Preparation and Application of Zwitterionic Modified Titanium Carbide Nanosheet Filled Film
By blending zwitterionic modified titanium carbide nanosheets with cross-linked polyethylene oxide polymer matrix, a hybrid matrix membrane was prepared, which solved the problem of low CO2 capture and separation efficiency and achieved a highly efficient CO2/N2 gas separation effect.
Patent Information
- Application Number
- CN202310268372.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing CO2 capture and separation technologies suffer from low efficiency and high energy consumption. Traditional separation technologies also suffer from high energy consumption and byproduct generation during greenhouse gas separation. The application prospects of two-dimensional nanosheet materials in the field of gas separation have not been fully realized.
A hybrid matrix membrane was prepared by blending zwitterionic modified titanium carbide nanosheets with a cross-linked polyethylene oxide polymer matrix. By enhancing the dissolution-diffusion mechanism of CO2 gas molecules, the separation efficiency of CO2/N2 gas was improved.
It achieves high permeability and high selectivity separation of CO2, with a CO2 permeability of 4953 Barrer and a maximum CO2/N2 gas selectivity of 29, which is superior to traditional methods.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of membrane separation technology, and mainly to the preparation and application of zwitterionic modified titanium carbide nanosheet filled membrane. Technical Background
[0002] Fossil fuels, considered the lifeblood of industry since the Industrial Revolution, will continue to play a crucial role in the next half-century. However, fossil fuels emit large amounts of CO2. CO2 is a major component of greenhouse gases; excessive CO2 emissions damage the ozone layer, directly contributing to global warming, triggering extreme weather events such as heat waves, droughts, and torrential rains, and causing sea-level rise, threatening human survival and marine life. Therefore, developing efficient and economical CO2 capture and separation technologies is a pressing technical problem that needs to be solved in global industrial production.
[0003] Membrane separation technology is an emerging and highly efficient separation technology with significant advantages such as simple process, low energy consumption, convenient operation, and easy scale-up. Furthermore, due to its mild reaction conditions, absence of phase change, and lack of introduction of a third component, membrane separation technology has the potential to replace traditional separation technologies. Gas separation membrane technology, driven by the pressure difference across the membrane, boasts low energy consumption; the production process generates no byproducts, making it environmentally friendly; the process is simple, easy to scale up, and offers extremely high economic benefits.
[0004] Two-dimensional transition metal carbides / nitrides, namely MXene nanosheets, are a novel type of two-dimensional nanosheet material. They possess abundant surface functional groups, excellent mechanical properties, and nanoscale thickness, making them widely applicable in gas separation, water treatment, and photocatalysis. Titanium carbide (Ti3C2T) x Nanosheets are a typical representative of the MXene family. Their surface contains a large number of -OH functional groups, which are easy to chemically modify. The thickness of a single nanosheet is 0.98 nm, and the surface is smooth, which is conducive to the rapid mass transfer of gas molecules. The size of the nanosheets is adjustable from the nanometer to the micrometer level, and they have good application prospects in the field of gas separation. Summary of the Invention
[0005] In summary, the purpose of this invention is to provide a method for preparing and applying a zwitterionic modified titanium carbide nanosheet filled membrane. This invention targets CO2 separation by blending zwitterionic modified titanium carbide nanosheets with a cross-linked polyethylene oxide (XLPEO) polymer matrix to prepare a mixed matrix membrane. By enhancing the dissolution-diffusion mechanism of CO2 gas molecules, CO2 / N2 gas separation is achieved.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0007] A zwitterionic modified titanium carbide nanosheet filled film, wherein the zwitterionic modified titanium carbide nanosheet filled film is composed of a polyethylene oxide polymer matrix film and zwitterionic modified titanium carbide nanosheets filled in the matrix film, wherein the modified titanium carbide nanosheets (i.e. pSBMA@Ti3C2T) x Nanosheets are two-dimensional nanosheet materials with high specific surface area and nanoscale thickness, and rich in zwitterionic compounds (polymethacryloylethyl sulfobetaine) on their surface.
[0008] Preferably, the lateral dimension of the zwitterionic modified titanium carbide nanosheet material is 200 nm to 500 nm.
[0009] Preferably, the polyethylene oxide polymer in the zwitterionic modified titanium carbide nanosheet filling film is composed of polyethylene glycol methyl ether acrylate (PEGMEA) and polyethylene glycol diacrylate (PEGDA) in a mass ratio of (5-8):(2-5).
[0010] Preferably, the zwitterionic modified titanium carbide nanosheet filled film contains pSBMA@Ti3C2T x The mass ratio of the crosslinked polyethylene oxide to the ethylene oxide is (0.001~0.008):1.
[0011] Preferably, the thickness of the zwitterionic modified titanium carbide nanosheet filling film is 100–220 μm.
[0012] Preferably, the zwitterionic modified titanium carbide nanosheet filled membrane is in the form of a flat sheet membrane, a hollow fiber membrane, or a tubular membrane.
[0013] This invention also provides a method for preparing the zwitterionic modified titanium carbide nanosheet filled film described in the above technical solution, the steps of which are as follows:
[0014] Step 1: Prepare titanium carbide nanosheets, denoted as Ti3C2T x
[0015] Ti3C2T was prepared by chemical etching of aluminum carbide (Ti3AlC2) precursor using a hydrochloric acid + lithium fluoride system. x A hydrochloric acid solution was measured and added to a polytetrafluoroethylene reactor. Lithium fluoride was weighed and added to the reactor, and the mixture was stirred until dissolved. Then, aluminum carbide was slowly added to the solution, with a mass ratio of hydrochloric acid, lithium fluoride, and aluminum carbide of (8.76–17.52):(2.6–3.8):2. The mixture was stirred and reacted at 10–45°C for 24–48 hours. The mixture was then washed 5–6 times by centrifugation with deionized water. Deionized water was added to the precipitate, and the mixture was sonicated for 1 hour in an ice bath under an inert gas atmosphere to obtain Ti3C2T. xSolution. Finally, add 1 mol / L sodium hydroxide solution, let stand for 30 min, Ti3C2T x The volume ratio of the solution to the sodium hydroxide solution was 20:(5-3). The solution was washed by centrifugation with deionized water until the pH of the supernatant was less than 8. The bottom precipitate was then freeze-dried for 24 hours to obtain Ti3C2T. x Nanosheets.
[0016] Step 2: Prepare zwitterionic modified titanium carbide nanosheets, denoted as pSBMA@Ti3C2T x
[0017] pSBMA@Ti3C2T was prepared by precipitation polymerization. x Weigh Ti3C2T x The nanosheets, anhydrous ethanol, and deionized water were mixed in a mass ratio of 0.3:(32–55):(5–10) until homogeneous. The pH was adjusted to 3.5–4.5, and excess 3-(methacryloyloxy)propyltrimethoxysilane (MPS) was added dropwise to the mixture. MPS reacted with Ti3C2T... x The nanosheets were mixed at a mass ratio of (0.01045–0.03135):3. After stirring at room temperature for 48 h, the product was washed with anhydrous ethanol by centrifugation and finally dried under vacuum at 50 °C for 24 h. The resulting product was designated as MPS-Ti3C2T. x Measure acetonitrile and deionized water at a volume ratio of (70-77):(3-10) into a three-necked flask. Weigh MPS-Ti3C2T x The mass ratio of polymethacryloylethyl sulfobetaine (SBMA), ethylene glycol dimethacrylate (EDGMA), α-methacrylic acid (MAA), and azobisisobutyronitrile (AIBN) was 3:(2–6):(0.0022–0.0066):(0.0005–0.0015):(0.1–0.3), and the mixture was added to a three-necked flask and stirred until homogeneous. The mixture was heated to boiling until half of the acetonitrile was distilled off. The precipitate was washed with ethanol by centrifugation, and the final product was dried under vacuum at 40°C for 24 h to obtain pSBMA@Ti3C2T. x Nanosheets.
[0018] Step 3: Preparation of zwitterionic modified titanium carbide nanosheet filled film
[0019] This invention employs a UV crosslinking method to prepare zwitterionic modified titanium carbide nanosheet filled films. pSBMA@Ti3C2T xPolyethylene glycol methyl ether acrylate (PEGMEA), polyethylene glycol diacrylate (PEGDA), and 1-hydroxycyclohexylphenyl ketone (HCPK) were added to a beaker in a mass ratio of (0.01–0.04):(5–8):(2–5):(0.001–0.005), stirred for 1 hour, and sonicated for 1 hour to obtain a mixed dispersion. The above mixed dispersion was placed in the middle of a quartz plate and cured under ultraviolet light for 10–20 minutes to obtain a zwitterionic modified titanium carbide nanosheet filled film.
[0020] This invention provides a zwitterionic modified titanium carbide nanosheet filled membrane. The invention is based on the fact that the separation mechanism of CO2 in the membrane is mainly a dissolution-diffusion mechanism. Polyethylene oxide contains a large number of polar ether radical groups, which have a strong affinity for CO2, thereby improving the solubility selectivity of CO2 in the membrane. The zwitterionic group contains organic sulfate groups (-SO3). - This can increase the total water content in the membrane, thereby improving the solubility selectivity of CO2 in the membrane; the zwitterionic ions contain quaternary ammonium groups (-N) + (CH3)3) can promote CO2 mass transfer in the membrane and improve CO2 permeability in the membrane when water is present; nanoscale thickness pSBMA@Ti3C2T x The introduction of nanosheets reduces the mass transfer resistance of CO2 in the membrane and forms a fast channel for CO2 mass transfer, thereby improving the CO2 separation efficiency. Data from the examples show that the zwitterionic modified titanium carbide nanosheet-filled membrane provided by this invention has a maximum CO2 permeation capacity of 4953 Barrer and a maximum CO2 / N2 gas selectivity of 29, which is superior to membranes without pSBMA@Ti3C2T. x The separation and absorption of gases using a single base membrane and numerous adsorption materials. Attached Figure Description
[0021] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.
[0022] 1. Figure 1 This is a cross-sectional SEM image of the cross-linked polyethylene oxide pure membrane prepared in Comparative Example 1 of this invention.
[0023] 2. Figure 2 This is a cross-sectional SEM image of the zwitterionic modified titanium carbide nanosheet filling film prepared in Example 3 of the present invention. Detailed Implementation
[0024] The following detailed description, in conjunction with embodiments, illustrates the preparation method and application of the zwitterionic modified titanium carbide nanosheet filling film provided by the present invention. However, these descriptions should not be construed as limiting the scope of protection of the present invention.
[0025] Comparative Example 1:
[0026] 40 ml of 9 mol / L hydrochloric acid solution was added to a polytetrafluoroethylene reactor, followed by 3.2 g of lithium fluoride. The mixture was stirred for 30 min. 2 g of titanium aluminum carbide precursor was slowly added to the above solution, and the mixture was stirred at 35 °C for 24 h. The mixture was then washed 5–6 times by centrifugation with deionized water at 3500 rpm. 150 ml of deionized water was added to the precipitate, and the mixture was sonicated for 1 h in an ice bath under an inert gas atmosphere to obtain Ti3C2T. x Solution. Finally, add 25 ml of 1 mol / L sodium hydroxide solution, let stand for 30 min, centrifuge and wash with deionized water until the pH of the supernatant is less than 8, and freeze-dry the bottom precipitate for 24 h to obtain Ti3C2T. x Nanosheets.
[0027] Weigh the Ti3C2T obtained above x 0.3 g of nanosheets were placed in a glass beaker, and 50 ml of anhydrous ethanol and 10 ml of deionized water were added and stirred until homogeneous. The pH was adjusted to 3.5 using glacial acetic acid, and 1 ml of 3-(methacryloyloxy)propyltrimethoxysilane was added dropwise. After stirring at room temperature for 48 h, the product was washed three times by centrifugation with anhydrous ethanol, and finally dried under vacuum at 50 °C for 24 h. The obtained product was designated as MPS-Ti3C2T. x Measure 75 ml of acetonitrile and 5 ml of deionized water into three-necked flasks, respectively. Weigh 0.3 g of MPS-Ti3C2T into each flask. x 0.4 g of polymethacryloylethyl sulfobetaine (SBMA), 0.4 ml of ethylene glycol dimethacrylate (EDGMA), 0.1 ml of α-methacrylic acid (MAA), and 0.02 g of azobisisobutyronitrile (AIBN) were added to a three-necked flask and sonicated and stirred until homogeneous. The mixture was heated to boiling until half of the acetonitrile was distilled off. The precipitate was washed with ethanol by centrifugation, and the final product was dried under vacuum at 40 °C for 24 h to obtain pSBMA@Ti3C2T. x Nanosheets.
[0028] 1.4 g, 0.6 g, and 0.002 g of polyethylene glycol methyl ether acrylate (PEGMEA), polyethylene glycol diacrylate (PEGDA), and 1-hydroxycyclohexylphenyl ketone (HCPK) were weighed and added to a beaker, stirred for 1 h, and sonicated for 1 h to obtain a prepolymer dispersion. The dispersion was placed in the center of a quartz plate, and copper wires with a diameter of 200 μm were placed on both sides of the quartz plate to control the film thickness. The film was cured under ultraviolet light for 10 min to obtain a pure cross-linked polyethylene oxide film.
[0029] The cross-section of the cross-linked polyethylene oxide pure membrane prepared in Comparative Example 1 was characterized by SEM, and the structure is as follows: Figure 1 As shown.
[0030] The cross-linked polyethylene oxide pure membrane was tested for CO2 and N2 gas permeability using a pure gas permeameter at 25°C and a feed pressure of 0.2 MPa. The CO2 gas permeability was 435 Barrer, and the CO2 / N2 selectivity was 50.8.
[0031] Comparative Example 2
[0032] Ti3C2T x The preparation methods for the nanosheets and the membrane were the same as those in Comparative Example 1, except that 0.002 g of Ti3C2T was added to the prepolymer dispersion. x Nanoparticle powder.
[0033] The test conditions and methods were the same as those for Comparative Example 1, with CO2 gas permeability of 411 Barrer and CO2 / N2 selectivity of 53.
[0034] Comparative Example 3
[0035] Ti3C2T x The preparation methods for the nanosheets and the membrane were the same as those in Comparative Example 1, except that 0.004 g of Ti3C2T was added to the prepolymer dispersion. x Nanoparticle powder.
[0036] The test conditions and methods were the same as those for Comparative Example 1, with CO2 gas permeability of 396 Barrer and CO2 / N2 selectivity of 57.
[0037] Comparative Example 4
[0038] Ti3C2T x The preparation methods for the nanosheets and the membrane were the same as those in Comparative Example 1, except that 0.006 g of Ti3C2T was added to the prepolymer dispersion. x Nanoparticle powder.
[0039] The test conditions and methods were the same as those in Comparative Example 1, with CO2 gas permeability of 408 Barrer and CO2 / N2 selectivity of 61.
[0040] Comparative Example 5
[0041] Ti3C2T x The preparation methods for the nanosheets and the membrane were the same as those in Comparative Example 1, except that 0.008 g of Ti3C2T was added to the prepolymer dispersion. x Nanoparticle powder.
[0042] The test conditions and methods were the same as those for Comparative Example 1, with CO2 gas permeability of 380 Barrer and CO2 / N2 selectivity of 51.
[0043] Example 1:
[0044] 1.4 g, 0.6 g, and 0.002 g of polyethylene glycol methyl ether acrylate (PEGMEA), polyethylene glycol diacrylate (PEGDA), and 1-hydroxycyclohexylphenyl ketone (HCPK) were weighed and added to a beaker, stirred for 1 h, and sonicated for 1 h to obtain a prepolymer dispersion. The dispersion was placed in the center of a quartz plate, and copper wires with a diameter of 200 μm were placed on both sides of the quartz plate to control the film thickness. UV curing was performed for 10 min to obtain a pure polyethylene oxide film. The film was then immersed in deionized water for 7 days to allow for full water absorption.
[0045] The polyethylene oxide pure membrane was tested at 25°C and a feed pressure of 0.2 MPa. At 25°C, the CO2 / N2 mixed gas volume ratio was CO2:N2 = 80%:20%, the CO2 permeability coefficient was 2646 Barrer, and the selectivity was 13.
[0046] Example 2
[0047] pSBMA@Ti3C2T x The preparation of the nanosheets was the same as in Comparative Example 1, and the preparation method of the film was the same as in Example 1. The difference was that 0.002 g of pSBMA@Ti3C2T was added to the prepolymer dispersion. x Nanosheets.
[0048] The test conditions and methods were the same as in Example 1, with a CO2 permeability coefficient of 4011 Barrer and a selectivity of 21.
[0049] Example 3
[0050] pSBMA@Ti3C2T x The preparation of the nanosheets was the same as in Comparative Example 1, and the preparation method of the film was the same as in Example 1. The difference was that 0.004 g of pSBMA@Ti3C2T was added to the prepolymer dispersion. x Nanosheets.
[0051] The cross-section of the zwitterionic modified titanium carbide nanosheet-filled film prepared in Comparative Example 3 was characterized by SEM, and the structure is as follows: Figure 2 As shown, by Figure 2 It can be seen that the zwitterionic modified titanium carbide nanosheet filled film prepared in this embodiment contains pSBMA@Ti3C2T x It has a two-dimensional nanosheet structure and is uniformly distributed within the film without obvious aggregation.
[0052] The testing conditions and methods were the same as in Example 1, with a CO2 permeability coefficient of 4953 Barrer and a selectivity of 28.
[0053] Example 4
[0054] pSBMA@Ti3C2T x The preparation of the nanosheets was the same as in Comparative Example 1, and the preparation method of the film was the same as in Example 1. The difference was that 0.006 g of pSBMA@Ti3C2T was added to the prepolymer dispersion. x Nanosheets.
[0055] The testing conditions and methods were the same as in Example 1, with a CO2 permeability coefficient of 4754 Barrer and a selectivity of 27.
[0056] Example 5
[0057] pSBMA@Ti3C2T x The preparation of the nanosheets was the same as in Comparative Example 1, and the preparation method of the film was the same as in Example 1. The difference was that 0.008 g of pSBMA@Ti3C2T was added to the prepolymer dispersion. x Nanosheets.
[0058] The testing conditions and methods were the same as in Example 1, with a CO2 permeability coefficient of 4015 Barrer and a selectivity of 30.
[0059] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A zwitterionic modified titanium carbide nanosheet filled film, characterized in that, The zwitterionic modified titanium carbide nanosheet filled film consists of a base film and zwitterionic modified titanium carbide nanosheets filled in the base film. The base film is polyethylene oxide. The zwitterionic modified titanium carbide nanosheets are obtained by first reacting the hydroxyl groups of titanium carbide with a silane coupling agent to graft carbon-carbon double bonds on the surface of titanium carbide, and then coating the surface of titanium carbide with polyzwitterionic polymethacryloylethyl sulfobetaine pSBMA through a precipitation polymerization reaction.
2. The zwitterionic modified titanium carbide nanosheet filled film according to claim 1, characterized in that, The zwitterionic modified titanium carbide nanosheets have a lateral dimension of 200 nm to 500 nm.
3. The zwitterionic modified titanium carbide nanosheet filled film according to claim 1, characterized in that, In the zwitterionic modified titanium carbide nanosheet filling film, the polyethylene oxide is obtained by reacting polyethylene glycol methyl ether acrylate and polyethylene glycol diacrylate through ultraviolet crosslinking, with a mass ratio of (5-8):(2-5), and the mass ratio of zwitterionic modified titanium carbide nanosheets to polyethylene oxide is (0.001-0.008):
1.
4. The zwitterionic modified titanium carbide nanosheet filled film according to any one of claims 1-3, characterized in that, The thickness of the zwitterionic modified titanium carbide nanosheet filled film is 100–220 μm.
5. The zwitterionic modified titanium carbide nanosheet filled film according to any one of claims 1-3, characterized in that, The zwitterionic modified titanium carbide nanosheet filled membrane can be in the form of a flat sheet membrane, a hollow fiber membrane, or a tubular membrane.
6. The synthesis steps of the zwitterionic modified titanium carbide nanosheet filled film according to any one of claims 1-5 are as follows: Step 1: Prepare titanium carbide nanosheets, denoted as Ti3C2T x Ti3C2T was prepared by chemical etching of aluminum carbide (Ti3AlC2) precursor using a hydrochloric acid + lithium fluoride system. x Measure out hydrochloric acid solution and add it to the polytetrafluoroethylene reactor. Weigh out lithium fluoride and add it to the reactor. Stir to dissolve, then slowly add aluminum carbide to the above solution, wherein the mass ratio of hydrochloric acid, lithium fluoride, and aluminum carbide is (8.76–17.52):(2.6–3.8):
2. Finally, stir and react at 10–45°C for 24–48 h, wash 5–6 times with deionized water, add deionized water to the obtained precipitate, and sonicate for 1 h in an ice bath under an inert gas atmosphere to obtain Ti3C2T. x Finally, add 1 mol / L sodium hydroxide solution to the solution, let it stand for 30 min, and then add Ti3C2T. x The volume ratio of the solution to the sodium hydroxide solution was 20:(5-3). The solution was washed by centrifugation with deionized water until the pH of the supernatant was less than 8. The bottom precipitate was then freeze-dried for 24 hours to obtain Ti3C2T. x Nanosheets; Step 2: Prepare zwitterionic modified titanium carbide nanosheets, denoted as pSBMA@Ti3C2T x pSBMA@Ti3C2T was prepared by precipitation polymerization. x Weighing Ti3C2T x The nanosheets, anhydrous ethanol, and deionized water were mixed in a mass ratio of 0.3:(32–55):(5–10), and the pH was adjusted to 3.5–4.
5. An excess of 3-(methacryloyloxy)propyltrimethoxysilane (MPS) was then added dropwise to the mixture. The MPS reacted with Ti3C2T… x The nanosheets were mixed at a mass ratio of (0.01045–0.03135):
3. After stirring at room temperature for 48 h, the product was washed with anhydrous ethanol by centrifugation and finally dried under vacuum at 50 °C for 24 h. The resulting product was designated as MPS-Ti3C2T. x Measure acetonitrile and deionized water in a volume ratio of (70-77):(3-10) into a three-necked flask, and weigh MPS-Ti3C2T. x The mass ratio of polymethacryloylethyl sulfobetaine (pSBMA), ethylene glycol dimethacrylate (EDGMA), α-methacrylate (MAA), and azobisisobutyronitrile (AIBN) was 3:(2–6):(0.0022–0.0066):(0.0005–0.0015):(0.1–0.3). This mixture was added to a three-necked flask and stirred thoroughly. The mixture was heated to boiling until half of the acetonitrile evaporated. The precipitate was washed with ethanol by centrifugation. The final product was vacuum dried at 40°C for 24 hours to obtain pSBMA@Ti3C2T. x Nanosheets; Step 3: Preparation of zwitterionic modified titanium carbide nanosheet filled film Amphoteric modified titanium carbide nanosheets were prepared by ultraviolet crosslinking: pSBMA@Ti3C2T x A mixture of polyethylene glycol methyl ether acrylate (PEGMEA), polyethylene glycol diacrylate (PEGDA), and 1-hydroxycyclohexylphenyl ketone (HCPK) in a mass ratio of (0.01–0.04):(5–8):(2–5):(0.001–0.005) was added to a beaker, stirred for 1 hour, and sonicated for 1 hour to obtain a mixed dispersion. The above mixed dispersion was placed in the middle of a quartz plate and cured under ultraviolet light for 10–20 minutes to obtain a zwitterionic modified titanium carbide nanosheet filling film.
Citation Information
Patent Citations
Zwitterionic pervaporation separation membrane and preparation method thereof