Polyetheretherketone, composition and sheet
By introducing inorganic compounds into polyether ether ketone (PEEK) and optimizing the synthesis conditions, the problem of PEEK mechanical strength improvement space is solved, and the mechanical strength is significantly improved in high-performance applications.
Patent Information
- Application Number
- CN202180060621.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-02
- Filing Date
- 2021-09-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-09-02
AI Technical Summary
There is room for improvement in the existing polyether ether ketone (PEEK) in terms of mechanical strength, especially in terms of increasing tensile strength, which is difficult to meet the needs of certain high-performance applications.
Ensure the hydroxyl group in PEEK by introducing specific inorganic compounds such as glass fibers and carbon fibers in PEEK and controlling their synthesis conditions, such as the reaction ratio and reaction time of 4,4'-dichlorobenzophenone and hydroquinone, The presence and fluorine and chlorine content are within a suitable range, thereby increasing its mechanical strength.
The mechanical strength of PEEK has been significantly improved, especially in terms of tensile strength, forming formed bodies suitable for high-performance materials, such as aerospace and gear applications.
Smart Images

Figure CN116209708B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to polyetheretherketone, composition and sheet.
[0002] Specifically, the present invention relates to polyetheretherketone, a composition, and a sheet that can exhibit excellent mechanical strength by adding an inorganic compound. Background Art
[0003] As a representative resin of engineering plastics, polyetheretherketone (hereinafter, polyetheretherketone may be referred to as "PEEK") is known.
[0004] Generally, when PEEK is produced, 4,4'-difluorobenzophenone and hydroquinone, which are considered to have high reactivity, are used as raw materials.
[0005] On the other hand, in Patent Document 1, when producing PEEK, a mixed solvent of 100 parts by mass of an aromatic sulfone and 1 to 20 parts by mass of a solvent having a boiling point of 270 to 330° C. is used as an essential condition, and 4,4′-dichlorobenzophenone and hydroquinone are used as raw materials.
[0006] In addition, in Patent Document 2, when producing PEEK, 4,4'-dichlorobenzophenone and hydroquinone are used as raw materials in the presence of one or more alkali metal fluorides selected from sodium fluoride, potassium fluoride, rubidium fluoride and cesium fluoride as an essential condition.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 3-122120
[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 64-65129 Summary of the invention
[0011] However, in the conventional PEEK represented by Patent Documents 1 and 2, room for further improvement has been found from the viewpoint of improving mechanical strength.
[0012] One of the objects of the present invention is to provide a polyetheretherketone, a composition and a sheet which can exhibit excellent mechanical strength by adding an inorganic compound.
[0013] The present inventors have conducted intensive studies and have found that excellent mechanical strength can be exhibited by blending an inorganic compound into a specific PEEK, thereby completing the present invention.
[0014] According to the present invention, the following polyetheretherketone and the like can be provided.
[0015] 1. A polyetheretherketone comprising a repeating unit represented by the following formula (1), wherein the polyetheretherketone satisfies one or both of the following conditions (A) and (B) and has a hydroxyl group at one or both ends of the main chain.
[0016] [Chemical formula 1]
[0017]
[0018] (A) The fluorine atom content a is less than 2 mg / kg.
[0019] (B) The chlorine atom content b is 2 mg / kg or more.
[0020] 2. The polyetheretherketone according to item 1, wherein the raw materials thereof include 4,4'-dichlorobenzophenone.
[0021] 3. The polyetheretherketone according to 1 or 2, wherein 1 The area ratio of the peak at the α-position of the hydroxyl group in H-NMR measurement to the main chain peak is 0.10 to 2.00%.
[0022] 4. The polyetheretherketone according to any one of 1 to 3, wherein the reduced viscosity η sp / c is 0.40~1.00dl / g.
[0023] 5. A composition comprising polyetheretherketone and an inorganic compound, wherein the polyetheretherketone comprises a repeating unit represented by the following formula (1) and satisfies one or both of the following conditions (A) and (B).
[0024] [Chemical formula 2]
[0025]
[0026] (A) The fluorine atom content a is less than 2 mg / kg.
[0027] (B) The chlorine atom content b is 2 mg / kg or more.
[0028] 6. The composition according to 5, wherein the polyetheretherketone has a hydroxyl group at one or both ends of the main chain.
[0029] 7. The composition according to 5 or 6, wherein the polyetheretherketone 1 The area ratio of the peak at the α-position of the hydroxyl group in H-NMR measurement to the main chain peak is 0.10 to 2.00%.
[0030] 8. The composition according to any one of 5 to 7, wherein the reduced viscosity η of the polyetheretherketone is sp / c is 0.40~1.00dl / g.
[0031] 9. The composition according to any one of 5 to 8, wherein the inorganic compound is one or more selected from glass fiber, carbon fiber and boron nitride.
[0032] 10. The composition according to any one of 5 to 9, wherein the inorganic compound is one or more selected from glass fiber and carbon fiber, and the inorganic compound is in the form of one or more selected from chopped strands, rovings, fabrics, nonwoven fabrics and unidirectional materials.
[0033] 11. The composition according to any one of 5 to 10, wherein the inorganic compound is glass fiber.
[0034] 12. A sheet comprising:
[0035] A cloth comprising an inorganic compound; and
[0036] The polyetheretherketone according to any one of 1 to 4 impregnated in the above-mentioned cloth.
[0037] 13. The sheet according to 12, wherein the cloth is a unidirectional material.
[0038] 14. The sheet according to 12 or 13, wherein the cloth contains one or more selected from glass fiber and carbon fiber.
[0039] According to the present invention, it is possible to provide a polyetheretherketone, a composition, and a sheet capable of exhibiting excellent mechanical strength by adding an inorganic compound. DETAILED DESCRIPTION
[0040] Hereinafter, the polyetheretherketone, composition and sheet of the present invention will be described in detail.
[0041] In addition, in this specification, "x to y" represents a numerical range of "x or more and y or less." The upper limit value and the lower limit value described in the numerical range can be arbitrarily combined.
[0042] In addition, in each of the embodiments of the mode according to the present invention described below, two or more embodiments that do not contradict each other may be combined with each other, and an embodiment obtained by combining two or more embodiments is also an embodiment of the mode according to the present invention.
[0043] 1. Polyetheretherketone
[0044] PEEK according to one embodiment of the present invention includes a repeating unit represented by the following formula (1), satisfies one or both of the following conditions (A) and (B), and has a hydroxyl group at one or both ends of the main chain.
[0045] [Chemical formula 3]
[0046]
[0047] (A) The fluorine atom content a is less than 2 mg / kg.
[0048] (B) The chlorine atom content b is 2 mg / kg or more.
[0049] The PEEK of this embodiment can exhibit excellent mechanical strength by blending an inorganic compound.
[0050] The reason why such an effect is exerted is not necessarily clear, but it is presumed that the hydroxyl groups in PEEK put the interface between PEEK and the inorganic compound in a state suitable for exerting excellent mechanical strength.
[0051] The mechanical strength mentioned here may be, for example, tensile strength.
[0052] In one embodiment, the PEEK of the present invention 1 The area ratio of the peak at the α position of the hydroxyl group to the main chain peak in H-NMR measurement (hereinafter, sometimes simply referred to as "area ratio X") is 0.10 to 2.00%.
[0053] It should be noted that the area ratio X is recorded in the examples. 1 The value obtained by H-NMR measurement. When obtaining the area ratio X, the area of the main chain peak is obtained by connecting the intensity of the chemical shift 7.32ppm and the intensity of 7.36ppm with a straight line (baseline) and integrating the range surrounded by the baseline and the peak. In addition, the area of the peak at the α position of the hydroxyl group is obtained by connecting the intensity of the chemical shift 6.98ppm and the intensity of 7.03ppm with a straight line (baseline) and integrating the range surrounded by the baseline and the peak.
[0054] In one embodiment, the PEEK of the present embodiment is formed of one type of PEEK having the same area ratio X.
[0055] In one embodiment, the PEEK of this embodiment is a mixture of two or more PEEKs having different area ratios X. In this case, 1 In H-NMR measurement, the area ratio X is 0.10 to 2.00%. Here, the two or more types of PEEK may include PEEK whose area ratio X is 0%, or may not include PEEK whose area ratio X is 0%.
[0056] In one embodiment, the area ratio X is 0.10% or more, 0.12% or more, or 0.14% or more, and is 2.0% or less, 1.8% or less, or 1.6% or less. In addition, the area ratio X may be, for example, 0.10 to 2.0%, 0.12 to 1.8%, or 0.14 to 1.6%. Thus, the effect of the present invention is well exerted.
[0057] In one embodiment, when PEEK is synthesized using 4,4'-dichlorobenzophenone and hydroquinone, the area ratio X can be adjusted to 0.10 to 2.00% by adjusting the molar ratio of 4,4'-dichlorobenzophenone to hydroquinone to be close to 1.00.
[0058] In one embodiment, when PEEK is synthesized using 4,4'-dichlorobenzophenone and hydroquinone, the reaction time is adjusted so that the reaction stops before the Cl terminal of 4,4'-dichlorobenzophenone and the OH terminal of hydroquinone react completely, thereby making the area ratio X 0.10 to 2.00%.
[0059] The fluorine atom content a and the chlorine atom content b of PEEK are values measured by combustion ion chromatography described in Examples.
[0060] In one embodiment, the fluorine atom content a of PEEK is less than 2 mg / kg. Thus, the effect of the present invention is well exerted. The lower limit is not particularly limited, and may be 0 mg / kg, for example.
[0061] Here, the fluorine atom content a is the sum of the fluorine atom content a1 contained in the molecular structure of PEEK and the fluorine atom content a2 contained as a component not contained in the molecular structure of PEEK (free component).
[0062] In one embodiment, the fluorine atom content a of PEEK can be made less than 2 mg / kg by not using a raw material containing fluorine atoms (such as 4,4'-difluorobenzophenone) or reducing the amount of raw materials containing fluorine atoms used in PEEK synthesis.
[0063] In one embodiment, the free component in the fluorine atom content a2 is one or both of potassium fluoride and 4,4'-difluorobenzophenone.
[0064] In one embodiment, the content b of chlorine atoms in PEEK is 2 mg / kg or more, 10 mg / kg or more, 100 mg / kg or more, 500 mg / kg or more, 700 mg / kg or more, 1000 mg / kg or more, 2000 mg / kg or more, 33000 mg / kg or more, or 4000 mg / kg or more. Thus, the effect of the present invention is well exerted. The upper limit is not particularly limited, for example, it can be less than 10000 mg / kg, less than 9000 mg / kg, less than 8000 mg / kg, less than 7000 mg / kg, or less than 6000 mg / kg.
[0065] In addition, the content b of chlorine atoms in PEEK is, for example, 2 to 10,000 mg / kg, preferably 700 to 9,000 mg / kg, and more preferably 1,000 to 8,000 mg / kg.
[0066] Here, the content b of chlorine atoms is the sum of the content b1 of chlorine atoms contained in the molecular structure of PEEK and the content b2 of chlorine atoms contained in components (free components) not contained in the molecular structure of PEEK.
[0067] In one embodiment, by including 4,4'-dichlorobenzophenone in the raw materials during the synthesis of PEEK, the content b of chlorine atoms in PEEK can be 2 mg / kg or more. In addition, as the raw materials for PEEK synthesis, 4,4'-dichlorobenzophenone and hydroquinone are used, and by increasing the ratio of the amount of 4,4'-dichlorobenzophenone used to the amount of hydroquinone used, the content b of chlorine atoms in PEEK can be increased within the range of 2 mg / kg or more.
[0068] In one embodiment, the content b1 of chlorine atoms is 0 mg / kg or more, 100 mg / kg or more, 200 mg / kg or more, or 400 mg / kg or more. The upper limit is not particularly limited and can be, for example, 10,000 mg / kg or less, 9,000 mg / kg or less, 8,000 mg / kg or less, or 7,000 mg / kg or less.
[0069] In one embodiment, the content b2 of chlorine atoms is 0 mg / kg or more, 2 mg / kg or more, 5 mg / kg or more, or 10 mg / kg or more. The upper limit is not particularly limited and can be, for example, 500 mg / kg or less, 400 mg / kg or less, or 300 mg / kg or less.
[0070] In one embodiment, the above free component in the above content b2 of chlorine atoms is one or both of potassium chloride and 4,4'-dichlorobenzophenone.
[0071] The chlorine atoms contained in PEEK in the form of potassium chloride as a free component are quantified by the following method.
[0072] <Method for measuring chlorine atoms contained in PEEK in the form of potassium chloride as a free component>
[0073] The solid sample (PEEK) is pulverized in a mixer, washed successively with acetone and water, and dried in an explosion-proof dryer at 180°C. It should be noted that when using the reaction mixture (product) after the reaction of freshly produced PEEK as the sample, after the reaction is completed, the product is cooled and solidified to prepare the above solid sample. The mixer used is not particularly limited, and for example, a 7010HS manufactured by Waring can be used.
[0074] Weigh approximately 1 g of the dried sample, add 100 ml of ultrapure water (1: liter) thereto, stir at a liquid temperature of 50 °C for 20 minutes, allow to cool, and then filter to separate into a solid component and an aqueous solution. Analyze the aqueous solution by ion chromatography, and quantify the chloride ions in the aqueous solution based on a standard curve prepared from a reference of known concentration. The conditions for ion chromatography are as described below.
[0075] <Ion Chromatography>
[0076] Analytical device: Metrohm 940IC Vario
[0077] Column: Connect the (Metrosep A Supp 5Guard) as a guard column and the (Metrosep A Supp 4) as a separation column for use (both columns are manufactured by Metrohm). Eluent: Na2CO3 (1.8 mmol / l) + NaHCO3 (1.7 mmol / l)
[0078] Flow rate: 1.0 ml / min
[0079] Column temperature: 30 °C
[0080] Measurement mode: Suppression mode
[0081] Detector: Conductivity detector
[0082] The chlorine atoms contained in PEEK in the form of 4,4'-dichlorobenzophenone as a free component are quantified by the following method.
[0083] <Method for Determining Chlorine Atoms Contained in PEEK in the Form of 4,4'-Dichlorobenzophenone as a Free Component>
[0084] Crush the solid sample (PEEK) in a mixer, wash successively with acetone and water, and dry in an explosion-proof dryer at 180 °C. It should be noted that when using the reaction mixture (product) after the reaction of freshly produced PEEK as a sample, after the reaction is completed, the product is cooled and solidified to prepare the above solid sample. The mixer used is not particularly limited, and for example, a 7010HS manufactured by Waring can be used.
[0085] Weigh about 1g of the dried sample in an eggplant-shaped flask, add 10ml of acetone and boiling stones, and heat to reflux in a water bath for 5 hours. After cooling to room temperature, remove the solid content by filtration. After the obtained acetone solution is dried with an evaporator, add 10ml of acetone with a whole pipette to redissolve it. By measuring it with gas chromatography, calculate the amount of 4,4'-dichlorobenzophenone in the sample (mg / kg). The amount of chlorine atoms (mg / kg) contained in PEEK in the form of 4,4'-dichlorobenzophenone as a free component is converted by the following calculation formula.
[0086] The amount of chlorine atoms contained in PEEK as 4,4'-dichlorobenzophenone as a free component (mg / kg) = the amount of 4,4'-dichlorobenzophenone in the sample (mg / kg) ÷ 251.11 (molecular weight of 4,4'-dichlorobenzophenone) × 35.45 (atomic weight of chlorine) × 24,4'-dichlorobenzophenone The quantitative value is obtained based on a standard curve prepared from a reference with a known concentration. The measurement conditions are shown below.
[0087] <Gas Chromatography>
[0088] Analytical device: Agilent Technologies 7890B
[0089] GC column: Agilent Technologies DB-5MS (length 30 m, inner diameter 0.25 mm, film thickness 0.25 μm)
[0090] Inlet temperature: 250℃
[0091] Oven temperature: 100℃(1min)→30℃ / min→250℃(10min)
[0092] Flow rate: 1ml / min
[0093] Injection volume: 1μl
[0094] Split ratio: 40:1
[0095] Detector: FID
[0096] Detector temperature: 250°C
[0097] The repeating unit represented by the formula (1) is a linker of the structural unit represented by the following formula (2) and the structural unit represented by the following formula (3).
[0098] [Chemical formula 4]
[0099]
[0100] In PEEK of one embodiment, the structural unit represented by formula (2) is disposed at one or more ends of the molecular chain. In this case, the terminal structure bonded to the structural unit may be a chlorine atom (Cl).
[0101] In one embodiment of PEEK, the structural unit represented by formula (3) is arranged at one or more ends of the molecular chain. In this case, the terminal structure bonded to the structural unit can be, for example, a hydrogen atom (H) or the like (when the terminal structure is a hydrogen atom (H), it forms a hydroxyl group together with the oxygen atom (O) in the structural unit.).
[0102] The terminal structure of PEEK may be, for example, a structure in which the chlorine atom (Cl) or the hydroxyl group is substituted with a hydrogen atom (H) or the like. It should be noted that the terminal structure is not limited to these examples, and may be any structure.
[0103] In one embodiment, PEEK does not contain any other structural units other than the repeating unit represented by formula (1). The ends of the molecular chains may have the terminal structures described above.
[0104] In one embodiment, PEEK does not contain any other structural units other than the structural units represented by formula (2) and formula (3). The ends of the molecular chains may have the terminal structures described above.
[0105] In one embodiment, PEEK contains other structural units other than the structural units represented by formula (2) and formula (3) within a range that does not impair the effects of the present invention.
[0106] In one embodiment, based on all the monomers provided for the reaction, the total ratio (mass %) of the structural units represented by formula (2) and formula (3) contained in all the monomers is 50 mass % or more, 60 mass % or more, 70 mass % or more, 80 mass % or more, 90 mass % or more, 95 mass % or more, 97 mass % or more, 99 mass % or more, 99.5 mass % or more, or 100 mass %.
[0107] In one embodiment, in PEEK, the molar ratio of the structural unit represented by formula (2) to the structural unit represented by formula (3) ([1A]: [2A]) is 47.5:52.5-52.5:47.5, 48.0:52.0-52.0:48.0, 48.5:51.5-51.5:48.5, 49.0:51.0-51.0:49.0 or 49.5:50.5-50.5:49.5.
[0108] The mol number of the structural unit represented by formula (2) may be greater than the mol number of the structural unit represented by formula (3), may be less than the mol number of the structural unit represented by formula (3), or may be the same as the mol number of the structural unit represented by formula (3).
[0109] The above-mentioned molar ratio is usually 1:1, assuming that the total ratio of the structural units represented by the formula (2) and the formula (3) contained in all monomers constituting PEEK is 100% by mass.
[0110] In one embodiment, the melt flow index (abbreviated as "MI": synonymous with the melt flow rate (abbreviated as "MFR") described in ASTM D 1238-13) of PEEK is 1500 g / 10 min or less, 1000 g / 10 min or less, 500 g / 10 min or less, 300 g / 10 min or less, 200 g / 10 min or less, 100 g / 10 min or less, 80 g / 10 min or less, or 60 g / 10 min or less, and is 0.0001 g / 10 min or more, 0.0005 g / 10 min or more, or 0.001 g / 10 min or more.
[0111] The melt flow index of PEEK is, for example, 0.0001 to 1500 g / 10 min, preferably 0.0005 to 500 g / 10 min, and more preferably 0.001 to 100 g / 10 min.
[0112] The melt flow index of PEEK is preferably 100 g / 10 min or less. PEEK having a melt flow index of 100 g / 10 min or less has a sufficiently high molecular weight, and can be preferably granulated using an extruder, for example.
[0113] The melt flow index of PEEK is a value measured by the method described in Examples.
[0114] The melt flow index of PEEK can be adjusted by the temperature conditions of the reaction mixture (maximum temperature, temperature holding time, heating rate, etc.) and the ratio of the raw materials (4,4'-dichlorobenzophenone and hydroquinone, etc.) in the reaction mixture.
[0115] In addition, the melt flow index of PEEK can also be measured by the following measurement method. When measured by this measurement method, the preferred range and the like are also as described above.
[0116] The melt flow index of PEEK was measured under the following measurement conditions in accordance with JIS K 7210-1: 2014 (ISO 1133-1: 2011) using a melt flow indexer (L-220) manufactured by TATEYAMA KAGAKU HIGH-TECHNOLOGIES CO., LTD.
[0117] [Measurement conditions]
[0118] ·Measurement temperature (resin temperature): 380℃
[0119] ·Measurement load: 2.16kg
[0120] ·Barrel inner diameter: 9.550mm
[0121] ·Die head inner diameter: 2.095mm
[0122] Die head length: 8.000mm
[0123] · Piston head length: 6.35mm
[0124] Piston head diameter: 9.474mm
[0125] Piston weight: 110.0 g (the above measured load includes the piston weight)
[0126] ·operate:
[0127] The sample is dried at 150°C for more than 2 hours in advance. The sample is placed in the barrel, the piston is inserted and preheated for 6 minutes. A load is applied, the piston guide is removed, and the molten sample is extruded from the die. The sample is cut within the specified range and specified time (t[s]) of piston movement and the weight (m[g]) is measured. MI is calculated according to the following formula. MI[g / 10min]=600 / t×m
[0128] In one embodiment, the reduced viscosity η of PEEK is sp / c is 0.36 dl / g or more, more than 0.36 dl / g, 0.37 dl / g or more, 0.38 dl / g or more, 0.39 dl / g or more, 0.40 dl / g or more, 0.46 dl / g or more, or 0.48 dl / g or more, and is 1.50 dl / g or less, 1.30 dl / g or less, or 1.20 dl / g or less.
[0129] In addition, the reduced viscosity η of PEEK spThe preferred range of / c is, for example, 0.36 to 1.50 dl / g, more than 0.36 and 1.50 dl / g or less, 0.37 to 1.50 dl / g, 0.40 to 1.50 dl / g, 0.46 to 1.30 dl / g, or 0.48 to 1.20 dl / g. Thus, a molding material can be obtained that ensures appropriate melt fluidity during molding and exhibits more excellent strength.
[0130] Reduced viscosity η of PEEK sp / c is a value measured by the method described in the Examples. In the method described in the Examples, the PEEK concentration in the sulfuric acid solution (sample solution) used for measurement is 0.1 g / dl.
[0131] Reduced viscosity η of PEEK sp / c can be adjusted by the temperature conditions of the reaction mixture (maximum temperature, temperature holding time, heating rate, etc.) and the ratio of the raw materials (4,4'-dichlorobenzophenone and hydroquinone, etc.) in the reaction mixture. sp The same is true for / c.
[0132] It should be noted that the reduced viscosity η of PEEK sp / c can also be measured by the following measurement method. When measured by this measurement method, the preferred range and the like are also as described above.
[0133] PEEK was vacuum dried at 120°C for 6 hours. Next, the PEEK was dissolved in concentrated sulfuric acid (purity 98% by mass), and a sample solution was prepared using a volumetric flask in such a manner that the concentration C [g / dl] of PEEK became 0.1 g / dl. Next, in accordance with JIS K 7367-5:2000 (ISO 1628-5:1998), a 25°C constant temperature water bath (constant temperature bath for kinematic viscosity measurement (THOMAS KAGAKU Instrument Co., Ltd. TV-5S)) and an Ubbelohde viscometer (No. 2) were used to measure the flow time t0 [s] of the solvent (concentrated sulfuric acid (purity 98% by mass)) and the flow time t [s] of the sample solution, and the reduced viscosity η was calculated according to the following formula: sp / c. Reduced viscosity η sp / c[dl / g]=(t-t0) / (t0×C)
[0134] In one embodiment, regarding PEEK, the reduced viscosity η′ measured at 25° C. is a sulfuric acid solution (sample solution) obtained by dissolving PEEK in concentrated sulfuric acid at a concentration of 0.5 g / dl. sp / c (not the reduced viscosity η measured by the method described in the examples) sp / c) is more than 0.36 dl / g, 0.37 dl / g or more, 0.38 dl / g or more, 0.39 dl / g or more, 0.40 dl / g or more, 0.46 dl / g or more, 0.48 dl / g or more, 0.50 dl / g or more, or 0.52 dl / g or more, and is 1.50 dl / g or less, 1.30 dl / g or less, or 1.20 dl / g or less.
[0135] Reduced viscosity η' of PEEK sp The preferred range of / c is, for example, more than 0.36 and 1.50 dl / g or less, 0.37 to 1.50 dl / g, 0.40 to 1.50 dl / g, 0.46 to 1.30 dl / g, or 0.48 to 1.20 dl / g. This ensures appropriate melt flowability during molding and provides a molding material that exhibits more excellent strength.
[0136] It should be noted that the reduced viscosity of PEEK tends to increase as the PEEK concentration in the sample solution used for measurement increases. For example, when measuring the same PEEK, the reduced viscosity η' sp The value of / c (PEEK concentration 0.5 g / dl) has a value greater than the reduced viscosity η sp / c (PEEK concentration 0.1 g / dl) value trend. For example, in the case of PEEK reduced viscosity η sp When / c is 0.36 dl / g, it is estimated that the reduced viscosity η' sp / c is greater than 0.36dl / g.
[0137] In one embodiment, the intrinsic viscosity η of PEEK is inh It is 0.47 dl / g or more, 0.48 dl / g or more, 0.49 dl / g or more, or 0.50 dl / g or more, and is 2.00 dl / g or less, 1.80 dl / g or less, 1.50 dl / g or less, 1.30 dl / g or less, or 1.20 dl / g or less.
[0138] In addition, the intrinsic viscosity of PEEK ηinh The preferred range of is, for example, 0.47 to 2.00 dl / g, 0.47 to 1.50 dl / g, 0.48 to 1.30 dl / g, or 0.50 to 1.20 dl / g. Thus, a molding material can be obtained which ensures appropriate melt fluidity during molding and exhibits more excellent strength.
[0139] It should be noted that the intrinsic viscosity η of PEEK inh It is a value measured by the following measurement method.
[0140] PEEK was vacuum dried at 120°C for 6 hours. Next, the PEEK was dissolved in concentrated sulfuric acid (purity 95% by mass or more) to obtain a plurality of sample solutions with different PEEK concentrations C [g / dl]. Then, in accordance with JIS K 7367-5: 2000 (ISO1628-5: 1998), a 25°C constant temperature water bath (constant temperature bath for kinematic viscosity measurement (THOMAS KAGAKU Instrument Co., Ltd. TV-5S)) and an Ubbelohde viscometer (No. 2) were used to measure the flow time t0 [s] of the solvent (concentrated sulfuric acid (purity 95% by mass or more)) and the flow time t [s] of the sample solution, and the reduced viscosity η was calculated according to the following formula: sp / c. Reduced viscosity η sp / c[dl / g]=(t-t0) / (t0×C)
[0141] The concentration C [g / dl] of each sample solution can be plotted on the horizontal axis and the reduced viscosity η sp The linear correlation equation was obtained by plotting two-dimensionally with / c as the vertical axis, and the reduced viscosity η at zero concentration (intercept) was calculated. sp The intrinsic viscosity η inh And find out.
[0142] Intrinsic viscosity η of PEEK inh The reaction mixture can be adjusted by adjusting the temperature conditions (maximum temperature, temperature holding time, heating rate, etc.) of the reaction mixture and the ratio of the raw materials (4,4'-dichlorobenzophenone and hydroquinone, etc.).
[0143] Using the PEEK of this embodiment, for example, a pellet containing the PEEK can be manufactured. The pellet can be used as various molding materials that require heat resistance, solvent resistance, insulation, etc. The pellet can be used to manufacture a molded body by a molding method such as injection molding using a mold. In addition, the pellet can be used to manufacture a molded body by a molding method such as extrusion molding, press molding, sheet molding, film molding, etc.
[0144] The application of PEEK in this embodiment is not particularly limited. PEEK is suitable for aerospace applications, sliding members such as gears and bearings, and various resin compositions.
[0145] The molded body containing PEEK of this embodiment is suitable as a molded body for aerospace, a molded body for sliding components, and a wire material for a 3D printer. In addition, the molded body containing this PEEK is suitable as an injection molded body for aerospace, and an injection molded body for sliding components.
[0146] The PEEK according to one embodiment of the present invention described above can be produced by reacting 4,4′-dichlorobenzophenone with hydroquinone.
[0147] 4,4'-Dichlorobenzophenone and hydroquinone are monomers used to polymerize PEEK.
[0148] Through the step of reacting 4,4'-dichlorobenzophenone and hydroquinone, PEEK which is a copolymer of these compounds (monomer units) can be obtained.
[0149] 4,4'-Dichlorobenzophenone and hydroquinone can be easily synthesized and are also available as commercial products.
[0150] In the following description, "reaction mixture" refers to the reaction system from the reaction of 4,4'-dichlorobenzophenone and hydroquinone to the end of the reaction, preferably in the form of a solution containing a solvent described later in addition to these monomers. The composition of the reaction mixture may change as the reaction proceeds. Usually, as the reaction proceeds, the concentration of the reactants (4,4'-dichlorobenzophenone and hydroquinone) in the reaction mixture decreases, and the concentration of the product (PEEK) increases.
[0151] The “maximum temperature” of the reaction mixture refers to the highest temperature (maximum reached temperature) reached by the reaction mixture during the period from the start to the end of the reaction of 4,4′-dichlorobenzophenone and hydroquinone.
[0152] In one embodiment, the maximum temperature of the reaction mixture may be 260°C or more, 265°C or more, 270°C or more, 275°C or more, 280°C or more, 285°C or more, 290°C or more, more than 290°C, 295°C or more, 300°C or more, 305°C or more, 310°C or more, 315°C or more, 320°C or more, 325°C or more, 330°C or more, or 335°C or more. The upper limit is not particularly limited, and is, for example, 360°C or less. In addition, the maximum temperature of the reaction mixture is, for example, 260 to 360°C, preferably more than 290°C and less than 360°C, and more preferably 295 to 360°C.
[0153] In one embodiment, the method for producing PEEK of the present embodiment includes the step of heating the reaction mixture to 150° C. or higher and then maintaining the temperature. The temperature during the temperature maintenance is not particularly limited, and may be, for example, 150 to 360° C. The temperature maintenance time is not particularly limited, and may be, for example, 0.1 to 12 hours.
[0154] In one embodiment, the method for producing PEEK of the present embodiment comprises heating the reaction mixture to 150° C. or higher, and then performing the steps of heating and maintaining the temperature once, or repeating the steps of heating and maintaining the temperature multiple times. The number of repetitions is not particularly limited, and may be, for example, 2, 3, 4, 5, 6, 7, 8, 9, or 10 times.
[0155] By repeating the temperature increase and temperature maintenance multiple times, the reaction can be efficiently carried out.
[0156] In one embodiment, the method for producing PEEK of the present embodiment includes the step of maintaining the reaction mixture at 180 to 220° C. for 0.5 to 2 hours, preferably 0.6 to 1.8 hours, and more preferably 0.7 to 1.5 hours (hereinafter also referred to as “temperature maintenance (i)”). Thus, the reaction can be promoted while suppressing the volatilization of the raw materials, and PEEK with a higher molecular weight can be obtained.
[0157] In one embodiment, the method for producing PEEK of the present embodiment includes the step of maintaining the reaction mixture at 230 to 270° C. for 0.5 to 2 hours, preferably 0.6 to 1.8 hours, and more preferably 0.7 to 1.5 hours (hereinafter also referred to as “temperature maintenance (ii)”). Thus, the reaction can be promoted while suppressing the volatilization of the raw materials, and a higher molecular weight PEEK can be obtained.
[0158] In one embodiment, the method for producing PEEK of the present embodiment includes the step of maintaining the reaction mixture at 280 to 360° C. for 1 to 8 hours, preferably 1 to 6 hours, and more preferably 1 to 4 hours (hereinafter also referred to as “temperature maintenance (iii)”). In this way, PEEK of a desired molecular weight can be obtained.
[0159] In one embodiment, the method for producing PEEK of this embodiment may include 2 or 3 selected from the above-mentioned temperature maintenance (i) to (iii). The 2 or 3 temperature maintenances are preferably implemented in sequence starting from the lowest temperature. Between the 2 or 3 temperature maintenances, a step of raising the temperature of the reaction mixture may be included.
[0160] The heating rate when heating the reaction mixture is not particularly limited, and may be, for example, 0.1 to 15°C / min, 0.1 to 10°C / min, 0.1 to 8°C / min, or 0.1 to 5°C / min. This can promote the reaction while suppressing volatilization of the raw materials, and can produce PEEK with a higher molecular weight.
[0161] In one embodiment, in the method for producing PEEK of the present embodiment, the time from the time when the temperature of the reaction mixture reaches 150° C. to the time when the temperature reaches the maximum temperature is 2.0 to 10 hours.
[0162] In one embodiment, the reaction mixture comprises a solvent. The reaction mixture comprising a solvent may be in the form of a solution. The solution may comprise 4,4'-dichlorobenzophenone and hydroquinone dissolved in the solvent.
[0163] The solvent is not particularly limited, and for example, a neutral polar solvent can be used. Examples of the neutral polar solvent include N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dipropylacetamide, N,N-dimethylbenzamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-isopropyl-2-pyrrolidone, N-isobutyl-2-pyrrolidone, N-n-propyl-2-pyrrolidone, N-n-butyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N-methyl-3-methylpyrrolidone, and N-methyl-3-methylpyrrolidone. -2-pyrrolidone, N-ethyl-3-methyl-2-pyrrolidone, N-methyl-3,4,5-trimethyl-2-pyrrolidone, N-methyl-2-piperidone, N-ethyl-2-piperidone, N-isopropyl-2-piperidone, N-methyl-6-methyl-2-piperidone, N-methyl-3-ethylpiperidone, dimethyl sulfoxide, diethyl sulfoxide, 1-methyl-1-oxocyclopentane, 1-ethyl-1-oxocyclopentane, 1-phenyl-1-oxocyclopentane, N,N'-dimethylimidazolidinone, diphenyl sulfone, etc.
[0164] In one embodiment, the reaction mixture contains aromatic sulfone, and the content of the solvent having a boiling point of 270 to 330° C. is 0 to less than 1 part by mass based on 100 parts by mass of the aromatic sulfone. This makes it easy to control the reaction temperature.
[0165] The reaction mixture may contain one or more solvents. In particular, it is preferred that the reaction mixture contains only one solvent (single solvent) as a solvent, thereby simplifying the process.
[0166] In one embodiment, the reaction mixture comprises potassium carbonate. Thus, the reaction is facilitated.
[0167] In one embodiment, potassium carbonate satisfies at least one of the following conditions (A) and (B). Thereby, the molecular weight of the obtained PEEK can be increased.
[0168] (A) The bulk density of potassium carbonate is 1.2 g / ml (1: liter) or less.
[0169] (B) When the average particle size of potassium carbonate is D (μm) and the specific surface area is S (m 2 / g), D / S≤600.
[0170] In one embodiment, the bulk density of potassium carbonate is 1.2 g / ml or less, 1.1 g / ml or less, or 1.0 g / ml or less, and is 0.05 g / ml or more, or 0.10 g / ml or more.
[0171] The bulk density of potassium carbonate may be, for example, 0.05 g / ml to 1.2 g / ml, 0.05 g / ml to 1.1 g / ml, 0.05 g / ml to 1.0 g / ml, 0.10 g / ml to 1.2 g / ml, 0.10 g / ml to 1.1 g / ml, or 0.10 g / ml to 1.0 g / ml.
[0172] By setting the bulk density of potassium carbonate to 1.2 g / ml or less, the molecular weight of the obtained PEEK can be increased.
[0173] The bulk density of potassium carbonate is a value measured by the following method.
[0174] About 50 g of potassium carbonate (mass m (g)) weighed with an accuracy of 0.1 mass % is gently placed in a dry 100 ml graduated cylinder (minimum scale unit: 1 ml) without compacting. The upper surface of the powder layer is carefully leveled without compacting, and the loose bulk volume V0 (ml) is read to the smallest scale unit, and the bulk density is calculated by the following formula.
[0175] Bulk density (g / ml) = m / V0
[0176] When the loose bulk volume V0 exceeded 100 ml, the mass m of potassium carbonate as a sample was subtracted to adjust the capacity so that the loose bulk volume V0 became 100 ml or less, and the loose bulk volume V0 was read to calculate the bulk density.
[0177] In one embodiment, when the average particle size of potassium carbonate is D (μm) and the specific surface area is S (m 2 / g), the value of D / S is 600 or less, 550 or less, or 500 or less, and is 0.1 or more, 0.2 or more, or 0.5 or more.
[0178] The value of D / S may be, for example, 1 to 600, 1 to 550, 1 to 500, 2 to 600, 2 to 550, 2 to 500, 5 to 600, 5 to 550, or 5 to 500.
[0179] By setting D / S ≤ 600, the molecular weight of the obtained PEEK can be increased.
[0180] The average particle size D (μm) of potassium carbonate is a value measured by the method described below.
[0181] The particle size distribution was measured by a dry method using a CAMSIZER manufactured by Microtrac BEL Co., Ltd. The sample (potassium carbonate) was dropped into the measuring section using a vibrating feeder, and the particles were photographed with a camera to measure the particle size. When the observed image was processed, the average particle size D was calculated by automatic calculation based on the program provided by the measuring device using the numerical value obtained by processing the data of the short diameter of the particle image.
[0182] The specific surface area of potassium carbonate S (m 2 / g) was measured by the method shown below.
[0183] (i) Pre-treatment
[0184] As a pretreatment of the sample (potassium carbonate), heating vacuum exhaust was performed at 100° C. for 1 hour or more using BELPREP vacII manufactured by Microtrac BEL. The pretreatment was completed when the vacuum degree reached 10 Pa (75 mTorr).
[0185] (ii) Determination
[0186] The specific surface area was measured by nitrogen adsorption at liquid nitrogen temperature using BELSORP-miniII manufactured by Microtrac BEL Co., Ltd. The nitrogen introduction amount was set in the "simple mode" of the device, and the target relative pressure was 0.10, 0.15, 0.20, 0.25, and 0.30.
[0187] (iii) Analysis
[0188] BEL Master was used as the analysis software. The analysis method was based on JIS Z 8830:2013, and the specific surface area S was calculated by the BET multipoint method using 4 or more points from the measurement results of the higher relative pressure.
[0189] In one embodiment, potassium carbonate can be measured by the above method, for example, by using a bulk density of 0.90 [g / ml], an average particle size D = 460 [μm], and a specific surface area S = 1.51 [m 2 / g], potassium carbonate with D / S=305, etc.
[0190] In one embodiment, the reaction mixture contains alkali metal salts such as alkali metal carbonates and alkali metal bicarbonates other than potassium carbonate. These alkali metal salts can be used in combination with potassium carbonate. For example, potassium carbonate and sodium carbonate can also be used in combination.
[0191] Examples of the alkali metal carbonate include lithium carbonate, rubidium carbonate, and cesium carbonate.
[0192] Examples of the alkali metal hydrogen carbonate that can be used together with potassium carbonate include lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, rubidium hydrogen carbonate, and cesium hydrogen carbonate.
[0193] These alkali metal salts may be used alone or in combination of two or more.
[0194] The total concentration of the alkali metal salt (including potassium carbonate and the above-mentioned other alkali metal salts) in the reaction mixture is not particularly limited.
[0195] In one embodiment, the total amount of the alkali metal salt in the reaction mixture is 100 mol parts or more relative to 100 mol parts of hydroquinone incorporated into the reaction mixture, and is 180 mol parts or less, 160 mol parts or less, 140 mol parts or less, or 120 mol parts or less. If the total amount of the alkali metal salt is 100 mol parts or more, the reaction time can be shortened. If the total amount of the alkali metal salt is 180 mol parts or less, the formation of the gel component can be suppressed. In addition, the total amount of the alkali metal salt in the reaction mixture is, for example, 100 to 180 mol parts relative to 100 mol parts of hydroquinone incorporated into the reaction mixture, preferably 100 to 140 mol parts, and more preferably 100 to 120 mol parts.
[0196] In one embodiment, potassium carbonate is blended as the alkali metal salt in the above-mentioned blending amount.
[0197] In one embodiment, the reaction mixture does not contain any of sodium fluoride, potassium fluoride, rubidium fluoride and cesium fluoride. In this embodiment, even if these compounds are not contained, high molecular weight PEEK can be obtained. In addition, by not containing these compounds, these compounds can be avoided from remaining in the obtained PEEK, and the purification cost can be reduced. Thus, PEEK that can exert excellent mechanical strength by combining inorganic compounds can be manufactured at low cost.
[0198] The molar ratio ([DCBP]:[HQ]) of 4,4′-dichlorobenzophenone (DCBP) and hydroquinone (HQ) used in the reaction is not particularly limited.
[0199] The molar ratio ([DCBP]:[HQ]) can be appropriately adjusted for the purpose of controlling the molecular weight of the obtained PEEK.
[0200] In one embodiment, the molar ratio ([DCBP]:[HQ]) is 47.5:52.5-52.5:47.5, 48.0:52.0-52.0:48.0, 48.5:51.5-51.5:48.5, 49.0:51.0-51.0:49.0, or 49.5:50.5-50.5:49.5.
[0201] The mol number of 4,4'-dichlorobenzophenone (DCBP) may be greater than the mol number of hydroquinone (HQ), may be less than the mol number of hydroquinone (HQ), or may be the same as the mol number of hydroquinone (HQ).
[0202] In one embodiment, the total concentration of 4,4'-dichlorobenzophenone and hydroquinone in the reaction mixture (based on the amount of compounding) is not particularly limited, for example, 1.0 mol / l or more, 1.2 mol / l or more, 1.3 mol / l or more, 1.4 mol / l or more, or 1.5 mol / l or more, and 6.0 mol / l or less, 5.0 mol / l or less, or 4.0 mol / l or less. In addition, the total concentration of 4,4'-dichlorobenzophenone and hydroquinone in the reaction mixture (based on the amount of compounding) is, for example, 1.0 to 6.0 mol / l, preferably 1.3 to 5.0 mol / l, and more preferably 1.5 to 4.0 mol / l.
[0203] In one embodiment, as the monomers used in the above reaction, no monomers other than 4,4′-dichlorobenzophenone and hydroquinone are used.
[0204] In one embodiment, in the above reaction, other monomers other than 4,4′-dichlorobenzophenone and hydroquinone are used in combination within a range that does not impair the effects of the present invention.
[0205] In one embodiment, the total ratio (mass %) of 4,4'-dichlorobenzophenone and hydroquinone based on all monomers supplied to the reaction is 50 mass % or more, 60 mass % or more, 70 mass % or more, 80 mass % or more, 90 mass % or more, 95 mass % or more, 97 mass % or more, 99 mass % or more, 99.5 mass % or more, or 100 mass %.
[0206] In one embodiment, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 99% by mass or more, 99.5% by mass or more, 99.9% by mass or more, or substantially 100% by mass of the reaction mixture at the start of the reaction is:
[0207] 4,4'-dichlorobenzophenone, hydroquinone, alkali metal salt and solvent,
[0208] 4,4'-dichlorobenzophenone, hydroquinone, one or more alkali metal salts selected from potassium carbonate and sodium carbonate, and diphenyl sulfone, or
[0209] 4,4'-Dichlorobenzophenone, hydroquinone, potassium carbonate, and diphenyl sulfone.
[0210] In addition, in the case of "substantially 100 mass %", inevitable impurities may be contained.
[0211] The reaction of 4,4'-dichlorobenzophenone and hydroquinone can be carried out in an inert gas atmosphere. The inert gas is not particularly limited, and examples thereof include nitrogen and argon.
[0212] 2. Composition
[0213] A composition according to one embodiment of the present invention includes PEEK and an inorganic compound, wherein the PEEK includes a repeating unit represented by the following formula (1) and satisfies one or both of the following conditions (A) and (B).
[0214] [Chemical formula 5]
[0215]
[0216] (A) The fluorine atom content a is less than 2 mg / kg.
[0217] (B) The chlorine atom content b is 2 mg / kg or more.
[0218] The composition of this embodiment exhibits excellent mechanical strength.
[0219] Regarding the conditions (A) and (B), the description of PEEK according to one embodiment of the present invention is cited, and a detailed description thereof is omitted here.
[0220] The PEEK contained in the composition of the present embodiment is not particularly limited as long as it satisfies one or both of the conditions (A) and (B).
[0221] In one embodiment, the PEEK contained in the composition of this aspect is the PEEK of one aspect of the present invention described above. Thereby, the composition exhibits more excellent mechanical strength.
[0222] In one embodiment, the inorganic compound is one or more selected from glass fiber, carbon fiber and boron nitride. Thereby, the strength of the composition is further improved.
[0223] In one embodiment, the inorganic compound is one or more selected from glass fiber and carbon fiber, and is in the form of one or more selected from chopped strands, rovings, fabrics, nonwoven fabrics, and unidirectional materials (also referred to as "UD materials"), thereby further improving the strength of the composition.
[0224] In one embodiment, the inorganic compound is glass fiber.
[0225] In one embodiment, the composition may be a fiber composite material including PEEK as a matrix and a fibrous inorganic compound such as glass fiber, carbon fiber, etc. The fiber composite material may be a so-called fiber reinforced thermoplastic (FRTP).
[0226] The fibrous inorganic compound can be treated with a sizing agent. The fibrous inorganic compound can be bundled into a bundle by the sizing agent. The fibrous inorganic compound treated with the sizing agent has the sizing agent attached to its surface. The sizing agent is not particularly limited, and examples thereof include epoxy sizing agents, urethane sizing agents, polyamide sizing agents, and the like. In addition, as a sizing agent, PEEK of one embodiment of the present invention can also be used. As a sizing agent, one of them can be used alone, or two or more can be used in combination. As a fibrous inorganic compound, an inorganic compound that has not been treated with a sizing agent can be used.
[0227] In one embodiment, the inorganic compound is an inorganic compound that has a reinforcing effect on PEEK. Here, the "inorganic compound that has a reinforcing effect on PEEK" is an inorganic compound that has a tensile strength greater than the tensile strength of PEEK without the inorganic compound when 43 parts by mass of the inorganic compound is uniformly contained in 100 parts by mass of PEEK. The tensile strength is measured by the method described in the examples.
[0228] The content of the inorganic compound in the composition is not particularly limited.
[0229] In one embodiment, the content of the inorganic compound in the composition is, for example, 5 parts by mass or more, 10 parts by mass or more, or 20 parts by mass or more, and is 60 parts by mass or less, 55 parts by mass or less, or 50 parts by mass or less, relative to 100 parts by mass of PEEK. The upper limit and the lower limit may be combined arbitrarily.
[0230] The composition may include other components other than PEEK and the inorganic compound. Other components are not particularly limited, and for example, other resins other than PEEK may be cited. As other resins, for example, fluororesins such as polytetrafluoroethylene may be cited. As other components, one may be used alone, or two or more may be used in combination.
[0231] In one embodiment, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, 99% by mass or more, 99.5% by mass or more, or substantially 100% by mass of the composition is:
[0232] PEEK,
[0233] PEEK and inorganic compounds,
[0234] PEEK and other components mentioned above, or
[0235] PEEK, inorganic compounds and other ingredients listed above.
[0236] In addition, in the case of "substantially 100 mass %", unavoidable impurities may be contained.
[0237] The method for preparing the composition is not particularly limited, and examples thereof include mixing with a known mixer, melt kneading with an extruder, etc. The inorganic compound may be fed to the PEEK side using a twin-screw kneader.
[0238] The composition can be pelletized and used as a raw material for producing a molded body.
[0239] In one embodiment, the method for producing pellets includes the steps of chopping a fibrous inorganic compound into short strands and then adding PEEK to the short strands. The pellets (also referred to as "short fiber pellets") are produced by mixing the short strands and PEEK and granulating them.
[0240] In one embodiment, in a method for producing pellets, a fibrous inorganic compound roving is immersed in molten PEEK and drawn and then cut into a desired pellet length to produce pellets (also referred to as "long-fiber pellets"). When producing long-fiber pellets as described above, the breakage of the fibrous inorganic compound can be suppressed.
[0241] By shaping the composition (which may be in the form of the above-mentioned pellets), a molded body can be manufactured. The molding can be performed using known methods such as injection molding, extrusion molding, and blow molding. In addition, the composition can also be press-molded, and known methods such as cold pressing and hot pressing can be used. In addition, the composition can also be used as a resin composition for a 3D printer and molded using a 3D printer.
[0242] In one embodiment, the tensile strength of the composition is more than 76MPa, more than 78MPa, more than 80MPa, more than 82MPa, more than 84MPa, more than 86MPa, more than 88MPa, more than 89MPa, more than 90MPa, more than 91MPa or more than 92MPa. Thus, the composition can be more suitably used for purposes requiring mechanical strength. The upper limit is not particularly limited, for example, less than 300MPa, less than 200MPa, less than 180MPa, less than 150MPa, less than 130MPa or less than 120MPa.
[0243] The tensile strength of the composition is, for example, 76 to 300 MPa, preferably 80 to 200 MPa, and more preferably 90 to 180 MPa.
[0244] The tensile strength of the composition is a value measured by the method described in Examples.
[0245] 3. Slices
[0246] A sheet according to one embodiment of the present invention comprises a cloth containing an inorganic compound and PEEK impregnated in the cloth. According to this sheet, excellent mechanical strength is exhibited similarly to the case where the inorganic compound is contained in PEEK.
[0247] The cloth is not particularly limited as long as it contains fibers of an inorganic compound. In one embodiment, the cloth is composed of fibers arranged in a planar shape. The cloth may be, for example, a woven fabric, a nonwoven fabric, a unidirectional material, or the like.
[0248] Unidirectional materials are made of fibers that are aligned in one direction.
[0249] The fibers contained in the cloth are not particularly limited.
[0250] The cloth preferably contains one or more selected from glass fibers and carbon fibers. In one embodiment, the cloth contains glass fibers.
[0251] In one embodiment, the sheet can be a fiber composite material comprising PEEK as a matrix and a fibrous inorganic compound such as glass fiber, carbon fiber, etc. The fiber composite material can be a so-called fiber reinforced thermoplastic (FRTP). For example, by using a unidirectional material as a cloth, a unidirectional fiber reinforced plastic can be obtained.
[0252] In the sheet of one embodiment, PEEK is impregnated between fibers contained in the cloth. The cloth may be a single sheet or a laminated body formed by laminating two or more sheets. When the cloth is a laminated body, PEEK can also contribute to the bonding between the cloths.
[0253] The sheet may contain other components in addition to PEEK and cloth. As other components, the components described in the composition can be used.
[0254] In one embodiment, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, 99% by mass or more, 99.5% by mass or more, or substantially 100% by mass of the sheet is:
[0255] PEEK and cloth, or
[0256] PEEK, cloth and other ingredients listed above.
[0257] In addition, in the case of "substantially 100 mass %", unavoidable impurities may be contained.
[0258] The method for producing the sheet is not particularly limited.
[0259] In one embodiment, the method for manufacturing the sheet includes the step of impregnating the cloth with PEEK. In this case, for example, a solution obtained by dissolving PEEK in a suitable solvent, a mixture obtained by mixing PEEK with a suitable carrier, or a melt of PEEK can be applied to the carbon fiber and impregnated.
[0260] In one embodiment, a method of making a sheet includes the step of making a cloth from fibers bundled with a sizing agent comprising PEEK.
[0261] In one embodiment, the method for manufacturing a sheet includes the steps of laminating a film including PEEK on a cloth and performing melt pressing.
[0262] In one embodiment, the method for manufacturing the sheet includes the steps of directly adding PEEK powder to the cloth and then melting the powder.
[0263] In the above description of the method for producing a sheet, the cloth impregnated with PEEK may be the above-mentioned laminate.
[0264] In one embodiment, the sheet is planar across its entire surface.
[0265] In one embodiment, a three-dimensional shape is imparted to the sheet. The sheet shape being "three-dimensional" means that the sheet includes a curved portion (including a bent portion).
[0266] The method for producing the sheet imparted with a three-dimensional shape is not particularly limited.
[0267] In one embodiment, a method for producing a sheet imparted with a three-dimensional shape includes the step of impregnating a cloth imparted with a three-dimensional shape with PEEK.
[0268] In one embodiment, a method for producing a sheet having a three-dimensional shape comprises impregnating a cloth with PEEK to obtain a sheet (eg, a planar sheet), and then forming the sheet so as to give the sheet a three-dimensional shape. Forming can be performed, for example, by applying pressure to the sheet under heating.
[0269] In the above description of the sheet, PEEK may be impregnated into the cloth as the composition of one embodiment of the present invention. In this case, the composition may or may not contain an inorganic compound.
[0270] Example
[0271] Hereinafter, examples of the present invention will be described, but the present invention is not limited to these examples.
[0272] (Example 1)
[0273] In a 300 ml four-necked flask equipped with a stirrer, a thermometer, a nitrogen inlet tube, and a water recovery container connected to a condenser, 40.613 g (0.162 mol) of 4,4'-dichlorobenzophenone, 17.809 g (0.162 mol) of hydroquinone, 25.704 g (0.186 mol) of potassium carbonate, and 140.01 g of diphenyl sulfone were added, and nitrogen gas was flowed.
[0274] The reaction mixture was allowed to react under the following temperature control.
[0275] <Temperature Control>
[0276] (1) After heating to 150°C, heat to 200°C over 30 minutes
[0277] (2) Maintain at 200°C for 1 hour
[0278] (3) Heating from 200°C to 250°C (heating rate 1.7°C / min)
[0279] (4) Maintain at 250°C for 1 hour
[0280] (5) Heating from 250°C to 340°C (maximum temperature of the reaction mixture) (heating rate 3.0°C / min)
[0281] (6) Maintain at 340°C (maximum temperature of the reaction mixture) for 2 hours
[0282] After the reaction was completed, the product was pulverized with a mixer (7010HS manufactured by Waring Co.), washed with acetone and water in that order, and then dried in a dryer at 180° C. to obtain powdered PEEK.
[0283] The obtained PEEK was subjected to the following measurements (1) to (5).
[0284] (1) Melt flow index (MI)
[0285] The melt flow index of PEEK was measured at a resin temperature of 380° C. and a load of 2.16 kg in accordance with ASTM D 1238-13 using a melt flow indexer (L-227) manufactured by Tateyama Kagaku High-Technologies Co., Ltd.
[0286] (2) 1 H-NMR measurement (area ratio X)
[0287] PEEK is used in 1In H-NMR measurement, the ratio (area ratio X) of the peak area at the α position of the hydroxyl group (area of chemical shift 6.98 ppm to 7.03 ppm) to the main chain peak area (area of chemical shift 7.32 ppm to 7.36 ppm) was determined by the following formula.
[0288] Area ratio X[%] = (area of the peak at the α position of the hydroxyl group / area of the main chain peak) × 100
[0289] 1 The measurement conditions of H-NMR measurement are as follows.
[0290] < 1 H-NMR measurement conditions>
[0291] ·NMR device: Ascend500 manufactured by Bruker Japan Co., Ltd.
[0292] Probe: 5mm φTCI cryoprobe (Cryoprobe)
[0293] NMR sample tube diameter: 5mm φ
[0294] Preparation of sample solution: 0.6 ml of methanesulfonic acid was added to about 20 mg of a sample, and the mixture was stirred at room temperature for 1 hour. Then, 0.4 ml of deuterated dichloromethane was added, and the mixture was further stirred at room temperature for 30 minutes to dissolve the sample to prepare a sample solution.
[0295] Observation range: 20ppm
[0296] Observation center: 6.175ppm
[0297] Number of data points: 64kB
[0298] Pulse repetition time: 10 seconds
[0299] Total times: 256 times
[0300] Flip angle: 30°
[0301] ·Measurement temperature: 25℃
[0302] Chemical shift reference: The central peak among the three peaks of deuterated dichloromethane was set to 5.32 ppm
[0303] (3) Combustion ion chromatography
[0304] The fluorine atom content a and the chlorine atom content b in PEEK were measured by combustion ion chromatography.
[0305] Specifically, the sample is introduced into a combustion furnace and burned in a combustion gas containing oxygen. After the generated gas is captured in an absorbent, the absorbent is separated and quantified using an ion chromatograph. The quantitative value is obtained based on a standard curve made from a reference of known concentration. The measurement conditions are shown below.
[0306] <Sample Combustion>
[0307] Combustion device: AQF-2100H manufactured by Mitsubishi Chemical Analytech Co., Ltd.
[0308] Combustion furnace set temperature: 800℃ for the front section, 1100℃ for the rear section
[0309] Argon flow rate: 400ml / min
[0310] Oxygen flow rate: 200ml / min
[0311] Absorbent: Hydrogen peroxide
[0312] <Ion Chromatography>
[0313] Analytical device: Integrion manufactured by Thermo Fisher Scientific Co., Ltd.
[0314] Column: A guard column (Dionex IonPac AG12A) and a separation column (Dionex IonPac AS12A) were connected and used (both columns were manufactured by Dionex)
[0315] Eluent: Na2CO3 (2.7mmol / 1) + NaHCO3 (0.3mmol / 1)
[0316] Flow rate: 1.5ml / min
[0317] Column temperature: 30°C
[0318] Measurement mode: Suppression mode
[0319] Detector: Conductivity detector
[0320] It should be noted that the detection limit of fluorine and chlorine atoms in the above determination method is 2 mg / kg. When these atoms are less than the detection limit, they are marked as "<2" (mg / kg) in Table 1 (the same applies to Table 2 below).
[0321] (4) Reduced viscosity η sp / c
[0322] The reduced viscosity η of a solution prepared by dissolving PEEK in concentrated sulfuric acid (purity 95 mass % or more) to a concentration of 0.1 g / dl was measured at 25° C. using an Ubbelohde viscometer in accordance with JIS K7367-5:2000. sp / c.
[0323] (5) Reinforcement of Inorganic Compounds (Determination of Tensile Strength)
[0324] 100 parts by mass of the obtained PEEK and 43 parts by mass of an inorganic compound (glass fiber; "T-786H" manufactured by Nippon Electric Glass Co., Ltd., average fiber diameter 10 μm, average fiber length 3.0 mm) were kneaded at 380° C. for 5 minutes using a plastic order manufactured by Brabender to obtain a composition.
[0325] The obtained composition was press-formed into a thickness of 2 mm at 380° C. using a vacuum press manufactured by Imoto Seisakusho Co., Ltd., and annealed at 200° C. to obtain a press-formed plate. The press-formed plate was cut into a dumbbell-shaped 5A shape specified in JIS K7161 as a test piece. The obtained test piece was subjected to a tensile test at a test speed of 5 mm / min and a distance between chucks of 50 mm to measure the tensile strength.
[0326] The above results are shown in Table 1.
[0327] (Example 2)
[0328] In Example 1, PEEK was obtained in the same manner as in Example 1, except that acetone, water, and N-methyl-2-pyrrolidone were used in sequence for washing after the reaction. The obtained PEEK was subjected to the same measurement as in Example 1. The results are shown in Table 1.
[0329] (Example 3)
[0330] In Example 1, PEEK was obtained in the same manner as in Example 1 except that the composition of the reaction mixture was changed to 52.499 g (0.209 mol) of 4,4'-dichlorobenzophenone, 22.464 g (0.204 mol) of hydroquinone, 32.4324 g (0.235 mol) of potassium carbonate, and 120.02 g of diphenyl sulfone. The obtained PEEK was subjected to the same measurement as in Example 1. The results are shown in Table 1.
[0331] (Example 4)
[0332] In Example 1, PEEK was obtained in the same manner as in Example 1 except that the amount of 4,4'-dichlorobenzophenone was changed to 41.224 g (0.164 mol) and the maximum temperature of the reaction mixture was set to 280°C. The obtained PEEK was subjected to the same measurements as in Example 1. The results are shown in Table 1.
[0333] (Example 5)
[0334] In Example 1, PEEK was obtained in the same manner as in Example 1 except that the amount of 4,4'-dichlorobenzophenone was changed to 41.209 g (0.164 mol) and the maximum temperature of the reaction mixture was set to 300°C. The obtained PEEK was subjected to the same measurements as in Example 1. The results are shown in Table 1.
[0335] (Comparative Example 1)
[0336] The PEEK obtained in Example 5 was subjected to the same tensile strength measurement as in Example 1, except that reinforcement with an inorganic compound was omitted.
[0337] Specifically, the PEEK obtained in Example 5 was press-formed into a thickness of 2 mm at 380° C. using a vacuum press manufactured by Imoto Manufacturing Co., Ltd., and annealed at 200° C. to obtain a press-formed plate. The press-formed plate was cut into a dumbbell-shaped 5A shape specified in JIS K7161 as a test piece. The obtained test piece was subjected to a tensile test at a test speed of 5 mm / min and a distance between chucks of 50 mm to measure the tensile strength.
[0338] The results are shown in Table 1.
[0339] [Table 1]
[0340]
[0341] (Synthesis example 1)
[0342] In Example 1, a 2-liter reaction container (equipped with a stirrer, a thermometer, a nitrogen inlet tube, and a water recovery container connected to a condenser) was used instead of a 300-ml four-necked flask, and 284.30 g (1.132 mol) of 4,4'-dichlorobenzophenone, 124.66 g (1.132 mol) of hydroquinone, 179.91 g (1.302 mol) of potassium carbonate, and 980.01 g of diphenyl sulfone were added to the reaction container to prepare a reaction mixture. Powdered PEEK was obtained in the same manner as in Example 1, except that the reaction mixture was prepared.
[0343] The melt flow index (MI), area ratio X, chlorine atom content b and reduced viscosity η of the obtained PEEK were measured in the same manner as in Example 1. sp / c, the results are as follows.
[0344] MI: 42g / 10min
[0345] Area ratio X: 1.22%
[0346] Chlorine atom content: 1400mg / kg
[0347] Reduced viscosity η sp / c: 0.52dl / g
[0348] Several embodiments and / or examples of the present invention have been described in detail above, but those skilled in the art can easily make more changes to these illustrative embodiments and / or examples without departing from the new teachings and effects of the present invention. Therefore, these more changes are included in the scope of the present invention.
[0349] The contents of the documents described in this specification and the applications on which the Paris Convention priority claim of the present application is based are incorporated herein by reference in their entirety.
Claims
1. A composition comprising: polyetheretherketone, wherein the polyetheretherketone comprises a repeating unit represented by the following formula (1), wherein the polyetheretherketone satisfies one or both of the following conditions (A) and (B), and has a hydroxyl group at one or both ends of the main chain, wherein 1 The area ratio of the peak at the α position of the hydroxyl group to the main chain peak in H-NMR measurement is 0.24% to 2.00%; and One or more selected from glass fiber and carbon fiber, The intrinsic viscosity η of the polyetheretherketone inh 0.50dl / g~2.00dl / g, The reaction mixture for producing the polyetheretherketone contains only potassium carbonate as the alkali metal salt, (A) the fluorine atom content a is less than 2 mg / kg, (B) The chlorine atom content b is 2 mg / kg or more.
2. The composition according to claim 1, wherein The raw material of the polyetheretherketone contains 4,4'-dichlorobenzophenone.
3. The composition according to claim 1 or 2, wherein The reduced viscosity η of the polyetheretherketone sp / c is 0.40dl / g~1.00dl / g.
4. The composition according to claim 1 or 2, wherein The one or more selected from glass fibers and carbon fibers are in the form of one or more selected from chopped strands, rovings, fabrics, nonwoven fabrics, and unidirectional materials.
5. The composition according to claim 1 or 2, wherein The at least one selected from glass fiber and carbon fiber is glass fiber.
6. A sheet comprising: A cloth containing one or more selected from glass fiber and carbon fiber as a constituent material; and polyetheretherketone impregnated in the cloth, The polyetheretherketone comprises a repeating unit represented by the following formula (1) and satisfies one or both of the following conditions (A) and (B), and has a hydroxyl group at one or both ends of the main chain. 1 The area ratio of the peak at the α position of the hydroxyl group to the main chain peak in H-NMR measurement is 0.24% to 2.00%. The intrinsic viscosity η of the polyetheretherketone inh 0.50dl / g~2.00dl / g, The reaction mixture for producing the polyetheretherketone contains only potassium carbonate as the alkali metal salt, (A) the fluorine atom content a is less than 2 mg / kg, (B) The chlorine atom content b is 2 mg / kg or more.
7. The sheet according to claim 6, wherein The cloth is a unidirectional material.