Preparation of CeO on Hastelloy Alloy Matrix 2 Thin film method
By performing oxygen atmosphere annealing on the Hastelloy alloy base tape to form a c-axis oriented NiO film, and using radio frequency magnetron sputtering to prepare the CeO2 film, the problem of difficulty in growing the CeO2 film on the Hastelloy alloy base tape was solved, and stable, low-cost c The preparation of axially oriented CeO2 films reduces equipment requirements and lays a good foundation for the preparation of high-temperature superconducting films.
Patent Information
- Application Number
- CN202211654613.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-22
AI Technical Summary
It is difficult to directly grow a CeO2 film with c-axis orientation on the Hastelloy alloy substrate, which makes the preparation of superconducting films difficult. The existing methods require high equipment and high costs.
By annealing the Hastelloy alloy substrate in an oxygen atmosphere, a c-axis oriented NiO film is formed to improve the lattice matching between the substrate and the isolation layer. The radio frequency magnetron sputtering method is used to prepare a CeO2 film on the surface after annealing.
It significantly reduces the (111) orientation problem of CeO2 films, simplifies the process flow, reduces costs and equipment requirements, achieves stable growth of c-axis oriented CeO2 films on Hastelloy alloy substrates, and lays the foundation for the preparation of high-temperature superconducting films.
Smart Images

Figure CN116219356B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of thin film materials and high temperature superconducting materials. More specifically, the present invention relates to a method for preparing CeO on a Hastelloy alloy substrate. 2 Thin film method. Background Art
[0002] Hastelloy alloy is a general term for a series of corrosion-resistant alloys produced by Haynes International, USA. The chemical components of the alloy mainly include Ni, Cr, Mo, W, Co, Fe, P, S, etc. As a Ni-based alloy, Hastelloy alloy has excellent physical and chemical properties and is widely used in aviation, chemical industry and other fields.
[0003] With the continuous development of materials science, various types of high-temperature superconducting materials have been discovered, among which the most representative is the Tl series high-temperature superconducting material. High-temperature superconducting materials can work in the liquid nitrogen temperature zone, which greatly reduces the application cost compared to low-temperature superconducting materials. The superconducting properties exhibited by high-temperature superconducting materials can be widely used in the fields of electronics and power technology, and have great development potential. If high-temperature superconducting materials are needed to make electronic devices, a key step is to prepare high-temperature superconducting films, and the growth of the films needs to be attached to a certain substrate material. The excellent physical and chemical properties of Hastelloy alloy make it a good substrate material. Hastelloy alloy can not only be used as a carrier for superconducting films, but also as a carrier for superconducting tapes. However, since Hastelloy alloy will undergo atomic interdiffusion with superconducting film crystals under high temperature conditions, and there is a serious lattice mismatch between the two, it is impossible to directly prepare superconducting films or tapes on its surface. If it is necessary to prepare superconducting films or tapes on the surface of the Hastelloy alloy substrate, it is necessary to grow an isolation layer film on the surface of the Hastelloy alloy substrate to solve this problem. At present, CeO is usually used. 2 As an isolation layer material, CeO is grown directly on the Hastelloy alloy substrate. 2 The obtained films are mostly (111) oriented, and it is difficult to prepare (00l) oriented (a series of crystal planes oriented along the c-axis, such as 002, 004, 006, etc.) CeO 2 If you need to obtain high-quality superconducting films, CeO 2 The film must have a good (00l) orientation, so that the out-of-plane texture of the superconducting film can be accurately induced. To address this problem, a rolling-assisted biaxially textured substrate (RABiTS) method was proposed, which can obtain a flexible substrate with a strong cubic texture and small-angle grain boundaries, which can make CeO 2Preferred orientation growth of thin films. However, this technology has high requirements for experimental equipment and the processing cost is also high, which is not easy to implement in laboratories with insufficient conditions. Summary of the invention
[0004] An object of the present invention is to solve at least the above problems and to provide at least the advantages which will be described hereinafter.
[0005] One object of the present invention is to provide a method for preparing CeO on a Hastelloy alloy substrate. 2 The method comprises the following steps: pre-treating a Hastelloy alloy substrate to form a metal oxide film mainly composed of NiO on its surface, and preparing a CeO film having a c-axis orientation. 2 The film has a positive promoting effect.
[0006] In order to achieve these objects and other advantages of the present invention, a method for preparing CeO on a Hastelloy alloy substrate is provided. 2 The method comprises the following steps: annealing the Hastelloy alloy substrate in an oxygen atmosphere; and then preparing CeO on the surface of the annealed Hastelloy alloy substrate. 2 film.
[0007] After annealing pretreatment, the Hastelloy alloy substrate can form a c-axis oriented NiO film on its surface. This film improves the lattice matching problem between the substrate and the isolation layer and can better induce CeO 2 The isolation layer is grown in a c-axis orientation.
[0008] Preferably, the cut and cleaned Hastelloy alloy base strip is placed in a heating device, and O is poured into the heating device. 2 , annealing treatment is performed in an oxygen atmosphere.
[0009] Preferably, 1 atm high purity O is poured into the heating device. 2 .
[0010] Preferably, the annealing treatment conditions are: heating rate of 0.7-55°C / s, heating to 850-900°C, keeping constant temperature for 5-30 minutes, and then naturally cooling to room temperature.
[0011] Preferably, CeO is prepared on the surface of the annealed Hastelloy alloy substrate by radio frequency magnetron sputtering. 2 film.
[0012] Preferably, CeO 2 The sputtering target is loaded into a magnetron sputtering instrument and high-purity Ar or Ar, O 2The mixture is used as the sputtering atmosphere; during the sputtering process, the sputtering pressure is controlled at 0.5-2Pa, the sputtering temperature is controlled at 650-700℃, and the sputtering power is controlled at 80-120W. The CeO 2 The thickness of the film.
[0013] Preferably, CeO 2 Preparation method of sputtering target is CeO 2 The powder was pressed by a tablet press and placed in a tubular sintering furnace. 2 , keep the temperature at 1050℃ for 30h. After the constant temperature is over, wait for it to cool naturally.
[0014] Preferably, the prepared CeO 2 The film thickness is 50-500nm.
[0015] The present invention has at least the following beneficial effects:
[0016] First, the method of the present invention pre-treats the Hastelloy alloy substrate to improve its surface environment, thereby creating a suitable CeO 2 The conditions for the preferred orientation of the film solve the problem of CeO grown by previous methods. 2 The problem is that most films are (111) oriented. Compared with other pretreatment methods, it significantly reduces the cost and difficulty.
[0017] Second, the method of the present invention is relatively simple in process and highly operable, and can easily grow c-axis oriented CeO on the surface of the Hastelloy alloy substrate. 2 Films and prepared CeO 2 The film effect is stable and very suitable for large-scale application.
[0018] Third, the method of the present invention has low requirements on equipment and does not need to grow multiple isolation layers on the Hastelloy alloy substrate, which effectively reduces the preparation cost and lays a good foundation for the subsequent growth of high-temperature superconducting thin films on its surface.
[0019] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The CeO prepared in Example 1 of the present invention 2 Film, image obtained by XRD θ-2θ scanning;
[0021] Figure 2 The CeO prepared in Example 2 of the present invention 2The film is subjected to XRD θ-2θ scanning to obtain an image;
[0022] Figure 3 The CeO prepared in Example 3 of the present invention 2 The film is subjected to XRD θ-2θ scanning to obtain an image;
[0023] Figure 4 The CeO prepared in Comparative Example 1 of the present invention 2 The film is subjected to XRD θ-2θ scanning to obtain an image;
[0024] Figure 5 The CeO prepared in Comparative Example 2 of the present invention 2 The film is subjected to XRD θ-2θ scanning to obtain an image;
[0025] Figure 6 The CeO prepared in Comparative Example 3 of the present invention 2 The film is subjected to XRD θ-2θ scanning to obtain an image;
[0026] Figure 7 The CeO prepared in Comparative Example 4 of the present invention 2 The film is subjected to XRD θ-2θ scanning to obtain an image;
[0027] Figure 8 The CeO prepared in Comparative Example 5 of the present invention 2 The film is subjected to XRD θ-2θ scanning to obtain an image;
[0028] Fig. 9 The CeO prepared in Comparative Example 6 of the present invention 2 The film is subjected to XRD θ-2θ scanning to obtain an image;
[0029] Fig.10 CeO prepared on the unannealed Hastelloy alloy substrate 2 The film is subjected to XRD θ-2θ scanning to obtain an image;
[0030] Fig.11 This is the Ni2p spectrum of the surface of the Hastelloy alloy substrate without annealing treatment;
[0031] Fig.12 This is the Ni2p spectrum of the surface of the Hastelloy alloy substrate treated under the annealing conditions of Comparative Example 9;
[0032] Fig.13 This is the Ni2p spectrum of the surface of the Hastelloy alloy substrate treated under the annealing conditions of Comparative Example 10;
[0033] Fig.14 This is the Ni2p spectrum of the surface of the Hastelloy alloy substrate treated under the annealing conditions of Comparative Example 11;
[0034] Fig.15 The Hastelloy alloy substrate treated in Comparative Example 12 was subjected to XRD θ-2θ scanning to obtain an image;
[0035] Fig.16 The CeO prepared in Example 1 of the present invention 2 Thin film, CeO under SEM observation 2 Surface morphology of the film, obtained image. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0037] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0038] It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial channels unless otherwise specified.
[0039] A method for preparing CeO on Hastelloy alloy substrate 2 The method comprises the following steps: annealing the Hastelloy alloy substrate in an oxygen atmosphere; and then preparing CeO on the surface of the annealed Hastelloy alloy substrate. 2 film.
[0040] After annealing pretreatment, the Hastelloy alloy substrate can form a c-axis oriented NiO film on its surface. This film improves the lattice matching problem between the substrate and the isolation layer and can better induce CeO 2 The isolation layer is grown in a c-axis orientation.
[0041] In one technical solution, the cut and cleaned Hastelloy alloy base strip is placed in a heating device, and O is poured into the heating device. 2 , and annealing treatment is performed in an oxygen atmosphere. The heating device can be a rapid heating sintering furnace, or other high-temperature heating devices, such as a muffle furnace.
[0042] In one technical solution, 1 atm high-purity O 2 .
[0043] In one technical solution, the annealing treatment conditions are: heating rate of 0.7-55°C / s, heating to 850-900°C, keeping constant temperature for 5-30 minutes, and then naturally cooling to room temperature.
[0044] In one technical solution, CeO is prepared on the surface of the annealed Hastelloy alloy substrate by using a radio frequency magnetron sputtering method. 2 film.
[0045] In one technical solution, CeO 2 The sputtering target is loaded into a magnetron sputtering instrument and high-purity Ar or Ar, O 2 The mixture is used as the sputtering atmosphere; during the sputtering process, the sputtering pressure is controlled at 0.5-2Pa, the sputtering temperature is controlled at 650-700℃, and the sputtering power is controlled at 80-120W. The CeO 2 The thickness of the film.
[0046] In one technical solution, CeO 2 Preparation method of sputtering target is CeO 2 The powder was pressed by a tablet press and placed in a tubular sintering furnace. 2 , keep the temperature at 1050℃ for 30h. After the constant temperature is over, wait for it to cool naturally.
[0047] In one technical solution, the prepared CeO 2 The film thickness is 50-500nm.
[0048] <Example 1>
[0049] A method for preparing CeO on Hastelloy alloy substrate 2 The method of the thin film comprises the following steps:
[0050] Step 1: Place the cut and cleaned Hastelloy alloy substrate into a rapid heating sintering furnace and pour 1atm high-purity O into the furnace. 2 ; Adjust the heating rate to 0.7°C / s to raise the temperature from room temperature to 850°C, keep the temperature constant at this temperature for 10 minutes, wait for the temperature in the furnace to drop to room temperature after the constant temperature is completed, and take out the Hastelloy alloy substrate;
[0051] Step 2: Take an appropriate amount of high-purity CeO 2 The powder is pressed by a tablet press and placed in a tubular sintering furnace, and a flowing O 2 In this environment, the temperature was kept constant at 1050℃ for 30h; after the constant temperature was completed, it was allowed to cool naturally to obtain CeO 2 Sputtering targets;
[0052] Step 3: Prepare CeO on the surface of the annealed Hastelloy alloy substrate by using RF magnetron sputtering method 2 Film; wherein CeO 2 The sputtering target was loaded into a magnetron sputtering instrument, and high-purity Ar was used as the sputtering atmosphere. During the sputtering process, the sputtering gas pressure was controlled at 0.5 Pa, the sputtering temperature was controlled at 650° C., the sputtering power was controlled at 80 W, and the sputtering time was controlled at 30 min.
[0053] <Example 2>
[0054] A method for preparing CeO on Hastelloy alloy substrate 2 The method of the thin film comprises the following steps:
[0055] Step 1: Place the cut and cleaned Hastelloy alloy substrate into a rapid heating sintering furnace and pour 1atm high-purity O into the furnace. 2 ; Adjust the heating rate to 55°C / s to raise the temperature from room temperature to 900°C, keep the temperature constant for 5 minutes, wait for the temperature in the furnace to drop to room temperature after the constant temperature is completed, and take out the Hastelloy alloy substrate;
[0056] Step 2: Take an appropriate amount of high-purity CeO 2 The powder is pressed by a tablet press and placed in a tubular sintering furnace, and a flowing O 2 In this environment, the temperature was kept constant at 1050℃ for 30h; after the constant temperature was completed, it was allowed to cool naturally to obtain CeO 2 Sputtering targets;
[0057] Step 3: Prepare CeO on the surface of the annealed Hastelloy alloy substrate by using RF magnetron sputtering method 2 Film; wherein CeO 2 The sputtering target was loaded into a magnetron sputtering apparatus, and high-purity Ar was used as the sputtering atmosphere. During the sputtering process, the sputtering gas pressure was controlled at 2 Pa, the sputtering temperature was controlled at 700° C., the sputtering power was controlled at 120 W, and the sputtering time was controlled at 30 min.
[0058] <Example 3>
[0059] A method for preparing CeO on Hastelloy alloy substrate 2 The method of the thin film comprises the following steps:
[0060] Step 1: Place the cut and cleaned Hastelloy alloy substrate into a rapid heating sintering furnace and pour 1atm high-purity O into the furnace. 2; Adjust the heating rate to 25°C / s to raise the temperature from room temperature to 875°C, keep the temperature constant for 30 minutes, wait for the temperature in the furnace to drop to room temperature after the constant temperature is completed, and take out the Hastelloy alloy substrate;
[0061] Step 2: Take an appropriate amount of high-purity CeO 2 The powder is pressed by a tablet press and placed in a tubular sintering furnace, and a flowing O 2 In this environment, the temperature was kept constant at 1050℃ for 30h; after the constant temperature was completed, it was allowed to cool naturally to obtain CeO 2 Sputtering targets;
[0062] Step 3: Prepare CeO on the surface of the annealed Hastelloy alloy substrate by using RF magnetron sputtering method 2 Film; wherein CeO 2 The sputtering target was loaded into a magnetron sputtering instrument, and high-purity Ar was used as the sputtering atmosphere. During the sputtering process, the sputtering gas pressure was controlled at 1 Pa, the sputtering temperature was controlled at 680° C., the sputtering power was controlled at 100 W, and the sputtering time was controlled at 30 min.
[0063] In the present invention, Ar, O 2 Similar results can be obtained by using a mixture of as the sputtering atmosphere.
[0064] In the present invention, CeO can also be prepared on the surface of the annealed Hastelloy alloy substrate by laser pulse deposition, sol-gel method, etc. 2 Thin films can also obtain similar results.
[0065] <Effect Test>
[0066] 1. CeO 2 Crystallization of thin films
[0067] Measurement Example 1 Preparation of CeO 2 The crystallization of the film, such as Figure 1 As shown, it shows that the CeO prepared under the conditions described in Example 1 2 The film has a relatively pure (00l) orientation, that is, c-axis orientation.
[0068] Measurement Example 2 Preparation of CeO 2 The crystallization of the film, such as Figure 2 As shown, it shows that the CeO prepared under the conditions described in Example 2 2 The film has a relatively pure (00l) orientation.
[0069] Measurement Example 3 Preparation of CeO 2 The crystallization of the film, such as Figure 3As shown, it shows that the CeO prepared under the conditions described in Example 3 2 The film has a relatively pure (00l) orientation.
[0070] 2. Effects of different conditions on CeO 2 Effect of film crystallization
[0071] Comparative Example 1: The preparation method of Example 1 was adopted, except that the temperature was raised to 700°C and kept constant.
[0072] Comparative Example 2: The preparation method of Example 2 was adopted, except that the constant temperature time was 40 minutes.
[0073] Comparative Example 3: The preparation method of Example 2 was adopted, except that the constant temperature time was 2 minutes.
[0074] Comparative Example 4: The preparation method of Example 3 was adopted, except that the sputtering temperature was 550°C.
[0075] Comparative Example 5: The preparation method of Example 3 was adopted, except that the sputtering gas pressure was 3Pa.
[0076] Comparative Example 6: The preparation method of Example 3 was adopted, except that the sputtering power was 50W.
[0077] Comparative Example 7: The preparation method of Example 3 was adopted, except that the Hastelloy alloy was not annealed.
[0078] Measurement of Comparative Example 1 Preparation of CeO 2 The crystallization of the film, such as Figure 4 The results show that after the heating temperature is changed, the subsequent prepared CeO 2 The film is not purely c-axis oriented, and there are many (111) oriented grains. This is because the insufficient annealing temperature may cause the failure to form a continuous metal oxide film on the surface of the Hastelloy alloy substrate, thus failing to form CeO 2 The film provides a good growth environment.
[0079] Measurement of Comparative Example 2 Preparation of CeO 2 The crystallization of the film, such as Figure 5 The results show that the extended constant temperature time will increase the subsequent preparation of CeO 2 The film is not purely c-axis oriented, and there are many (111) oriented grains. This is because too long annealing time may cause other complex chemical reactions to continue on the surface of the Hastelloy alloy substrate after oxidation, which destroys the suitable CeO 2 Metal oxide environments for thin film growth.
[0080] Measurement of Comparative Example 3 Preparation of CeO 2 The crystallization of the film, such as Figure 6 The results show that shortening the constant temperature time can improve the quality of the CeO prepared later. 2 The film is not purely c-axis oriented, and there are many (111) oriented grains. This is because the insufficient annealing time may result in the failure to form a continuous metal oxide film on the surface of the Hastelloy alloy substrate, thus failing to form CeO 2 The film provides a good growth environment.
[0081] Measurement of Comparative Example 4 Preparation of CeO 2 The crystallization of the film, such as Figure 7 The results show that the prepared CeO 2 The film does not have pure c-axis orientation, but rather has a relatively large (111) orientation component.
[0082] Measurement of Comparative Example 5 Preparation of CeO 2 The crystallization of the film, such as Figure 8 The results show that the growth of CeO 2 The film does not have pure c-axis orientation, but rather has a relatively large (111) orientation component.
[0083] Measurement of Comparative Example 6 Preparation of CeO 2 The crystallization of the film, such as Fig. 9 The results show that the prepared CeO 2 The film does not have pure c-axis orientation, but rather has a relatively large (111) orientation component.
[0084] Measurement of CeO prepared in Comparative Example 7 2 The crystallization of the film, such as Fig.10 The results show that the Hastelloy alloy substrate is not annealed, and the prepared CeO 2 The film does not have pure c-axis orientation, but rather has a relatively large (111) orientation component.
[0085] 3. Effect of annealing on the surface of Hastelloy alloy substrate
[0086] Comparative Example 8: XPS scanning of the Hastelloy alloy substrate that has not been annealed, the Ni2p spectrum on the surface of the Hastelloy alloy substrate, as shown in FIG. Fig.11 shown.
[0087] Comparative Example 9: The cut and cleaned Hastelloy alloy substrate was placed in a rapid heating sintering furnace, and 1 atm high purity O was poured into the furnace. 2; The heating rate was adjusted to 0.7°C / s to raise the temperature from room temperature to 850°C, and the temperature was kept constant at this temperature for 5 minutes. After the constant temperature was completed, the temperature in the furnace was lowered to room temperature, the Hastelloy alloy substrate was taken out, and XPS scanning was performed. The Ni2p spectrum on the surface of the Hastelloy alloy substrate was as follows: Fig.12 shown.
[0088] Comparative Example 10: The cut and cleaned Hastelloy alloy substrate was placed in a rapid heating sintering furnace, and 1 atm high purity O was poured into the furnace. 2 ; The heating rate was adjusted to 55°C / s to raise the temperature from room temperature to 850°C, and the temperature was kept constant at this temperature for 5 minutes. After the constant temperature was completed, the temperature in the furnace was lowered to room temperature, the Hastelloy alloy substrate was taken out, and XPS scanning was performed. The Ni2p spectrum on the surface of the Hastelloy alloy substrate was as follows: Fig.13 shown.
[0089] Comparative Example 11: The cut and cleaned Hastelloy alloy substrate was placed in a rapid heating sintering furnace, and 1 atm high purity O was poured into the furnace. 2 ; The heating rate was adjusted to 55°C / s to raise the temperature from room temperature to 900°C, and the temperature was kept constant at this temperature for 10 minutes. After the constant temperature was completed, the temperature in the furnace was lowered to room temperature, the Hastelloy alloy substrate was taken out, and XPS scanning was performed. The Ni2p spectrum on the surface of the Hastelloy alloy substrate was as follows: Fig.14 shown.
[0090] Comparative Example 12: The cut and cleaned Hastelloy alloy substrate was placed in a rapid heating sintering furnace, and 1 atm high purity O was poured into the furnace. 2 ; Adjust the heating rate to 55℃ / s to raise the temperature from room temperature to 850℃, keep the temperature constant at this temperature for 10 minutes, wait for the temperature in the furnace to drop to room temperature after the constant temperature, take out the Hastelloy alloy substrate, and perform XRD θ-2θ scanning on it. The image obtained is as follows Fig.15 shown.
[0091] From the above results, it can be seen that after the Hastelloy alloy substrate is annealed under appropriate conditions, a layer of c-axis oriented NiO-based metal oxide can be formed on its surface, which is CeO 2 A favorable environment for the film to grow in a pure c-axis orientation.
[0092] CeO prepared in Example 1 of the present invention 2 The surface of the film was observed using SEM. Fig.16 shown.
[0093] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. Preparation of CeO on Hastelloy Alloy Substrate 2 Thin film method, It is characterized in that The Hastelloy alloy substrate is annealed in an oxygen atmosphere; then CeO is prepared on the surface of the annealed Hastelloy alloy substrate. 2 film; The cut and cleaned Hastelloy alloy base strip is placed in a heating device, and O is poured into the heating device. 2 , annealing treatment is performed in an oxygen atmosphere; Fill the heating device with 1atm high-purity O 2 ; The annealing treatment conditions are: heating rate of 0.7-55°C / s, heating to 850-900°C, keeping constant temperature for 5-30 minutes, and then naturally cooling to room temperature.
2. The method for preparing CeO on a Hastelloy alloy substrate according to claim 1 2 Thin film method, It is characterized in that CeO was prepared on the surface of annealed Hastelloy alloy substrate by radio frequency magnetron sputtering. 2 film.
3. The method for preparing CeO on a Hastelloy alloy substrate according to claim 2 2 Thin film method, It is characterized in that CeO 2 The sputtering target is loaded into a magnetron sputtering instrument and high-purity Ar or Ar, O 2 The mixture acts as a sputtering atmosphere; During the sputtering process, the sputtering pressure was controlled at 0.5-2Pa, the sputtering temperature was controlled at 650-700℃, and the sputtering power was controlled at 80-120W. The CeO 2 The thickness of the film.
4. The method for preparing CeO on a Hastelloy alloy substrate according to claim 3 2 Thin film method, It is characterized in that CeO 2 Preparation method of sputtering target is CeO 2 The powder was pressed by a tablet press and placed in a tubular sintering furnace. 2 , keep the temperature at 1050℃ for 30h. After the constant temperature is over, wait for it to cool naturally.
5. The method for preparing CeO on a Hastelloy alloy substrate according to claim 1 2 Thin film method, It is characterized in that Preparation of CeO 2 The film thickness is 50-500nm.