermal conductivity, hardness and wear resistance of mold steel, the mold steel still has high toughness, which makes the comprehensive performance of mold steel excellent and can be used in a variety of working conditions.

[0034] The present invention also provides a method for manufacturing the high-performance die steel as described above, comprising the following steps:

[0035] S1. Smelting: First, iron (such as scrap steel), tungsten (such as ferrotungsten) and nickel (such as ferronickel or electrolytic nickel) raw materials are added according to the required ingredients, and smelting is carried out in any one of the following three types of furnaces: electric arc furnace, induction furnace, or induction furnace combined with AOD furnace, oxygen supply or addition of oxide scale to reduce Si and Mn content, control Si≤0.12%, Mn≤0.16%; then add deoxidizer for deoxidation, due to the strong oxygen supply or addition of oxide scale in the early stage, the oxygen content is high, the deoxidizer can be carbon powder, aluminum powder, aluminum particles or aluminum calcium, and chromium (such as ferrochrome), vanadium (such as ferrovanadium), molybdenum (such as ferromolybdenum) raw materials are added according to the composition for further smelting, bottom blowing is carried out at the end of smelting to promote the floating of inclusions in the molten steel, and then slag is removed, steel is tapped and a dephosphorization agent is added to make P≤0.020%, and the tapping temperature is controlled to be 1600-1640°C; the dephosphorization agent can be lime (CaO) or pre-melted slag containing lime, which has a good dephosphorization and desulfurization effect;

[0036] S2. Refining outside the furnace: First, the molten steel after smelting in step S1 is deoxidized by adding a deoxidizer through a LF furnace. Since the initial deoxidation in step S1 has been performed, the oxygen content is relatively low at this time. Therefore, aluminum wire, calcium wire or aluminum powder with better deoxidation effect is preferably used. At the same time, deoxidizers containing Si and Mn are prohibited to be used to avoid increasing the Si and Mn contents. White slag is desulfurized and refined for not less than 18 minutes to control S≤0.005% and temperature≥1600°C in the steel; then the slag is skimmed and refined in a VD furnace at a vacuum degree of ≤0.5tor for not less than 15 minutes to reduce the oxygen, hydrogen and nitrogen contents in the molten steel to 0.0025%, 0.0002% and 0.01% respectively, and then soft blowing is performed to tap steel, and the tapping temperature is controlled to be 1550-1590°C;

[0037] S3. Casting mother electrode: using inert gas protection, preferably argon, and pouring method to cast molten steel into mother electrodes of the specifications required for electroslag remelting, the pouring temperature is not higher than 1570°C, and the rising rate of molten steel during pouring is not higher than 10mm / s to reduce solidification defects such as segregation and looseness. After the casting is completed, the mold is cooled for ≥2h, and then the stress relief annealing is carried out at 740-780°C for more than 6h, and then the surface oxide scale is removed by grinding after being taken out of the furnace;

[0038] S4. Electroslag remelting: The mother electrode is remelted and refined in an atmosphere-protected electroslag furnace. The CaO content in the selected refined slag is ≥10%, and the SiO2 content is ≤1%. The remelting voltage is 50-64V, the current is 8000-14000A, and the melting rate does not exceed 0.8DKg / h (D is the diameter of the electroslag crystallizer). After the remelting is completed, the electroslag ingot is kept at 760-800℃ for more than 8h for annealing. After the insulation is completed, it is slowly cooled to ≤400℃ at ≤20℃ / h and then the heating is stopped;

[0039] S5. High temperature homogenization: The electroslag ingot after remelting annealing in step S4 is heated at a heating rate of ≤150°C / h, and then heated at 800-900°C for 2-4h and then heated to between 1250-1270°C for insulation, and the insulation time is not less than 8h;

[0040] S6. Forging: The electroslag ingot after high-temperature homogenization is forged by a forging press by a punching method to open the blank and forge it into the required specifications. If multiple forgings are adopted, the heating temperature of each fire is not less than 1180°C and the total forging ratio is not less than 8; the small-sized steel after forging is quickly cooled by water cooling or mist cooling, and is placed in the air after cooling to a surface temperature of ≤400°C; the large-sized steel is directly processed in step S7 after forging; the small-sized steel is the steel with a thickness of ≤360mm or a diameter of ≤500mm, and the large-sized steel is the steel with a thickness of >360mm or a diameter of >500mm. Generally, cooling after forging can prevent the generation of network carbides, promote more uniform organization and refine grains; however, after research, the large-sized material after forging in this application has uneven internal cooling, the core organization after forging is not easy to control, it is difficult to obtain an ideal organization, and there is a risk of water cooling cracking after forging, so omitting the rapid cooling step after forging and directly performing high-temperature refinement treatment will not produce other defects, which is relatively more conducive to obtaining a uniform organization; while the organization of small-sized steel after forging is easy to control, rapid cooling after forging is convenient for controlling the ideal organization, and small-sized steel after forging is not easy to crack, so this application processes large-sized steel and small-sized steel separately;

[0041] S7. High temperature refinement + annealing: Heat the furnace to 1030-1045℃ and keep it for more than 6 hours, then take it out of the furnace and water cool it until the surface temperature is within 400℃, then anneal it. The annealing temperature is 820-860℃, and the holding time is not less than 10 hours. After the holding is completed, slowly cool it to ≤500℃ at ≤15℃ / h, then stop heating, and take it out of the furnace when the temperature is lower than 300℃.

[0042] On the basis of optimizing the element content, the present invention optimizes the smelting process flow. During smelting, the bottom blowing process is used to promote the floating of inclusions, oxygen is supplied or scale is added to dephosphorize and reduce silicon, and the content of impurity elements such as O, N, and H in the steel is reduced through LF furnace and VD furnace refining. The steel of the present invention has a high content of alloy elements. After reasonable control of the electrical system, melting speed, and atmosphere protection of the slag, the electroslag remelting significantly improves the purity of the matrix, reduces the segregation of carbides in the steel, and thus improves the comprehensive performance of the material. Combined with high-temperature homogenization, upsetting forging, post-forging cooling, and high-temperature refinement + annealing processes, the manufactured mold steel has high purity, light element segregation, uniform structure, and no large-particle primary carbides. While improving the thermal conductivity, hardness, and wear resistance of the mold steel, the mold steel still has high toughness, so that the comprehensive performance of the mold steel is excellent.

[0043] The composition design and manufacturing method of the present invention are used to obtain a high-performance mold steel structure that meets the requirements of NADCA#AS1-AS5, the total number of inclusions is ≤2.5, the mold steel yield strength Rp0.2 is ≥1600MPa when the heat treatment hardness is ≥52HRC, the unnotched impact energy is ≥100J, the hardness is ≥38HRC after tempering at 600-650°C for 20h, the wear resistance is improved by more than 40% compared with H13 steel and Dievar steel, and the thermal conductivity is also significantly improved. The mold steel is suitable for working conditions with high requirements on strength, wear resistance, high temperature performance and certain requirements on toughness.

[0044] Preferably, in step S1, the chromium, vanadium and molybdenum raw materials are first preheated to 200-500°C before being added, and the smelting temperature after addition is greater than 1600°C. The bottom blowing gas is argon instead of nitrogen to control the nitrogen content. The bottom blowing time is not less than 5 minutes, and the gas flow rate is not less than 500Nm 3 / h.

[0045] Preferably, in step S2, the SiO2 content in the LF white slag is ≤5%, the argon flow rate during VD soft blowing is not greater than 8 L / min, and the soft blowing time is ≥10 min.

[0046] Preferably, the upsetting reduction in step S6 is 30-50% of the height, and the temperature is kept at no less than 1250°C for more than 6 hours before upsetting; the single downsizing during drawing is ≥100mm, the last heating temperature is 1180-1220°C, and the final forging temperature is not less than 850°C.

[0047] Preferably, the water cooling method for S7 is as follows: the single water entry time is between 0.5 and 5 minutes, and the water temperature is between 20 and 70°C.

[0048] Example 1

[0049] The high-performance mold steel provided in this embodiment includes, by mass percentage, C 0.46%, Si 0.04%, Mn 0.10%, Cr 2.8%, Mo 3.6%, V 0.38%, W 0.47%, Ni 0.43%, N 0.013%, P 0.011%, S0.001%, and the rest is Fe and unavoidable impurities.

[0050] The above die steel is manufactured using the following process:

[0051] (1) Smelting: Scrap steel, ferrotungsten, ferronickel and other raw materials are prepared according to the above-mentioned composition requirements, and smelted in an electric arc furnace. After about 5 minutes of initial smelting, molten initial slag is formed, and oxygen is blown to desiliconize and dephosphorize. The smelting temperature is 1630℃, Si is controlled to be 0.03%, Mn to be 0.08%, and then 1.25Kg / t carbon powder and 0.4Kg / t aluminum powder are added for deoxidation. After deoxidation for about 3 minutes, ferrochrome, ferrovanadium and ferromolybdenum preheated to 300℃ are added according to the composition requirements. At the end of smelting, argon is blown at the bottom for 7 minutes at a flow rate of 540Nm 3 / h, to even out the composition of the molten steel and promote the floating of inclusions in the molten steel, then slag, tap and add lime, the addition amount is 2kg / ton of molten steel, P is 0.010%, Si is 0.04%, and the tapping temperature is 1620℃;

[0052] (2) Refining outside the furnace: After smelting, the molten steel is deoxidized by adding 15 m / t of aluminum wire in the LF furnace, and desulfurized by making white slag. The SiO2 content in the slag is 2.8%. The refining time is 20 minutes, and the S content in the steel is controlled to be 0.004% and the temperature is 1610°C; after slagging, it is kept in a VD furnace under a vacuum degree of 0.3tor for 18 minutes. During the final soft blowing, the argon flow rate is 8 L / min and the soft blowing time is 11 minutes. The oxygen, hydrogen and nitrogen contents in the molten steel are 0.002%, 0.0001% and 0.009% respectively. After the vacuum is completed, the temperature of the molten steel is controlled to be 1580°C;

[0053] (3) Casting mother electrode: The molten steel is cast into a mother electrode with a specification of Φ360 mm through a long nozzle of protective atmosphere by a pouring method. The pouring temperature is 1550°C and the rising rate of the molten steel during pouring is 10 mm / s. After the pouring is completed, the mold is cooled for 2 hours and then loaded into an annealing furnace and kept at 740°C for 6 hours for stress relief annealing. The surface oxide scale is then removed from the furnace and polished;

[0054] (4) Electroslag remelting: The mother electrode is remelted and refined in a Φ500mm (crystallizer diameter) atmosphere-protected electroslag furnace. The pre-melted slag used contains 0.5% SiO2 and 20% CaO. The voltage is 50V, the current is about 9000A, and the melting rate is 350Kg / h. After the remelting is completed, the electroslag ingot is kept at 760°C for 8h, and then slowly cooled to 300°C at 15°C / h before stopping heating;

[0055] (5) High temperature homogenization: The electroslag ingot is charged into the furnace and heated at a rate of 150°C / h. After being kept at 850°C for 2h, the temperature is raised to 1260°C and kept at this temperature for 8h.

[0056] (6) Forging: The electroslag ingot after high temperature homogenization is forged into a 610×140mm (width×thickness) plate by a forging press through two upsetting and drawing processes. The upsetting ratio of the first fire is 50%, and the single drawing reduction is 140mm. The second fire is heated at 1250℃ and kept for 6h, and the upsetting ratio is 40%, and the single drawing reduction is 120mm. The third fire is heated at 1200℃ and the final forging temperature is 870℃, and the total forging ratio is 10. The forged steel is cooled to a surface temperature of 400℃ by water cooling and then placed in the air to wait for loading into the heat treatment furnace;

[0057] (7) High temperature refinement + annealing: After loading into the furnace, it is kept at 1045℃ for 6h, then taken out of the furnace and air-cooled for 30s and then immersed in water for cooling. The water temperature is 42℃. The first three water cooling times do not exceed 2min, and the subsequent water cooling time is between 2 and 4min. Gradually water-cooled to a surface temperature of 380℃, loaded into a resistance furnace for annealing. The annealing temperature is 860℃ and the holding time is 12h. After the holding is completed, it is slowly cooled to 500℃ at 10℃ / h and then the heating is stopped. When the temperature reaches 300℃, it is taken out of the furnace and air-cooled. The properties of the mold steel are measured according to the conventional method. The results are shown in Tables 1 and 2. Figures 1 to 4 shown.

[0058] Table 1

[0059]

[0060] Table 2

[0061]

[0062] from Figure 1 It can be seen that the die steel provided in this embodiment has a uniform annealed structure, dispersed and refined secondary carbides, and no large-sized eutectic carbides. According to the NADCA rating, the structure is AS2.

[0063] It has been determined that the sum of non-metallic inclusions in the mold steel is 2.0, the structure is AS2, the yield strength Rp0.2 of the mold steel is 1860MPa when the heat treatment hardness is 56HRC, the unnotched impact energy is 130J, and the thermal conductivity at 25℃ is 32W / (m·℃), which is higher than the 25W / (m·℃) of H13 steel and the 27W / (m·℃) of Dievar steel. After tempering at 600℃ for 20h, the hardness is 49HRC (37 for H13 steel and 40HRC for Dievar), the wear resistance is 50% higher than that of H13 steel, and the grain size is 8 to 8.5.

[0064] Example 2

[0065] The high-performance mold steel provided in this embodiment includes, by mass percentage, C 0.50%, Si 0.13%, Mn 0.14%, Cr 2.5%, Mo 3.1%, V 0.39%, W 0.47%, Ni 0.51%, N 0.012%, P 0.015%, S0.002%, and the rest is Fe and unavoidable impurities.

[0066] The above die steel is manufactured using the following process:

[0067] (1) Smelting: Low-Si scrap steel, ferrotungsten, ferronickel and other raw materials are prepared according to the above-mentioned composition requirements, and smelted in a medium frequency furnace. After about 40 minutes of melting, scale and lime are added. The smelting temperature is 1640°C, Si is 0.12%, Mn is 0.12%, and then 0.6 kg / t aluminum powder is added for deoxidation. After deoxidation for about 5 minutes, ferrochrome, ferrovanadium and ferromolybdenum preheated to 250°C are added according to the composition requirements. At the end of the smelting, argon is blown at the bottom for 10 minutes at a flow rate of 510 Nm 3 / h, uniform steel liquid composition, promote the floating of inclusions in the steel liquid, tap and add lime, the addition amount is 2kg / ton steel liquid, P is 0.014%, Si is 0.13%, and the tapping temperature is 1640℃;

[0068] (2) Refining outside the furnace: After smelting, the molten steel is deoxidized by adding 10 m / t of aluminum wire in the LF furnace, and white slag is made for desulfurization. The SiO2 content in the slag is 4.1%, and aluminum calcium powder is added. The refining temperature is 1620°C and the time is 22 minutes. The sulfur content in the steel is controlled to be 0.003%. After slagging, the molten steel is kept in a vacuum of 0.3tor for 20 minutes in a VD furnace. The argon flow rate during the final soft blowing is 8 L / min and the soft blowing time is 14 minutes. The oxygen, hydrogen and nitrogen contents in the molten steel are 0.002%, 0.0001% and 0.008% respectively. After the vacuum is ended, the temperature of the molten steel is controlled to be 1590°C;

[0069] (3) Casting mother electrode: The molten steel is cast into a mother electrode with a specification of Φ520 mm through a long nozzle of a protective atmosphere by a pouring method. The pouring temperature is 1570°C and the rising rate of the molten steel during pouring is 8 mm / s. After the pouring is completed, the mold is cooled for 4 hours and then loaded into an annealing furnace and kept at 740°C for 8 hours for stress relief annealing. The surface oxide scale is then removed from the furnace and polished;

[0070] (4) Electroslag remelting: The mother electrode is remelted and refined in a Φ750mm atmosphere-protected electroslag furnace. The pre-melted slag used contains 0.7% SiO2 and 10% CaO. The voltage is 56V, the current is about 13000A, and the melting rate is 560Kg / h. After the remelting is completed, the electroslag ingot is kept at 780°C for 10h, and then slowly cooled to 300°C at 12°C / h before stopping heating;

[0071] (5) High temperature homogenization: The electroslag ingot is charged into the furnace for heating at a rate of 120°C / h, and then kept at 850°C for 3h and then heated to 1250°C for 12h;

[0072] (6) Forging: The electroslag ingot after high temperature homogenization is forged into a 710×260mm (width×thickness) plate by a forging press through two upsetting and drawing processes. The upsetting ratio of the first fire is 50%, and the single drawing reduction is 140mm. The second fire is heated at 1250℃ and kept for 8h, and the upsetting ratio is 40%, and the single drawing reduction is 120mm. The last fire is heated at 1200℃ and the final forging temperature is 850℃, and the total forging ratio is 10. The forged steel is cooled to a surface temperature of 350℃ by water cooling and then placed in the air to wait for loading into the heat treatment furnace;

[0073] (7) High temperature refinement + annealing: After loading into the furnace, it is kept at 1030℃ for 10h, then taken out of the furnace and air-cooled for 30s before being immersed in water for cooling. The water temperature is 42℃. The first three water-cooling times do not exceed 3min, and the subsequent water-cooling time is between 3 and 4min. It is gradually water-cooled to a surface temperature of 360℃ and loaded into a resistance furnace for annealing. The annealing temperature is 820℃ and the holding time is 14h. After the holding is completed, it is slowly cooled to 500℃ at a rate of 10℃ / h and then the heating is stopped. When the temperature reaches 300℃, it is taken out of the furnace and air-cooled. The properties of the mold steel are measured according to the conventional method.

[0074] It has been determined that the sum of non-metallic inclusions in the mold steel is 2.5, the structure is AS4, the yield strength Rp0.2 of the mold steel is 1790MPa when the heat treatment hardness is 54HRC, the unnotched impact energy is 150J, and the thermal conductivity is 31W / (m·℃), which is higher than the 25W / (m·℃) of H13 steel and the 27W / (m·℃) of Dievar steel. After tempering at 620℃ for 20h, the hardness is 46HRC (34 for H13 steel and 36HRC for Dievar), the wear resistance is 40% higher than that of H13 steel, and the grain size is level 8.

[0075] Example 3

[0076] The high-performance mold steel provided in this embodiment includes, by mass percentage, C0.53%, Si 0.11%, Mn 0.14%, Cr 2.6%, Mo 3.7%, V 0.49%, W 0.47%, Ni 0.53%, N 0.013%, P 0.015%, S0.001%, and the rest is Fe and unavoidable impurities.

[0077] The above die steel is manufactured using the following process:

[0078] (1) Smelting: Scrap steel, ferrotungsten, ferronickel and other raw materials are prepared according to the above-mentioned composition requirements and smelted in an electric arc furnace. After about 6 minutes of smelting, molten initial slag is formed. Oxygen is blown to slag for desiliconization and dephosphorization. The smelting temperature is 1630°C, Si is 0.09%, Mn is 0.13%, and then 1.3 kg / t carbon powder and 0.4 kg / t aluminum powder are added for deoxidation. After deoxidation for about 4 minutes, ferrochrome, ferrovanadium and ferromolybdenum preheated to 300°C are added according to the composition requirements. At the end of the smelting, argon is blown for 8 minutes at a flow rate of 535 Nm 3 / h, uniform steel liquid composition, promote the floating of inclusions in the steel liquid, tap and add lime, the addition amount is 2kg / ton steel liquid, P is 0.014%, Si is 0.10%, and the tapping temperature is 1620℃;

[0079] (2) Refining outside the furnace: After smelting, the molten steel is deoxidized by adding 16 m / t of aluminum wire in the LF furnace, and desulfurized by making white slag. The SiO2 content in the slag is 3.9%. The refining time is 20 minutes, and the S content in the steel is controlled to be 0.003% and the temperature is 1610°C; after slagging, it is kept in a VD furnace under a vacuum degree of 0.2tor for 18 minutes. During the final soft blowing, the argon flow rate is 8 L / min and the soft blowing time is 11 minutes. The oxygen, hydrogen and nitrogen contents in the molten steel are 0.002%, 0.0001% and 0.008% respectively. After the vacuum is completed, the temperature of the molten steel is controlled to be 1570°C;

[0080] (3) Casting mother electrode: The molten steel is cast into a mother electrode with a specification of Φ520 mm through a long nozzle in a protective atmosphere by a pouring method. The pouring temperature is 1560°C and the rising rate of the molten steel during pouring is 8 mm / s. After the pouring is completed, the mold is cooled for 4 hours and then loaded into an annealing furnace and kept at 740°C for 8 hours for stress relief annealing. The surface oxide scale is then removed from the furnace and polished;

[0081] (4) Electroslag remelting: The mother electrode is remelted and refined in a Φ750mm atmosphere-protected electroslag furnace. The pre-melted slag used contains 0.6% SiO2 and 20% CaO. The voltage is 60V, the current is about 12000A, and the melting rate is 550Kg / h. After the remelting is completed, the electroslag ingot is kept at 780°C for 10h, and then slowly cooled to 300°C at 12°C / h before stopping heating;

[0082] (5) High temperature homogenization: The electroslag ingot is charged into the furnace and heated at a rate of 120°C / h. After being kept at 850°C for 2h, the temperature is raised to 1260°C and kept at this temperature for 10h.

[0083] (6) Forging: The electroslag ingot after high temperature homogenization is forged into a Φ280mm bar by a forging press through a first upsetting process. The upsetting ratio of the first fire is 50%, and the single drawing reduction is 140mm. The second fire is heated at 1250℃ and kept for 6h, and then gradually stretched to a single reduction of 100mm. The last fire is heated at 1210℃ and the final forging temperature is 860℃, with a total forging ratio of 14. The forged steel is cooled to a surface temperature of 400℃ by water cooling and then placed in the air to wait for loading into the heat treatment furnace;

[0084] (7) High temperature refinement + annealing: After loading into the furnace, it is kept at 1030℃ for 6h, then taken out of the furnace and air-cooled and immersed in water for cooling. The water temperature is 28℃. The first three water cooling times do not exceed 3min, and the subsequent water cooling time is between 3 and 5min. Gradually water-cooled to a surface temperature of 400℃, loaded into a resistance furnace for annealing. The annealing temperature is 820℃ and the holding time is 12h. After the holding is completed, it is slowly cooled to 500℃ at a rate of 10℃ / h and then the heating is stopped. When the temperature reaches 300℃, it is taken out of the furnace and air-cooled. The properties of the mold steel are measured according to the conventional method.

[0085] It was determined that the sum of non-metallic inclusions in the die steel was 1.5, the organization was AS2, the die steel yield strength Rp0.2 was 1960MPa when the heat treatment hardness was 58HRC, the unnotched impact energy was 120J, the thermal conductivity was 30W / (m·℃), which was higher than 25W / (m·℃) of H13 steel and 27W / (m·℃) of Dievar steel, and the hardness was 39HRC after tempering at 650℃ for 20h (27 for H13 steel and 29HRC for Dievar), and the wear resistance was improved by 70% compared with H13 steel. In addition, the grain size was determined to be 9.0 and the grain size was 9.

[0086] Example 4

[0087] The high-performance die steel provided in this embodiment has the same mass percentage as that in Embodiment 3, adopts the same smelting and refining process outside the furnace, and then adopts the following process to manufacture:

[0088] (3) Casting mother electrode: The molten steel is cast into a mother electrode with a specification of Φ640 mm through a long nozzle in a protective atmosphere by a pouring method. The pouring temperature is 1570°C and the rising rate of the molten steel during pouring is 6 mm / s. After the pouring is completed, the mold is cooled for 5 hours and then loaded into an annealing furnace and kept at 740°C for 10 hours for stress relief annealing. The surface oxide scale is then removed from the furnace and polished;

[0089] (4) Electroslag remelting: The mother electrode is remelted and refined in a Φ900mm atmosphere-protected electroslag furnace. The pre-melted slag used contains 0.5% SiO2 and 18% CaO. The voltage is 64V, the current is about 14000A, and the melting rate is 710Kg / h. After the remelting is completed, the electroslag ingot is kept at 780°C for 14h, and then slowly cooled to 300°C at 12°C / h before stopping heating;

[0090] (5) High temperature homogenization: The electroslag ingot is charged into the furnace and heated at a rate of 120°C / h. After being kept at 850°C for 2h, the temperature is raised to 1270°C and kept at this temperature for 14h.

[0091] (6) Forging: The electroslag ingot after high temperature homogenization is forged into a Φ600mm bar by a forging press through two upsetting and drawing processes. The upsetting ratio of the first fire is 45%, and the single drawing reduction is 120mm. The second fire is heated at 1260℃ and kept for 8h, and the upsetting ratio is 40%, and the single drawing reduction is 100mm. The last fire is heated at 1220℃ and the final forging temperature is 880℃, and the total forging ratio is 9. The forged bar is directly loaded into the heat treatment furnace for heating;

[0092] (7) High temperature refinement + annealing: After loading into the furnace, it is kept at 1045℃ for 8h, then taken out of the furnace and air-cooled and immersed in water for cooling. The water temperature is 26℃. The first three water cooling times do not exceed 4min, and the subsequent water cooling time is 5min. It is gradually cooled to a surface temperature of 300℃ and loaded into a resistance furnace for annealing. The annealing temperature is 820℃ and the holding time is 16h. After the holding is completed, it is slowly cooled to 500℃ at a rate of 10℃ / h and then the heating is stopped. When the temperature reaches 300℃, it is taken out of the furnace and air-cooled. The properties of the mold steel are measured according to the conventional method.

[0093] It has been determined that the sum of non-metallic inclusions in the mold steel is 2.0, the structure is AS4~5, the yield strength Rp0.2 of the mold steel is 1760MPa when the heat treatment hardness is 54HRC, the unnotched impact energy is 100J, and the thermal conductivity is 30W / (m·℃), which is higher than the 25W / (m·℃) of H13 steel and the 27W / (m·℃) of Dievar steel. After tempering at 650℃ for 20h, the hardness is 39HRC (H13 steel is 27HRC, Dievar is 29HRC), the wear resistance is 70% higher than that of H13 steel, and the grain size is 7.5~8.

[0094] Comparative Example 1

[0095] This embodiment provides a high-performance mold steel, the mass percentage of which is the same as that of Example 3. Except for the electroslag remelting process, the remaining processes adopt the same production process as that of Example 3. The electroslag remelting process is as follows:

[0096] (4) Electroslag remelting: The mother electrode is remelted and refined in a Φ750mm atmosphere-protected electroslag furnace. The pre-melted slag used is 37 slag (CaF2 is 70%, Al2O3 is 30%), the voltage is 58V, the current is 18000A, and the melting rate is 610Kg / h. After the remelting is completed, the electroslag ingot is kept at 780℃ for 10h, and then slowly cooled to 300℃ at 12℃ / h before stopping heating.

[0097] Compared with Example 3, this comparative example adopts a different pre-melted slag, and the current is larger and the melting rate is higher.

[0098] It was determined that the sum of non-metallic inclusions in the die steel was 2.5, the structure was AS4, the die steel yield strength Rp0.2 was 1950MPa when the heat treatment hardness was 58HRC, and the unnotched impact energy was 104J, which was lower than that in Example 3. The thermal conductivity was 30W / (m·℃), the hardness was 38HRC after tempering at 650℃ for 20h, and the wear resistance was slightly lower than that in Example 3. The grain size was 8.5.

[0099] Comparative Example 2

[0100] The high-performance die steel provided in this embodiment has the same mass percentage as that in Example 3, and adopts the same smelting, refining outside the furnace, casting mother electrode process, electroslag remelting, high-temperature homogenization and high-temperature refinement + annealing process as that in Comparative Example 1, but is different from Comparative Example 1 in the forging forming process:

[0101] (6) Forging: The electroslag ingot after high temperature homogenization is forged into a Φ260 mm bar by a forging press, with a single drawing reduction of 140 mm, a final heating temperature of 1210°C, a final forging temperature of 860°C, and a total forging ratio of 8. The forged steel is then placed in air to cool to 400°C before being loaded into a heat treatment furnace;

[0102] Compared with Comparative Example 1, this comparative example adopts a unidirectional drawing process during forging, and air cooling is adopted after forging.

[0103] It was determined that the sum of non-metallic inclusions in the die steel was 2.5, the structure was AS5, the die steel yield strength Rp0.2 was 1940MPa when the heat treatment hardness was 58HRC, and the unnotched impact energy was 95J, which was significantly lower than that of Example 3. The grain size was 8.0-8.5, and the other properties were similar to those of Comparative Example 1.

[0104] Comparative Example 3

[0105] This comparative example provides a high-performance die steel, the mass percentage of which is the same as that of Example 3, and is manufactured by the same smelting, refining outside the furnace, casting mother electrode, electroslag remelting, and high-temperature homogenization process as that of Comparative Example 1, and then by the following process:

[0106] (6) Forging: The electroslag ingot after high temperature homogenization is forged into a Φ260 mm bar by a forging press, with a single drawing reduction of 140 mm, a final heating temperature of 1210°C, a final forging temperature of 860°C, and a total forging ratio of 8. The forged steel is cooled by mist cooling or air cooling to a surface temperature of 400°C and then placed in the air to wait for loading into the heat treatment furnace;

[0107] (7) Annealing: The steel is placed in a resistance furnace for annealing at a temperature of 820°C and a holding time of 12 h. After the holding time, the steel is slowly cooled at a rate of 10°C / h to 500°C and then the heating is stopped. When the temperature reaches 300°C, the steel is taken out of the furnace and air-cooled. The properties of the mold steel are measured by conventional methods.

[0108] This comparative example is the manufacturing process currently adopted by some small die steel companies. Compared with comparative example 1, the forging adopts a unidirectional drawing process and does not use high-temperature refinement.

[0109] It was determined that the sum of non-metallic inclusions in the die steel was 2.5, the structure was AS6, the die steel yield strength Rp0.2 was 1920MPa when the heat treatment hardness was 58HRC, and the unnotched impact energy was 78J, which was significantly lower than that of Example 3. The grain size was 7.0-7.5, and the other properties were similar to those of Comparative Example 1.

[0110] Comparative Example 4

[0111] The high-performance die steel provided in this embodiment has the same mass percentage as that in Example 3, adopts the same smelting, refining outside the furnace, casting mother electrode, high-temperature homogenization and high-temperature refinement + annealing process as that in Comparative Example 1, and does not go through the electroslag remelting process. The forging forming process is as follows:

[0112] (6) Forging: The high-temperature homogenized die-cast ingot is forged into a Φ280mm bar by a forging press through two upsetting and drawing processes. The upsetting ratio of the first fire is 50%, and the single-time drawing reduction is 120mm. The second fire is heated to 1250℃ and kept for 6 hours, then upset by more than 30%, and gradually drawn, with a single-time reduction of 90mm. The last fire is heated to 1200℃, the final forging temperature is 860℃, and the total forging ratio is 12. The forged steel is cooled to a surface temperature of 400℃ by water and then placed in the air to wait for loading into the heat treatment furnace.

[0113] Compared with Comparative Example 1, this comparative example does not adopt the electroslag remelting process.

[0114] It was determined that the sum of non-metallic inclusions in the die steel was 3.0, the structure was AS5, the die steel yield strength Rp0.2 was 1920 MPa when the heat treatment hardness was 58 HRC, and the unnotched impact energy was 82 J, which was significantly lower than that of Example 3. The grain size was 8.0.

[0115] Comparative Example 5

[0116] The high-performance die steel provided in this embodiment has the same mass percentage as that in Example 4, and is manufactured by using the same smelting, refining process outside the furnace, casting mother electrode, electroslag remelting, and high-temperature homogenization process as in Example 4, and then using the following process:

[0117] (6) Forging: The electroslag ingot after high temperature homogenization is forged into a Φ600mm bar by a forging press through two upsetting and drawing processes. The upsetting ratio of the first fire is 45%, and the single drawing reduction is 120mm. The second fire is heated at 1260℃ and kept for 8h, and the upsetting ratio is 40%, and the single drawing reduction is 100mm. The last fire is heated at 1190℃ and the final forging temperature is 850℃, and the total forging ratio is 9. The forged bar is water-cooled, mist-cooled or air-cooled until the surface temperature of the bar is below 400℃;

[0118] (7) High temperature refinement + annealing: After loading into the furnace, it is kept at 1030℃ for 15h, then taken out of the furnace and air-cooled and immersed in water for cooling. The water temperature is 26℃. The first three water cooling times do not exceed 4min, and the subsequent water cooling time is 5min. It is gradually cooled to a surface temperature of 300℃ and loaded into a resistance furnace for annealing. The annealing temperature is 820℃ and the holding time is 16h. After the holding is completed, it is slowly cooled to 500℃ at a rate of 10℃ / h and then the heating is stopped. When the temperature reaches 300℃, it is taken out of the furnace and air-cooled. The properties of the mold steel are measured according to the conventional method.

[0119] Compared with Example 4, this comparative example is cooled after forging and before high-temperature refinement annealing, and the corresponding high-temperature refinement temperature is also reduced accordingly.

[0120] It was determined that the sum of non-metallic inclusions in the die steel was 2.0, the structure was AS6-7 or AS9, the yield strength Rp0.2 of the die steel was 1720 MPa when the heat treatment hardness was 54 HRC, and the unnotched impact energy was 83 J. The other properties were similar to those of Example 4.

[0121] By comparing Example 3 with Comparative Examples 1 to 4, it is found that the present invention, through reasonable electroslag remelting electrical system, melting rate and slag atmosphere protection electroslag remelting, as well as high-temperature homogenization, upsetting forging and post-forging cooling and high-temperature refinement + annealing process, makes the manufactured mold steel have high purity, uniform structure, no large particles of primary carbide, and refined grains. Combined with reasonable component optimization, while improving the thermal conductivity, hardness and wear resistance of the mold steel, the mold steel still has high toughness, so that the comprehensive performance of the mold steel is excellent.

[0122] Moreover, according to the difference in specifications, the relationship between forging and high-temperature refinement is reasonably connected (Example 4 and Comparative Example 5), ensuring that the large-size die steel still has a uniform structure and excellent performance.

[0123] Although preferred embodiments of the present invention have been described, additional changes and modifications may be made to these embodiments by those skilled in the art once the basic inventive concepts are known. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for manufacturing high-performance die steel, characterized in that: The chemical composition of the high performance die steel is as follows: C 0.45~0.54%、Si 0.02~0.15%、Mn 0.05~0.20%、Cr 2.2~3.0%、Mo 3.0~4.0%、V 0.32~0.55%、W 0.31~0.48%、Ni 0.34~0.55%、N≤0.015%、P≤0.020%、S≤0.003%、the balance is Fe and unavoidable impurity elements; The manufacturing method comprises the following steps: S1. Smelting: First, iron, tungsten and nickel raw materials are added for smelting, oxygen is supplied or oxide scale is added to control Si≤0.12%, Mn≤0.16%; then a deoxidizer is added for deoxidation, and chromium, vanadium and molybdenum raw materials are added for further smelting. At the end of smelting, bottom blowing is performed, and then slag is removed, steel is tapped and a dephosphorizing agent is added to make P≤0.020%, and the tapping temperature is controlled to be 1600-1640°C; S2. Refining outside the furnace: First, the molten steel after smelting in step S1 is further deoxidized by adding a deoxidizer in the LF furnace, desulfurized by making white slag, and refined for not less than 18min, controlling S≤0.005% in the steel, and the refining temperature ≥1600℃; then refined for not less than 15min in a VD furnace under vacuum ≤0.5tor, reducing the oxygen, hydrogen and nitrogen contents in the molten steel to 0.0025%, 0.0002% and 0.01% respectively, and then soft blowing and tapping, the tapping temperature is controlled to 1550~1590℃; S3. Casting mother electrode: Use inert gas protection and pouring method to cast molten steel into mother electrode of the required specifications for electroslag remelting, the pouring temperature is not higher than 1570℃, the rising rate of molten steel during pouring is not higher than 10mm / s, after the pouring is completed, the mold is cooled for ≥2h, and then the stress relief annealing is carried out at 740~780℃ for more than 6h, and then it is taken out of the furnace; S4. Electroslag remelting: The mother electrode is remelted and refined under atmosphere protection conditions, the CaO content in the selected refining slag is ≥10%, the SiO2 content is ≤1%, the remelting voltage is 50-64V, the current is 8000-14000A, and the melting rate does not exceed 0.8DKg / h, where D is the diameter of the electroslag crystallizer, in mm; after the remelting is completed, the electroslag ingot is kept at 760-800℃ for more than 8h for annealing, and after the insulation is completed, it is slowly cooled to ≤400℃ at ≤20℃ / h and then the heating is stopped; S5. High temperature homogenization: The electroslag ingot after remelting annealing in step S4 is heated at a heating rate of ≤150°C / h, and then heated at 800-900°C for 2-4h and then heated to between 1250-1270°C for insulation, and the insulation time is not less than 8h; S6. Forging: The electroslag ingot after high-temperature homogenization is blanked and forged into the required specifications by the upsetting and drawing process, and the heating temperature of each fire is not less than 1180°C and the total forging ratio is not less than 8 for multi-fire forging; the small-sized steel after forging is rapidly cooled by water cooling or mist cooling, and is placed in the air after cooling to a surface temperature of ≤400°C; the large-sized steel is directly processed by step S7 after forging; the small-sized steel is a steel with a thickness of ≤360mm or a diameter of ≤500mm, and the large-sized steel is a steel with a thickness of >360mm or a diameter of >500mm; S7. High temperature refinement + annealing: heat to 1030-1045℃ and keep warm for more than 6h, then take out of the furnace and water cool. After cooling to the surface temperature within 400℃, annealing is carried out. The annealing temperature is 820-860℃ and the holding time is not less than 10h. After the holding is completed, slowly cool to ≤500℃ at ≤15℃ / h and stop heating.

2. The method for manufacturing high performance die steel according to claim 1, characterized in that: The smelting in step S1 is carried out in any one of the following three types of furnaces: an electric arc furnace, an induction furnace, or an induction furnace combined with an AOD furnace.

3. The method for manufacturing high performance die steel according to claim 1, characterized in that: In step S1, the deoxidizer is carbon powder, aluminum or aluminum calcium, and the dephosphorization agent is lime or pre-melted slag containing lime; in step S2, the deoxidizer is aluminum wire, calcium wire or aluminum powder.

4. The method for manufacturing high performance die steel according to claim 1, characterized in that: Step S1: The chromium, vanadium and molybdenum raw materials are first preheated to 200-500°C before being added, and the melting temperature after addition is greater than 1600°C. The bottom blowing gas is argon gas, the bottom blowing time is not less than 5 minutes, and the gas flow rate is not less than 500Nm 3 / h.

5. The method for manufacturing high performance die steel according to claim 1, characterized in that: In step S2, the SiO2 content in the LF white slag is ≤5%, the argon flow rate during VD soft blowing is not greater than 8L / min, and the soft blowing time is ≥10min.

6. The method for manufacturing high performance die steel according to claim 1, characterized in that: In step S6, the upsetting reduction amount of the upsetting method is 30-50% of the height, and the temperature is kept at not less than 1250°C for more than 6 hours before upsetting; the single downsetting amount during the drawing is ≥100mm, the last heating temperature is 1180-1220°C, and the final forging temperature is not less than 850°C.

7. The method for manufacturing high performance die steel according to claim 1, characterized in that: The water cooling method for the furnace in step S7 is: the single water entry time is between 0.5 and 5 minutes, and the water temperature is between 20 and 70°C.

8. The method for manufacturing high performance die steel according to claim 1, characterized in that: Step S7: After the heating is stopped, the product is taken out of the furnace when the temperature is lower than 300°C.