A CPP film for lithium battery soft pack and preparation method thereof
By introducing specific polymer materials into the core layer and heat sealing layer of the CPP film, the problems of electrolyte corrosion resistance and slip agent migration of the lithium battery soft package are solved, and the electrolyte resistance and heat sealing layer of the aluminum plastic film are improved. The friction performance ensures the stability and consistency of the product.
Patent Information
- Application Number
- CN202310214456.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-03-07
AI Technical Summary
Existing CPP films perform poorly in terms of resistance to electrolyte corrosion and lubricant migration during long-term storage, which affects the performance and consistency of lithium battery soft packs.
It adopts a core layer composed of acid-modified polyolefin, random copolymerized propylene, block copolymerized propylene, polyolefin elastomer and alkaline polymer particles, combined with random copolymerized propylene and fluorinated acrylate resin modified polyolefin. The heat sealing layer uses alkaline polymer particles to absorb hydrofluoric acid and modified polyolefin to reduce the friction coefficient, improve electrolyte resistance and prevent slip agent migration.
It significantly improves the electrolyte resistance of the composite aluminum-plastic film, reduces the surface friction coefficient of the heat seal layer, and improves product consistency and long-term storage stability.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a CPP film for a lithium battery soft package. Background Art
[0002] As people's environmental awareness gradually improves, new energy vehicles are developing rapidly. Lithium batteries have the advantages of high energy density, long life, and high open circuit voltage, so they have become a major strategic industry that the country focuses on supporting and developing. Soft-pack lithium batteries have more advantages in lightweight and other aspects, and are the future development trend of lithium batteries. The shell of the soft-pack battery is an aluminum-plastic film, which is composed of nylon film, passivated aluminum foil, and CPP film through adhesive. As the inner layer, the CPP film is directly in contact with the electrolyte, and its performance is very important to the performance of the aluminum-plastic film. When the soft-pack lithium battery is in use, a small amount of water vapor will penetrate into the battery through the heat-sealed interface, and a small amount of water vapor will react with the electrolyte lithium hexafluorophosphate to produce hydrofluoric acid. The electrolyte is an organic solvent that has a swelling effect on the CPP film and the inner layer of glue. The hydrofluoric acid penetrates the CPP film with the electrolyte and contacts the inner adhesive layer and the aluminum foil passivation layer and corrodes them, resulting in a decrease in the peeling force.
[0003] On the other hand, the heat-sealing layer of CPP film needs to add a lubricant to ensure the low friction coefficient of the heat-sealing layer. Traditional lubricants are low-molecular-weight long-chain fatty amides or silicone resins. The disadvantage of long-chain fatty amides as lubricants is that when the aluminum-plastic film is laminated and matured (maturation temperature 50-80°C, aging time 3-7 days), the long-chain fatty amide lubricant of the heat-sealing layer migrates inward, causing the friction coefficient to increase, affecting the use of the production line and the depth of the shell punching. The poor compatibility of silicone resin and polyolefin makes it difficult to disperse evenly in the heat-sealing layer of CPP film, affecting product consistency.
[0004] The CPP films currently available on the market do not perform well in terms of resistance to electrolyte corrosion and long-term storage lubricant migration. How to solve the above two problems is one of the research directions that technicians in this field are committed to. Summary of the invention
[0005] In view of the above problems, the present invention proposes a CPP film for lithium battery soft pack and a preparation method thereof, which effectively solves the problem that the CPP film in the prior art has unsatisfactory performance in terms of resistance to electrolyte corrosion and long-term storage lubricant migration.
[0006] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: a CPP film for lithium battery soft pack, comprising an adhesive layer, a core layer and a heat-sealing layer, wherein the core layer is arranged between the adhesive layer and the heat-sealing layer and is bonded to the adhesive layer and the heat-sealing layer, wherein the adhesive layer is composed of acid-modified polyolefin and random copolymer polypropylene, the core layer is composed of block copolymer polypropylene, polyolefin elastomer and alkaline polymer particles, and the heat-sealing layer is composed of random copolymer polypropylene and fluorinated acrylate resin modified polyolefin. The introduction of alkaline polymer particles can effectively absorb the hydrofluoric acid generated by the hydrolysis of the electrolyte, thereby reducing the corrosion of the CPP film by the hydrofluoric acid. By introducing the fluorinated acrylate resin modified polyolefin as a lubricant and an opening agent in the heat-sealing layer, the long-term storage migration problem of the traditional small molecule long-chain fatty amide lubricant is effectively solved.
[0007] Furthermore, the particle size of the alkaline polymer particles is 0.3-2 um.
[0008] Furthermore, the acid-modified polyolefin in the bonding layer is one or more of maleic anhydride-grafted homopolypropylene, maleic anhydride-grafted ethylene-propylene random copolymer, maleic anhydride-grafted butene-propylene random copolymer, and maleic anhydride-grafted terpolymer random copolymer, with a melting temperature range of 90-150°C and a melt index of 1-20g / 10min.
[0009] Furthermore, the random copolymer polypropylene is one or more of ethylene-propylene random copolymer, butene-propylene random copolymer and terpolymer random copolymer, and has a melting temperature range of 110-160° C. and a melt index of 1-20 g / 10 min.
[0010] Furthermore, the block copolymer polypropylene is one or more of ethylene-propylene block copolymer, butene-propylene block copolymer and ternary block copolymer polypropylene, and has a melting temperature range of 130-170° C. and a melt index of 1-20 g / 10 min.
[0011] Furthermore, the polyolefin elastomer is one or more of ethylene-propylene random copolymer, butene-propylene random copolymer, and terpolymer random copolymer polypropylene-based elastomer, and has a melting temperature range of 80-120° C. and a melt index of 1-20 g / 10 min.
[0012] Furthermore, the thickness of the CPP film is 30-90 um, and the thickness ratio of the adhesive layer, the core layer and the heat-sealing layer is 1:3-4:1-1.5.
[0013] The present invention also describes a method for preparing a CPP film for a lithium battery soft package, wherein the adhesive layer, the core layer and the heat-sealing layer are prepared into the CPP film for a lithium battery soft package by a multi-layer co-extrusion casting process, and also includes a method for preparing alkaline polymer particles and a method for preparing fluorinated acrylate resin modified polyolefin;
[0014] The basic polymer particles include component one, component two, component three and component four;
[0015] The first component includes sodium lauryl alcohol polyoxyethylene ether sulfate, stearyl alcohol and deionized water in a ratio of 0.25-0.5:0.25-0.5:20 by mass;
[0016] The second component includes styrene, divinylbenzene, glycidyl methacrylate and deionized water in a ratio of 23-28:2:10-15:40 by mass;
[0017] The third component includes 30% pure hydrogen peroxide and deionized water in a ratio of 0.5:9.5 by mass;
[0018] The component four includes ascorbic acid and deionized water in a ratio of 0.5:9.5 by mass.
[0019] The preparation method of the basic polymer microparticles is described as follows:
[0020] Step 1: Add component 1 to the reactor and heat to 70°C, stir to completely melt and emulsify stearyl alcohol, add component 2, heat and stir to emulsify to 50°C and keep warm;
[0021] Step 2: Add component 3 and component 4 dropwise at the same speed to the reaction kettle where the reaction in step 1 is completed, and complete the addition within 3 hours. Keep warm for 1 hour, filter, and then wash with deionized water to obtain polymer microspheres;
[0022] Step 3: Add 3 parts of a xylene / acetone mixed solvent with a mass ratio of 2:1 and 1 part of polymer microspheres into the reaction kettle after the reaction in step 2 is completed and stir;
[0023] Step 4: Add an organic amine in an amount equivalent to the molar amount of the epoxy groups in the alkaline polymer particles into the reaction kettle after the reaction in step 3, and heat to 60° C. and keep warm for 4 hours;
[0024] Step 5: After the fourth step of heat preservation is completed, filter, wash the unreacted organic amine three times with a mixed solvent, and then dry at low temperature to obtain alkaline polymer particles.
[0025] The components of the fluorinated acrylate resin modified polyolefin include: component five and component six;
[0026] The component five comprises a fluorinated monomer, a glycidyl ester monomer and toluene in a mass ratio of 45:4:40, wherein the fluorinated monomer is one or more of hexafluorobutyl acrylate, dodecafluoroheptyl acrylate, tridecafluorooctyl acrylate, hexafluorobutyl methacrylate, dodecafluoroheptyl methacrylate and tridecafluorooctyl methacrylate; the glycidyl ester monomer is one or more of glycidyl methacrylate or glycidyl acrylate;
[0027] The component six includes tert-butyl peroxy-2-ethylhexanoate and toluene in a mass ratio of 1:10;
[0028] The preparation method of the fluorinated acrylate resin modified polyolefin is described as follows:
[0029] Step 1: Add component 5 into the reactor, stir and heat to 100°C, and add component 6 dropwise within 3 hours and keep warm;
[0030] Step 2: Add 50% solid EAA resin or EMA resin toluene solution to the reactor after the reaction in the first step, wherein the amount of the EAA resin or EMA resin toluene solution added is 10 times the amount of the glycidyl ester monomer mole in the EAA resin or EMA resin toluene solution, and add 1% of the mass of the EAA resin or EMA resin toluene solution DMP-30 as a catalyst, stir and keep warm for 4 hours, and then cool to room temperature;
[0031] Step 3: Add an excess of low-boiling point monohydric alcohol to the reaction solution after the second step reaction to precipitate the fluorinated acrylate resin modified polyolefin, and soak and wash it three times with the low-boiling point monohydric alcohol to remove the catalyst DMP-30, and finally dry it to obtain the fluorinated acrylate resin modified polyolefin for use.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The present invention significantly improves the electrolyte resistance of the composite aluminum-plastic film by adding alkaline polymer microspheres to the core layer of the CPP film.
[0034] The present invention adds fluorinated acrylate resin modified polyolefin to the heat seal layer of the CPP film, which can effectively reduce the surface friction coefficient of the heat seal layer and significantly improve the problem of increased friction coefficient during long-term storage caused by the migration of the lubricant.
[0035] In the present invention, the fluorinated acrylate resin modified polyolefin has good compatibility with the random copolymer polypropylene and is easy to disperse in the copolymer polypropylene, which is beneficial to the consistency of the CPP film product. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1: A CPP film for lithium battery soft pack and a preparation method thereof;
[0038] A CPP film for lithium battery soft pack: comprising an adhesive layer, a core layer and a heat-sealing layer, wherein the core layer is arranged between the adhesive layer and the heat-sealing layer and is bonded to the adhesive layer and the heat-sealing layer;
[0039] The acid-modified polyolefin in the bonding layer is Mitsui Chemicals QF551E, which has a melting temperature of 147°C, a melting index of 5.0, and a dosage of 15 parts by mass. The random copolymer polypropylene is Taiwan Formosa Plastics PP5060T, which has a melting temperature of 146°C, a melting index of 7.5g / 10min, and a dosage of 85 parts by mass.
[0040] The block copolymer polypropylene in the core layer is Korean Hanhua BI451, which has a melting temperature of 165°C, a melt index of 8g / 10min, and an amount of 93 parts by mass. The polyolefin elastomer is ExxonMobil's Vistamaxx™ 3588FL, which has a melting temperature of 103°C, a melt index of 8g / 10min, and an amount of 5 parts by mass. The amount of the basic polymer particles prepared in this example is 2 parts by mass.
[0041] The random copolymer polypropylene in the heat sealing layer is selected from Formosa Plastics PP5060T from Taiwan, China, with a melting temperature of 146° C., a melt index of 7.5 g / 10 min, and an amount of 93 parts by mass. The amount of fluorinated acrylate resin modified polyolefin prepared in this embodiment is 7 parts by mass.
[0042] The total thickness of the CPP film for lithium battery soft pack is 40um, and the thickness ratio of the adhesive layer, core layer and heat sealing layer is 1:4:1. It is prepared by a multi-layer co-extrusion casting process. The multi-layer co-extrusion casting process is a traditional film extrusion production process. It is a process for producing a multi-layer composite film by combining two or more different plastics through two or more extruders through a multi-channel composite die head. It is an existing process and will not be described here.
[0043] The components of the alkaline polymer particles include: Table 1 shows the components of the alkaline polymer particles:
[0044] Table 1
[0045]
[0046] The preparation method of the basic polymer microparticles is described as follows:
[0047] Step 1: Add component 1 to the reactor and heat to 70°C, stir to completely melt and emulsify stearyl alcohol, add component 2, heat and stir to emulsify to 50°C and keep warm;
[0048] Step 2: Add component 3 and component 4 dropwise at the same speed to the reaction kettle where the reaction in step 1 is completed, and complete the addition within 3 hours. Keep warm for 1 hour, filter, and then wash with deionized water to obtain polymer microspheres;
[0049] Step 3: Add 3 parts of a xylene / acetone mixed solvent with a mass ratio of 2:1 and 1 part of polymer microspheres into the reaction kettle after the reaction in step 2 is completed and stir;
[0050] Step 4: Add an organic amine in an amount equivalent to the molar amount of the epoxy groups in the alkaline polymer particles into the reaction kettle after the reaction in step 3, and heat to 60° C. and keep warm for 4 hours;
[0051] Step 5: After the fourth step of heat preservation is completed, filter, wash the unreacted organic amine three times with a mixed solvent, and then dry at low temperature to obtain alkaline polymer microparticles. The average particle size of the obtained alkaline polymer microparticles is 0.7 um.
[0052] Preparation of fluorinated acrylate resin modified polyolefin:
[0053] The fluorinated acrylate resin modified polyolefin is grafted with one or more combinations of acrylic acid-ethylene copolymer (EAA resin) and methacrylic acid-ethylene copolymer (EMA resin) and a fluorinated polyacrylate resin containing an epoxy functional group. In this embodiment, Dow acrylic acid-ethylene copolymer PRIMACOR3003 is selected, which has a melting temperature of 100° C. and a melt index of 7.8 g / 10 min. The components of the fluorinated acrylate resin modified polyolefin include: Table 2 shows the components of the fluorinated acrylate resin modified polyolefin:
[0054] Table 2
[0055]
[0056] The preparation method of the fluorinated acrylate resin modified polyolefin is described as follows:
[0057] Step 1: Add component 5 into the reactor, stir and heat to 100°C, and add component 6 dropwise within 3 hours and keep warm;
[0058] Step 2: Add 50% solid EAA resin or EMA resin toluene solution to the reactor after the reaction in the first step, and add 1% DMP-30 by mass of the EAA resin or EMA resin toluene solution as a catalyst, stir and keep warm for 4 hours, then cool to room temperature;
[0059] Step 3: Add an excess of low-boiling point monohydric alcohol to the reaction solution after the second step reaction to precipitate the fluorinated acrylate resin modified polyolefin, and soak and wash it three times with the low-boiling point monohydric alcohol to remove the catalyst DMP-30, and finally dry it to obtain the fluorinated acrylate resin modified polyolefin for use.
[0060] Example 2: A CPP film for lithium battery soft pack;
[0061] This embodiment describes a CPP film for lithium battery soft pack, which is different from the first embodiment in that:
[0062] The block copolymer polypropylene used in the core layer is 91.5 parts by weight of Korean Hanwha BI451, and the amount of the alkaline polymer particles prepared in Example 1 is 3.5 parts by weight.
[0063] Example 3: A CPP film for lithium battery soft pack;
[0064] This embodiment describes a CPP film for lithium battery soft pack, which is different from the first embodiment in that:
[0065] The block copolymer polypropylene used in the core layer is 90 parts by weight of Korean Hanwha BI451, and the amount of the alkaline polymer particles prepared in Example 1 is 5 parts by weight.
[0066] Comparative Example 1: A CPP film for lithium battery soft pack;
[0067] This embodiment describes a CPP film for lithium battery soft pack, which is different from the first embodiment in that:
[0068] The block copolymer polypropylene used in the core layer is 95 parts by weight of Korean Hanwha BI451, without the alkaline polymer particles prepared in Example 1.
[0069] Comparative Example 2: A CPP film for lithium battery soft pack;
[0070] This embodiment describes a CPP film for lithium battery soft pack, which is different from the first embodiment in that:
[0071] The random copolymer polypropylene in the heat-sealing layer is 98 parts by weight of Formosa Plastics PP5060T from Taiwan, China. The fluorinated acrylate resin modified polyolefin in Example 1 is replaced by a lubricant erucamide in an amount of 2 parts by weight.
[0072] Table 3 is a summary of the parameters of Examples 1-3 and Comparative Examples 1-2.
[0073] Table 3
[0074]
[0075] The CPP films prepared in the above embodiments and comparative examples were used to prepare aluminum-plastic films and the static friction coefficient of the CPP films after electrolyte resistance and aging was evaluated.
[0076] Test method for friction coefficient of aluminum-plastic film composite and CPP film heat sealing layer:
[0077] First, use polyurethane adhesive to bond 25um thick nylon film and 40um passivated aluminum foil matte surface, then coat the glossy surface of aluminum foil with inner layer adhesive, dry and bond with 40um cast polypropylene film, control the dry film thickness of adhesive to 3-5um, and put the bonded aluminum-plastic film into 80℃ oven for 3 days;
[0078] The cured aluminum-plastic film was cut into 100 mm × 15 mm sample strips to test the T-peel force between the polypropylene film and the aluminum foil;
[0079] The test strips were immersed in an electrolyte containing 1 mol / L lithium hexafluorophosphate and ethylene carbonate / dimethyl carbonate / diethyl carbonate in a ratio of 1:1:1 at a temperature of 85°C, and 2000 ppm of water was added to the electrolyte. The change trend of the T-type peel force at different immersion days was tested to characterize the electrolyte performance.
[0080] The static friction coefficient of CPP / CPP is determined by referring to the provisions of ASTM D1894. The test is carried out on a friction coefficient tester. The total weight of the slider and the sample is ensured to be 200±2g. At the same time, a sample of the same material is taken and the two surfaces are moved relative to each other at a speed of 100±10mm / min. The friction coefficient is recorded. The measurement is repeated three times and the average value is taken.
[0081] Table 4 shows the performance test results of the CPP composite aluminum-plastic films prepared in Examples 1-3 and Comparative Examples 1-2;
[0082] Table 4
[0083]
[0084] From the above table, we can get:
[0085] By comparing Example 1 with Comparative Example 1, the block copolymer polypropylene used in the core layer is 95 parts by weight of Korean Hanwha BI451, and there is no alkaline polymer microparticles prepared in Example 1. The electrolyte stripping resistance coefficient of the CPP film is significantly increased after the aluminum-plastic film is aged.
[0086] By comparing Example 1 with Comparative Example 2, the random copolymer polypropylene in the heat sealing layer is selected from Taiwan Formosa Plastics PP5060T, and its usage is 98 parts by mass. When the fluorinated acrylate resin modified polyolefin in Example 1 is replaced by the lubricant erucamide, and its usage is 2 parts by mass, the friction coefficient of the CPP film is significantly reduced before and after the aluminum-plastic film is aged.
[0087] Finally, the CPP film prepared by the present invention not only effectively improves the long-term electrolyte resistance of the composite aluminum-plastic film, but also reduces the increase in the friction coefficient of the heat-sealing layer of the CPP film after the aluminum-plastic film is matured.
[0088] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a CPP film for a lithium battery soft package, comprising a bonding layer, a core layer and a heat-sealing layer, wherein the core layer is arranged between the bonding layer and the heat-sealing layer and is bonded to the bonding layer and the heat-sealing layer, and the bonding layer, the core layer and the heat-sealing layer are prepared into a CPP film for a lithium battery soft package by a multi-layer co-extrusion casting process, characterized in that: The adhesive layer is composed of acid-modified polyolefin and random copolymer polypropylene, the core layer is composed of block copolymer polypropylene, polyolefin elastomer and alkaline polymer particles, and the heat-sealing layer is composed of random copolymer polypropylene and fluorinated acrylate resin modified polyolefin; The basic polymer particles include component one, component two, component three and component four; The first component includes sodium lauryl alcohol polyoxyethylene ether sulfate, stearyl alcohol and deionized water in a ratio of 0.25-0.5:0.25-0.5:20 by mass; The second component includes styrene, divinylbenzene, glycidyl methacrylate and deionized water in a ratio of 23-28:2:10-15:40 by mass; The third component includes 30% pure hydrogen peroxide and deionized water in a ratio of 0.5:9.5 by mass; The component 4 comprises ascorbic acid and deionized water in a ratio of 0.5:9.5 by mass; The preparation method of the basic polymer microparticles is described as follows: Step 1: Add component 1 to the reactor and heat to 70°C, stir to completely melt and emulsify stearyl alcohol, add component 2, heat and stir to emulsify to 50°C and keep warm; Step 2: Add component 3 and component 4 dropwise at the same speed to the reaction kettle where the reaction in step 1 is completed, and complete the addition within 3 hours. Keep warm for 1 hour, filter, and then wash with deionized water to obtain polymer microspheres; Step 3: Add 3 parts of a xylene / acetone mixed solvent with a mass ratio of 2:1 and 1 part of polymer microspheres into the reaction kettle after the reaction in step 2 and stir; Step 4: Add an organic amine in an amount equivalent to the molar amount of the epoxy groups in the alkaline polymer particles into the reaction kettle after the reaction in step 3, and heat to 60° C. and keep warm for 4 hours; Step 5: After the fourth step of heat preservation is completed, filter, wash the unreacted organic amine three times with a mixed solvent, and then dry at low temperature to obtain alkaline polymer particles; The components of the fluorinated acrylate resin modified polyolefin include: component five and component six; The component five comprises a fluorinated monomer, a glycidyl ester monomer and toluene in a mass ratio of 45:4:40, wherein the fluorinated monomer is one or more of hexafluorobutyl acrylate, dodecafluoroheptyl acrylate, tridecafluorooctyl acrylate, hexafluorobutyl methacrylate, dodecafluoroheptyl methacrylate and tridecafluorooctyl methacrylate; the glycidyl ester monomer is one or more of glycidyl methacrylate or glycidyl acrylate; The component six comprises tert-butyl peroxy-2-ethylhexanoate and toluene in a mass ratio of 1:10; The preparation method of the fluorinated acrylate resin modified polyolefin is described as follows: Step 1: Add component 5 into the reactor, stir and heat to 100°C, and add component 6 dropwise within 3 hours and keep warm; Step 2: Add 50% solid EAA resin or EMA resin toluene solution to the reactor after the reaction in the first step, the amount of the EAA resin or EMA resin toluene solution added is 10 times the molar amount of the carboxyl group in the EAA resin or EMA resin toluene solution to the molar amount of the glycidyl ester monomer, and add 1% DMP-30 as a catalyst based on the mass of the EAA resin or EMA resin toluene solution, stir and keep warm for 4 hours, and then cool to room temperature; Step 3: Add an excess of low-boiling point monohydric alcohol to the reaction solution after the second step reaction to precipitate the fluorinated acrylate resin modified polyolefin, and soak and wash it three times with the low-boiling point monohydric alcohol to remove the catalyst DMP-30, and finally dry it to obtain the fluorinated acrylate resin modified polyolefin for use.
2. The method for preparing a CPP film for a lithium battery soft package according to claim 1, characterized in that: The particle size of the alkaline polymer particles is 0.3-2 um.
3. The method for preparing a CPP film for a lithium battery soft package according to claim 1, characterized in that: The acid-modified polyolefin in the bonding layer is one or more of maleic anhydride-grafted homopolypropylene, maleic anhydride-grafted ethylene-propylene random copolymer, maleic anhydride-grafted butene-propylene random copolymer, and maleic anhydride-grafted terpolymer random copolymer, with a melting temperature range of 90-150°C and a melting index of 1-20g / 10min.
4. The method for preparing a CPP film for a lithium battery soft package according to claim 1, characterized in that: The random copolymer polypropylene is one or more of ethylene-propylene random copolymer, butene-propylene random copolymer and terpolymer random copolymer, and has a melting temperature range of 110-160° C. and a melting index of 1-20 g / 10 min.
5. The method for preparing a CPP film for a lithium battery soft package according to claim 1, characterized in that: The block copolymer polypropylene is one or more of ethylene-propylene block copolymer, butene-propylene block copolymer and ternary block copolymer polypropylene, and has a melting temperature range of 130-170° C. and a melting index of 1-20 g / 10 min.
6. The method for preparing a CPP film for a lithium battery soft package according to claim 1, characterized in that: The polyolefin elastomer is one or more of ethylene-propylene random copolymer, butene-propylene random copolymer and terpolymer random copolymer polypropylene-based elastomer, and has a melting temperature range of 80-120° C. and a melting index of 1-20 g / 10 min.
7. The method for preparing a CPP film for a lithium battery soft package according to claim 1, characterized in that: The thickness of the CPP film is 30-90 um, and the thickness ratio of the adhesive layer, the core layer and the heat-sealing layer is 1:3-4:1-1.5.
Citation Information
Patent Citations
Cast polypropylene film for aluminum-plastic composite film and preparation method of cast polypropylene film
CN109968762A
Aluminum-plastic composite film for lithium battery and preparation method of aluminum-plastic composite film
CN112937024A
Hardened anti-reflection flexible optical film, hardened coating liquid, anti-reflection coating liquid, preparation method and application
CN113138433A
Packing material for lithium cell and production method thereof
US20100015451A1
Packaging material for power storage device
US20180076421A1