membrane
By using specific compound compositions and crosslinking methods in bipolar films, the film structure with high crosslink density is solved, and the existing films have been solved in terms of penetration selectivity, resistance and mechanical strength, and the extreme pH is achieved Stability and fast and cheap production under conditions.
Patent Information
- Application Number
- CN202180064852.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2021-09-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-09-27
AI Technical Summary
The existing bipolar membranes have shortcomings in permeability, resistance and mechanical strength, and are difficult to maintain stability under extreme pH conditions, and are complex in production processes and costly.
Prepared by a specific compound composition curing method using a membrane containing anion exchange layer (AEL) and a cation exchange layer (CEL), using a -SO2X group to convert it into anionic group, combining non-polar compounds and ethylenically unsaturated Groups form film structures with high crosslink density, increasing mechanical strength and reducing swelling.
High permeability selectivity, low resistance and good mechanical strength are achieved, and good durability in acidic and alkaline media, allowing for rapid and inexpensive production of bipolar films.
Smart Images

Figure CN116234835B_ABST
Abstract
Description
[0001] The present invention relates to membranes (including bipolar membranes) and methods for their preparation and use.
[0002] Ion exchange membranes are used in electrodialysis, reverse electrodialysis, electrolysis, diffusion dialysis and many other processes. Typically, the transport of ions through a membrane occurs under the influence of a driving force, such as an ion concentration gradient or an electrical potential gradient.
[0003] Ion exchange membranes are generally classified according to their primary charge as cation exchange membranes (CEMs) or anion exchange membranes (AEMs). Cation exchange membranes contain negatively charged groups that allow cations to pass but repel anions, while anion exchange membranes contain positively charged groups that allow anions to pass but repel cations. Bipolar membranes (BPMs) have a cation layer and an anion layer.
[0004] Some bipolar membranes contain a porous support that provides mechanical strength. Such membranes are often referred to as "composite bipolar membranes" due to the presence of anionic and cationic polymers that discriminate between ions and the porous support that provides mechanical strength.
[0005] It is desirable to provide bipolar membranes with improved properties, such as high permselectivity, low electrical resistance, good mechanical strength, and stability at extreme pH. Ideally, such bipolar membranes could be produced rapidly, efficiently, and inexpensively.
[0006] According to a first aspect of the present invention, there is provided a membrane comprising an anion exchange layer (AEL) and a cation exchange layer (CEL), wherein the CEL is obtainable by a process comprising curing a curable composition comprising a compound of formula (I):
[0007]
[0008] in:
[0009] X is the formula -OC n H 2n+1 or -OC q H 2q-1 , wherein the value of n is 1 to 6, the value of q is 5 or 6; and the value of m is 1 or 2.
[0010] In this document (including the claims thereof), the verb "to comprise" and its conjugations are used in its non-limiting sense, meaning that the items following the word are included, but items not specifically mentioned are not excluded. In addition, an element referred to by the indefinite article "a" or "an" does not exclude the possibility that more than one element is present, unless the context clearly requires that there is one and only one element. Therefore, the indefinite article "a" or "an" generally means "at least one". The composition used to form an AEL is generally abbreviated herein as an "AEL composition". Similarly, the composition used to form a layer as a CEL is generally abbreviated herein as a "CEL composition".
[0011] The -SO2X group shown in formula (I) can be converted into an anionic group and can therefore be used to provide an anionic group to CEL.
[0012] The -SO2X group in formula (I) wherein X is as defined above is preferred over the group wherein X is Cl or OSO2R wherein R is C 1-6- Alkyl or C 6-12- aryl) because of their lower reactivity with nucleophiles. Therefore, compounds of formula (I) wherein X is as defined above are more favorable than compounds wherein X is Cl or OSO2R (where R is C 1-6- Alkyl or C 6-12- The corresponding compounds with aryl groups have better stability.
[0013] Compounds of formula (I) are known and many such compounds are commercially available.
[0014] In a preferred embodiment, m has a value of 1 or 2, and n has a value of 2 (ie, X is ethoxy) or q has a value of 6 (ie, X is cyclohexyloxy).
[0015] Component (a) is preferably highly miscible with non-polar compounds such as uncharged aromatic molecules, for example with divinylbenzene.
[0016] Examples of compounds of formula (I) include the following:
[0017]
[0018] Where R is –OC n H 2n+1 or –OC q H 2q-1 , wherein n has a value of 1 to 6 and q has a value of 5 or 6, for example methoxy, ethoxy, propoxy, tert-butoxy or cyclohexyloxy.
[0019] The curable composition from which CEL can be obtained (i.e., "CEL composition") preferably comprises the following ingredients:
[0020] (a) a compound of formula (I) (as defined above);
[0021] optional (b) a compound comprising at least two ethylenically unsaturated groups;
[0022] optionally (c) a non-aqueous solvent;
[0023] optionally (d) a free radical initiator; and
[0024] Optional (e) anionic monomers containing one and only one ethylenically unsaturated group.
[0025] Preferably, the CEL composition comprises component (b) and / or component (c).
[0026] Preferably, the CEL composition comprises at least one, more preferably at least two, especially at least three, more especially all four of components (b), (c), (d) and (e) (as defined above).
[0027] Preferably, the CEL composition comprises:
[0028] (a) 20 to 88 wt % of component (a);
[0029] (b) 10 to 60 wt % of component (b);
[0030] (c) 0 to 30 wt % of component (c);
[0031] (d) 0 to 2 wt % of component (d); and
[0032] (e) 0 to 15 wt % of component (e).
[0033] Preferred embodiments of compounds of formula (I) for use as component (a) in the CEL composition are as described above in relation to the first aspect of the invention.
[0034] Preferably, the CEL composition comprises 20 to 88 wt%, more preferably 30 to 80 wt%, most preferably 40 to 75 wt% of component (a).
[0035] Component (b) generally acts as a crosslinking agent and can provide the CEL layer with a desirably high crosslink density. A high crosslink density is preferred to limit swelling of the bipolar membrane in an aqueous environment.
[0036] Preferably, component (b) comprises an aromatic group, such as a phenyl or phenylene group (such as can be found in styrene).
[0037] Preferred ethylenically unsaturated groups include (meth)acrylic groups and / or vinyl groups (eg, vinyl ether groups, aromatic vinyl compounds, N-vinyl compounds, and allyl groups).
[0038] Examples of suitable (meth)acrylic acid groups include acrylate (H2C=CHCO-) groups, acrylamide (H2C=CHCONH-) groups, methacrylate (H2C=C(CH3)CO-) groups, and methacrylamide (H2C=C(CH3)CONH-) groups. Acrylic acid groups are preferred over methacrylic acid groups because acrylic acid groups are more reactive.
[0039] Preferred ethylenically unsaturated groups do not contain ester groups, as this can improve the stability and pH tolerance of the resulting composition. Ethylenically unsaturated groups that do not contain ester groups include vinyl groups.
[0040] As examples of compounds which can be used as component (b), the following may be mentioned:
[0041]
[0042] The above-mentioned materials useful as component (b) are available from commercial sources, for example, from Sigma-Aldrich.
[0043] It is particularly preferred that component (b) is or comprises divinylbenzene, since this compound is widely available (usually as a mixture of isomers) at low cost.
[0044] Preferably, the CEL composition comprises 10 to 60 wt%, more preferably 20 to 60 wt%, most preferably 20 to 55 wt% of component (b).
[0045] The molar ratio of component (a) to component (b) is preferably in the range of 3:1 to 1:2, more preferably 2:1 to 1:2, in particular 2:1 to 1:1, respectively.
[0046] Component (c) is preferably inert, ie, incapable of reacting with any other components of the CEL composition.
[0047] Preferably, component (c) is miscible with the other compounds of the CEL composition. Thus, component (c) can be used to dilute the other components of the CEL composition to provide a low viscosity CEL composition suitable for use in coating machines and equipment.
[0048] As examples of non-aqueous solvents that can be used as component (c) of the CEL composition, there can be mentioned alcohol solvents, ether solvents, amide solvents, ketone solvents, sulfoxide solvents, sulfone solvents, nitrile solvents and organic phosphorus solvents. Examples of alcohol solvents that can be used as or for component (c) include methanol, ethanol, isopropanol, n-butanol, ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol and a mixture comprising two or more thereof. In addition, preferred inert organic solvents that can be used for component (c) include dimethyl sulfoxide, dimethylimidazolidinone, sulfolane, N-methylpyrrolidone, dimethylformamide, acetonitrile, acetone, 1,4-dioxane, 1,3-dioxolane, tetramethylurea, hexamethylphosphoramide, hexamethylphosphoric triamide, pyridine, propionitrile, butanone, cyclohexanone, tetrahydrofuran, tetrahydropyran, 2-methyltetrahydrofuran, ethylene glycol diacetate, cyclopentyl methyl ether, methyl ethyl ketone, ethyl acetate, γ-butyrolactone, and mixtures containing two or more thereof. Preferred are dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylimidazolidinone, sulfolane, acetone, cyclopentyl methyl ether, methyl ethyl ketone, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, and mixtures containing two or more thereof.
[0049] Other examples of component (c) of the CEL composition include nonpolar aprotic solvents such as toluene, xylene, chloroform, dichloromethane, pyrrole, N-methylpyrrole, pyridine, pyrazine, and mixtures comprising two or more thereof.
[0050] Preferably, the CEL composition contains a small amount of component (c) so that a dense CEL can be prepared. If a large amount of component (c) is present in the CEL composition during curing, a membrane (or CEL) having an open structure may be formed in which component (c) fills the open space. After drying, such an open structure tends to swell in an aqueous environment, resulting in a decrease in permselectivity, which is undesirable.
[0051] Preferably, the CEL composition comprises 0 to 30 wt % of component (c), more preferably 4 to 20 wt %, especially 2 to 15 wt % of component (c).
[0052] Component (d) of the CEL composition is preferably or comprises a thermal initiator, a photoinitiator or a combination thereof. Most preferably, component (d) is or comprises a thermal initiator.
[0053] Examples of thermal initiators include: 2,2'-azobis(2-methylpropionitrile) (AIBN), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide, 1-[(1-cyano-1-methylethyl)azo]formamide, 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis(2-methylpropionamidine)dicarboxamide. hydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(1-imino-1-pyrrolidinyl-2-ethylpropane) dihydrochloride, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide} and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide].
[0054] Preferably, the CEL composition contains no component (d) or 0.001 to 2 wt%, more preferably 0.2 to 1 wt% of component (d). Component (d) is not required when the CEL composition is to be cured by electron beam (EB) or gamma irradiation.
[0055] Optionally, the CEL composition further comprises a small amount of component (e). Component (e) can be used to provide a small degree of hydrophilicity to the CEL, which helps to accelerate the hydrolysis process.
[0056] Examples of anionic monomers containing one and only one ethylenically unsaturated group which can be used as component (e) include sulfonated styrene in the form of a free acid or a salt, in particular a lithium salt, a sodium salt or a mixed salt of lithium and sodium.
[0057] Preferably, the CEL composition comprises from 0 to 15 wt%, more preferably less than 15 wt% of component (e).
[0058] In one embodiment, the CEL composition and / or the AEL composition comprises at least 60 wt % of a curable compound.
[0059] Preferably, the membrane of the present invention comprises a porous support. The porous support may be contained in the CEL, in the AEL, at the interface between the AEL and the CEL, or in two or more of the above positions. More than one porous support may also be provided at each position.
[0060] As the example of porous carrier, weaving and nonwoven synthetic fabrics and extruded films can be mentioned.Example includes wet-laid and dry-laid nonwoven materials, spunbond and melt-blown fabrics and nanofiber webs made of, for example, polyethylene, polypropylene, polyacrylonitrile, polyvinyl chloride, polyphenylene sulfide, polyester, polyamide, polyaryletherketone (for example, polyetheretherketone) and copolymers thereof.Porous carrier can also be porous membrane, for example, polysulfone, polyethersulfone, polyphenylene sulfone, polyphenylene sulfone, polyimide, polyetherimide (polyethermide), polyamide, polyamideimide, polyacrylonitrile, polycarbonate, polyacrylate, cellulose acetate, polypropylene, poly (4-methyl 1-pentene), polyvinylidene fluoride, polytetrafluoroethylene, polyhexafluoropropylene and polychlorotrifluoroethylene film and derivatives thereof.
[0061] The average thickness of the porous support is preferably from 10 to 200 μm, more preferably from 20 to 150 μm.
[0062] Preferably, the porous support has a porosity of 30% to 95%. The porosity of the support can be measured by a porometer such as the Porolux from IB-FT GmbH, Germany. TM 1000 determinations.
[0063] The porous support (if present) may be treated to modify its surface energy, for example to a value above 45 mN / m, preferably above 55 mN / m. Suitable treatments include corona discharge treatment, plasma glow discharge treatment, flame treatment, UV irradiation treatment or chemical treatment, for example to improve the wettability of the porous support and the adhesion to the porous support.
[0064] Commercially available porous supports are available from a number of sources, for example from Freudenberg Filtration Technologies (Novatexx materials), Lydall Performance Materials, Celgard LLC, A Porous Inc., SWM (Conwed Plastics, DelStar Technologies), Teijin, Hirose, Mitsubishi Paper Mills Ltd, and Sefar AG.
[0065] Preferably, the support is a polymer support.Preferably, the support is a woven or non-woven synthetic fabric or an extruded film that does not contain covalently bound ionic groups.
[0066] The membrane of the first aspect of the present invention is preferably a bipolar membrane or a membrane which can be converted into a bipolar membrane by hydrolysis.
[0067] The AEL of the film of the present invention is preferably obtained by curing a composition containing a curable cationic compound (ie, "AEL composition"). Therefore, the AEL composition preferably contains a curable cationic compound (referred to as component (a2) in the composition below).
[0068] Preferred curable cationic compounds contain at least two ethylenically unsaturated groups, such as compounds of formula (II).
[0069]
[0070] in:
[0071] L 1 is an alkylene group or an alkenylene group;
[0072] R a , R b , R c and R d are each independently an alkyl group or an aryl group, or
[0073] R a and R b , and / or R c and R d can form a ring together with the atoms to which they are attached;
[0074] n1 and n2 each independently represent an integer from 1 to 10; and
[0075] X1 - and X2 - Each independently represents an anion.
[0076] L 1 Preferred is ethylene, propylene, hexylene or vinylene.
[0077] When R a , R b , R c and R d When any one of is an alkyl group, preferably C 1-4 Alkyl groups, especially methyl.
[0078] When R a , R b , R c and R d When any one of is an aryl group, preferably C 6-10 Aryl groups, in particular phenyl.
[0079] When R a and R b , and / or R c and R d When forming a ring together with the atoms to which they are attached, the ring is preferably a 5-membered or 6-membered ring.
[0080] By X1 - and X2 - The anions represented are preferably each independently a halogen, in particular Cl - .
[0081] Therefore, the AEL composition preferably comprises the following ingredients:
[0082] (a2) a curable cationic compound comprising at least two ethylenically unsaturated groups;
[0083] Optional (b2) compounds containing one and only one ethylenically unsaturated group;
[0084] optionally (c2) a solvent; and
[0085] Optional (d2) free radical initiator.
[0086] Preferably, the AEL composition comprises at least one, more preferably at least two, especially all three of components (b2), (c2) and (d2).
[0087] Examples of compounds of formula (II) include the following:
[0088]
[0089] Synthesis methods can be found in, for example, EP3184558 and US2016 / 0001238.
[0090] The AEL composition preferably comprises 30 to 80 wt% of the compound of component (a2), more preferably 40 to 70 wt% of component (a2).
[0091] Preferably, the AEL composition comprises:
[0092] (i) 30 to 80 wt % of component (a2);
[0093] (ii) 0 to 40 wt % of component (b2); and
[0094] (iii) 10 to 40% by weight of component (c2).
[0095] Component (b2) preferably comprises aromatic groups.
[0096] Component (b2) preferably comprises cationic groups.
[0097] Examples of compounds useful as component (b2) of the AEL composition include the following:
[0098]
[0099] The above compounds can be prepared as described in, for example, US2016177006.
[0100] Preferably, the molar ratio of component (a2) to component (b2) in the AEL composition is from 9:1 to 1:4.
[0101] The AEL composition comprises from 0 to 60 wt%, more preferably from 5 to 45 wt%, most preferably from 10 to 40 wt% of component (b2).
[0102] Component (c2) of the AEL composition preferably comprises water and optionally an organic solvent, particularly where some or all of the organic solvent is water miscible. Water may be used to dissolve the compound of formula (II) and component (c2) (if present). The solvent may be used to reduce the viscosity and / or surface tension of the composition.
[0103] Examples of suitable solvents that can be used as component (c2) of the AEL composition include water, alcohol solvents, ether solvents, amide solvents, ketone solvents, sulfoxide solvents, sulfone solvents, nitrile solvents, organophosphorus solvents, and mixtures comprising two or more thereof. Examples of alcohol solvents that can be used as or for component (ii) (especially in combination with water) include methanol, ethanol, isopropanol, n-butanol, ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, and mixtures comprising two or more thereof. In addition, preferred inert organic solvents that can be used for component (ii) include dimethyl sulfoxide, dimethylimidazolidinone, sulfolane, N-methylpyrrolidone, dimethylformamide, acetonitrile, acetone, 1,4-dioxane, 1,3-dioxolane, tetramethylurea, hexamethylphosphoramide, hexamethylphosphoric triamide, pyridine, propionitrile, butanone, cyclohexanone, tetrahydrofuran, tetrahydropyran, 2-methyltetrahydrofuran, ethylene glycol diacetate, cyclopentyl methyl ether, methyl ethyl ketone, ethyl acetate, γ-butyrolactone, and mixtures comprising two or more thereof. Preferred are dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylimidazolidinone, sulfolane, acetone, cyclopentyl methyl ether, methyl ethyl ketone, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, and mixtures comprising two or more thereof.
[0104] In some embodiments, the AEL composition comprises 10 to 40 wt%, more preferably 10 to 35 wt%, most preferably 15 to 30 wt% of component (c2).
[0105] Examples of components (c2) to (d2) that may be included in the AEL composition for forming the AEL are as described above in relation to the CEL composition as components (c) and (d), respectively. However, component (c2) of the AEL composition is preferably aqueous.
[0106] Component (d2) is preferably or comprises a thermal initiator, a photoinitiator or a combination thereof. Most preferably, component (d) is or comprises a photoinitiator.
[0107] Examples of suitable photoinitiators that can be used as component (d2) of the AEL composition include aromatic ketones, acylphosphine compounds, aromatic onium salt compounds, organic peroxides, thio compounds, hexaarylbiimidazole compounds, ketoximate compounds, borate compounds, azinium compounds, metallocene compounds, active ester compounds, compounds having a carbon-halogen bond, and alkylamine compounds. Preferred examples of aromatic ketones, acylphosphine oxide compounds, and thio compounds include compounds having a benzophenone main chain or a thioxanthone main chain, which are described in "RADIATION CURING IN POLYMER SCIENCE AND TECHNOLOGY", pp. 77-117 (1993). More preferred examples thereof include α-thiobenzophenone compounds described in JP1972-6416B (JP-S47-6416B), JP1972-3981B (JP-S47-3981 B), benzoin ether compounds described in JP1972-22326B (JP-S47-22326B), benzoin derivatives described in JP1972-23664B (JP-S47-23664B), aromatic acylphosphonates described in JP1982-30704A (JP-S57-30704A), dialkoxybenzophenones described in JP1985-26483B (JP-S60-26483B), benzoin ethers described in JP1985-26403B (JP-S60-26403B) and JP1987-81345A (JP S62-81345A), JP1989-34242B (JP H01-34242B), U.S. Pat. α-Aminobenzophenone described in Patent No. 4,318,791A and EP0284561A1, p-bis(dimethylaminobenzoyl)benzene described in JP1990-211452A (JP-H02-211452A), thiosubstituted aromatic ketones described in JP1986-194062A (JP-S61-194062A), acylphosphine sulfides described in JP1990-9597B (JP-H02-9597B), acylphosphines described in JP1990-9596B (JP-H02-9596B), thioxanthones described in JP1988-61950B (JP-S63-61950B), and coumarin described in JP1984-42864B (JP-S59-42864B). In addition, photoinitiators described in JP2008-105379A and JP2009-114290A are also preferred.In addition, a photoinitiator described in "Ultraviolet Curing System" by Kato Kiyomi (published by Research Center Co., Ltd. in 1989), pages 65 to 148, can be used.
[0108] Particularly preferred photoinitiators useful as component (d2) of the AEL composition include Norrish type II photoinitiators having an absorption maximum at a wavelength greater than 380 nm when measured in one or more of the following solvents at a temperature of 23° C.: water, ethanol and toluene. Examples include xanthene, flavin, curcumin, porphyrin, anthraquinone, phenoxazine, camphorquinone, phenazine, acridine, phenothiazine, xanthone, thioxanthone, thioxanthene, acridone, flavonoid, coumarin, fluorenone, quinoline, quinolone, naphthoquinone, quinolone, arylmethane, azo, benzophenone, carotenoid, anthocyanin, phthalocyanine, dipyrromethene, squarine, stilbene, styryl, triazine or anthocyanin derived photoinitiators.
[0109] The AEL composition preferably comprises 0.001 to 2 wt. % of component (d2), more preferably 0.005 to 0.9 wt. %.
[0110] The AEL composition and the CEL composition may optionally each independently further comprise a polymerization inhibitor. The polymerization inhibitor may be used to stabilize the composition during storage and use.
[0111] As the polymerization inhibitor, a known polymerization inhibitor can be used, and examples thereof include phenol compounds, hydroquinone compounds, certain amine compounds, mercapto compounds, and nitroxyl radical compounds.
[0112] Examples of phenolic compounds include hindered phenols (phenols having a tert-butyl group at the ortho position, and representative 2,6-di-tert-butyl-4-methylphenol) and bisphenols. Specific examples of hydroquinone compounds include monomethyl ether hydroquinone. Specific examples of amine compounds include N-nitroso-N-phenylhydroxylamine and N,N-diethylhydroxylamine. Specific examples of nitroxyl radical compounds include 4-hydroxy TEMPO (4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl radical).
[0113] The AEL composition and the CEL composition may optionally each independently further comprise two or more polymerization inhibitors.
[0114] When the composition for forming an AEL or CEL contains a polymerization inhibitor, the content thereof is preferably 0.01 to 5 wt %, more preferably 0.01 to 1 wt %, further preferably 0.01 to 0.5 wt %, relative to the total weight of the composition.
[0115] The AEL composition and the CEL composition may optionally each independently further comprise a surfactant, a polymer dispersant and / or a crater inhibitor.
[0116] In order to adjust the film physical properties of the AEL composition and / or CEL composition, various polymer compounds may be included therein. Suitable polymer compounds include acrylic polymers, polyurethane resins, polyamide resins, polyester resins, epoxy resins, phenolic resins, polycarbonate resins, polyvinyl butyral resins, polyvinyl formal resins, shellac, vinyl resins, acrylic resins, rubber-based resins, waxes and natural resins, and combinations of two or more of the above.
[0117] The AEL composition and the CEL composition may optionally further comprise a surfactant independently of each other, such as a nonionic surfactant, a cationic surfactant or an organic fluorine surfactant, etc. Specific examples of surfactants include anionic surfactants (e.g., alkylbenzene sulfonates, alkylnaphthalene sulfonates, higher fatty acid salts, sulfonates of higher fatty acid esters, sulfates of higher alcohol ethers, sulfonates of higher alcohol ethers, alkyl carboxylates and alkyl phosphates of higher alkyl sulfone amides) and nonionic surfactants (e.g., poly(oxyethylene) alkyl ethers, poly(oxyethylene) alkylphenyl ethers, poly(oxyethylene) fatty acid esters, sorbitan fatty acid esters, ethylene oxide adducts of acetylene glycols, ethylene oxide adducts of glycerol, and polyoxyethylene sorbitan fatty acid esters). Other suitable examples of surfactants include amphoteric surfactants (e.g., alkyl betaines and amide betaines), silicone-based surfactants, and fluorine-based surfactants. The surfactant may be appropriately selected from surfactants known in the art or derivatives thereof.
[0118] The AEL composition and the CEL composition may each independently further comprise a polymeric dispersant.
[0119] Specific examples of the polymer dispersant include polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl methyl ether, polyethylene oxide, polyethylene glycol, polypropylene glycol and polyacrylamide. Among them, polyvinyl pyrrolidone is preferably used.
[0120] The AEL composition and the CEL composition may each independently further comprise an anti-cratering agent (sometimes referred to as a surface conditioner), a leveling agent or a slip agent to prevent unevenness of the surface of the CEL or AEL, examples of which include organic modified polysiloxane (a mixture of polyether siloxane and polyether), polyether modified polysiloxane copolymers and silicon modified copolymers.
[0121] Examples of commercially available anti-cratering agents that may be included in the composition for forming the AEL and / or CEL include Tego Glide manufactured by Evonikindustries GmbH. TM 432. Tego Glide TM 110. Tego Glide TM 130. TegoGlide TM 406. Tego Glide TM 410. Tego Glide TM 411. Tego Glide TM 415. Tego Glide TM 420、Tego Glide TM 435. Tego Glide TM 440、Tego Glide TM 450、Tego Glide TM 482. Tego Glide TM A115, Tego Glide TM B1484 and Tego Glide TM ZG400 (both are product names).
[0122] The AEL composition and the CEL composition preferably each independently comprise 0 to 10 wt. %, more preferably 0 to 5 wt. %, in particular 1 to 2 wt. % of an anticrater agent (relative to the total weight of the relevant composition).
[0123] In one embodiment, the membrane of the present invention comprises a catalyst. The catalyst may be included in the AEL composition and / or the CEL composition. The catalyst may also be applied (as a post-treatment step) to the AEL (e.g., before applying the CEL composition thereon) using, for example (but not limited to), dipping, air knife coating, micro-roll coating, spraying, chemical (vapor) deposition) or physical (vapor) deposition.
[0124] Examples of suitable catalysts include metal salts, metal oxides, organometallic compounds, monomers, polymers or copolymers. Examples include, but are not limited to, FeCl3, FeCl2, AlCl3, MgCl2, RuCl3, CrCl3, Fe(OH)3, Al2O3, NiO, Zr(HPO4)2, MoS2, graphene oxide, Fe-polyvinyl alcohol complexes, polyvinyl alcohol (PVA), polyethylene glycol (PEG), polyethyleneimine (PEI), polyacrylic acid (PAA), copolymers of acrylic acid and maleic anhydride (PAAMA) and hyperbranched aliphatic polyesters and combinations comprising two or more of the above.
[0125] When the AEL composition or CEL composition comprises a catalyst, the amount of catalyst is preferably up to 5 wt%, such as 0.001 wt% to 1 wt%, relative to the weight of the relevant composition. When a catalyst is present, the amount of catalyst in the AEL and / or CEL is preferably up to 5 wt%, such as 0.001 wt% to 1 wt%.
[0126] According to a second aspect of the present invention, there is provided a method for manufacturing a film, comprising the following steps:
[0127] (i) applying the AEL composition to a carrier;
[0128] (ii) at least partially curing the AEL composition to form an anion exchange layer (AEL);
[0129] (iii) applying the CEL composition to the AEL; and
[0130] (iv) curing the CEL composition to form a cation exchange layer (CEL) on the AEL.
[0131] In step (ii), the AEL composition is preferably photocured, for example using ultraviolet light. Thus, preferably, component (d2) of the AEL composition is or comprises a photoinitiator.
[0132] In step (ii), the AEL composition is preferably cured to such an extent that the resulting AEL can be handled in a curing composition application station while still having unreacted ethylenically unsaturated groups available for crosslinking to the monomers of the CEL composition.
[0133] In step (iv), the CEL composition is preferably thermally cured. Thus, preferably, component (d) of the CEL composition is or comprises a thermal initiator.
[0134] Suitable temperatures for curing the CEL composition are from 50 to 120°C, more preferably from 50 to 100°C, especially from 60 to 85°C.
[0135] Thermal curing of CEL compositions typically requires from more than a minute to several hours.
[0136] Alternatively, the CEL composition is sandwiched between polymer films prior to curing to prevent evaporation of component (c), if present.
[0137] In the method of the second aspect of the invention, the composition is preferably applied in steps (i) and (iii) in a continuous manner, preferably through a manufacturing unit, which comprises a composition application station, one or more curing stations including a radiation source (when the composition is photocurable), one or more curing stations including one or more heat sources (when the composition is thermally curable), a film collection station and a device for moving the carrier from the composition application station to the curing station and the film collection station.
[0138] The composition application station may be located upstream relative to the curing station, and the curing station is located upstream relative to the film collection station.
[0139] Examples of application techniques include slot coating, slide coating, air knife coating, roller coating, screen printing and dipping. Depending on the technique used and the desired end specification, it may be necessary to remove excess composition from the substrate by, for example, roll-to-roll extrusion, roll-to-blade or blade-to-roll extrusion, blade-to-blade extrusion or removal using a coating bar.
[0140] UV or visible light photocuring is preferably performed at a wavelength of 100 nm to 800 nm, typically using 40 to 1500 mJ / cm 2 Thermal curing is preferably carried out at a temperature of 20° C. to 100° C., for example, for a time of 0.01 hour to 24 hours.
[0141] Alternatively, the method of the second aspect further comprises, for example, converting group X into a hydroxyl group by hydrolysis. In this way, the membrane can be converted into a bipolar membrane or a bipolar membrane with a large number of acidic groups. Suitable hydrolysis methods include hydrolysis under acidic or alkaline conditions, for example, using an acid (for example hydrochloric acid) or a base (for example a metal hydroxide, particularly sodium hydroxide or potassium hydroxide).
[0142] According to a third aspect of the present invention there is provided a membrane comprising an anion exchange layer (AEL) and a layer comprising -SO2X groups, wherein X is as defined above.
[0143] According to a fourth aspect of the present invention, there is provided a method for preparing a bipolar membrane, which comprises hydrolyzing at least part of the -SO2X groups in the membrane of the first aspect of the present invention into -SO2OH groups or salts thereof.
[0144] In one embodiment, the method of the fourth aspect of the invention hydrolyzes the SO2X group to a -SO2OH group (in free acid or salt form) by contact with an acid and / or alkaline aqueous solution. The hydrolysis can be achieved, for example, by immersing the membrane of the first aspect of the invention in an acid and / or alkaline aqueous solution, preferably at an elevated temperature (e.g., at 50 to 100° C.). The hydrolysis is preferably carried out for a total time of 1 hour to 1 month, particularly 5 hours to 1 week, by contact with an acid and / or alkaline aqueous solution.
[0145] Optionally, the aqueous acid and / or base solution contains a surfactant.
[0146] Optionally, the aqueous acid and / or base solution comprises a water-miscible organic solvent.
[0147] Preferably, the aqueous acid and / or base solution is aqueous, in particular at a strength of 0.05 to 1.0N.
[0148] Suitable acids include hydrochloric acid and sulfuric acid.
[0149] Suitable bases include sodium carbonate, ammonium hydroxide, tetramethylammonium hydroxide, potassium hydroxide and sodium hydroxide.
[0150] Optionally, the acid and / or base comprises a polar solvent, such as dimethyl sulfoxide, isopropyl alcohol, dimethyl carbonate, ethylmethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, or two or more thereof.
[0151] The extent of hydrolysis can be monitored over time by infrared spectroscopy.
[0152] In one embodiment, the method of the second aspect or the fourth aspect of the present invention further comprises step (vi): drying the obtained film, preferably at a temperature of 40°C to 200°C.
[0153] The membranes of the present invention may be made by a variety of alternative methods, including those described above.
[0154] The membranes of the invention can be used in a variety of applications, including electrodialysis and acid / base production. The membranes of the invention comprising CEL and AEL can also be used as bipolar membranes, particularly because they have good durability, low swelling in acidic and alkaline media, and can be produced cheaply, quickly and efficiently.
[0155] The present invention is further illustrated by the following examples, in which all parts and percentages are by weight unless otherwise specified.
[0156] The performance of the bipolar membrane of the present invention is characterized by the curve of intensity vs. voltage. In order to measure this curve, a six-chamber battery cell was used. The first electrode chamber comprises a platinum plate as a cathode and is separated from the second chamber by a CEM (CMX from Astom). The electrode chamber is filled with 0.5M Na2SO4. There is a reference BPM (from Fumatech) between the second and third chambers. The second and third chambers all contain 0.5M NaCl solution. The BPM to be analyzed is placed between the third and fourth chambers. The same reference BPM (from Fumatech) is placed between the fourth and fifth chambers, and a CEM (from Astom's CMX) is placed between the fifth and sixth chambers. The fourth and fifth chambers are also filled with 0.5M NaCl solution. The sixth chamber comprising a platinum plate as an anode is an electrode chamber, containing 0.5M Na2SO4.
[0157] By using the above-mentioned battery cell, the solution was applied at 600A / m at a temperature of 25°C. 2 The bipolar voltage was measured by using a Harber luggin capillary placed on each side of the BPM to be analyzed.
[0158] resistance
[0159] ER (Ω.cm) of the membranes (or their precursors) prepared in the examples 2 ) was measured by the method described by Dlugolecki et al. in J. of Membrane Science, 319 (2008) pp. 217-218, with the following modifications:
[0160] The auxiliary membranes are CMX and AMX from Tokuyama Soda of Japan;
[0161] The capillary and Ag / AgCl reference electrode (Metrohm model 6.0750.100) contained 3 M KCl;
[0162] The calibration liquid and the liquid in compartments 2, 3, 4 and 5 are 0.5 M NaCl solutions at 25 °C;
[0163] ·Effective membrane area is 9.62cm 2 ;
[0164] The distance between capillaries is 5.0 mm;
[0165] The measurement temperature is 25℃;
[0166] All compartments use Cole Parmer Masterflex console drives (77521-47) with Easy Load II 77200-62 gear pumps;
[0167] The flow rate of each stream was controlled to be 475 ml / min by a Porter Instrument flow meter (150AV-B250-4RVS model) and a Cole Parmer flow meter (G-30217-90 model); and the sample was equilibrated in a 0.5 M NaCl solution at room temperature for at least 1 hour before measurement.
[0168] Preferably, the ER(NaCl) of the membrane is less than 5Ω / cm 2 .
[0169] Permselectivity
[0170] The permselectivity (%), i.e., the selectivity for the passage of ions of opposite charge to the membrane (or its precursor) prepared in the example, was measured as follows. The membrane to be analyzed was placed in a two-compartment system. One compartment was filled with a 0.05M NaOH solution and the other compartment was filled with a 0.5M NaOH solution.
[0171] set up
[0172] The capillary and Ag / AgCl reference electrode (Metrohm model 6.0750.100) contained 3 M KCl;
[0173] ·Effective membrane area is 9.62cm 2 ;
[0174] The distance between the capillaries is about 15 mm;
[0175] The measured temperature is 21.0±0.2℃;
[0176] Both compartments use a Cole Parmer Masterflex console drive (77521-47) with an Easy Load II 77200-62 gear pump;
[0177] The flow rate constant was controlled at 500 ml / min using a Porter Instrument flow meter (150AV-B250-4RVS model) and a Cole Parmer flow meter (G-30217-90 model); the membrane sample was equilibrated in a 0.5 M NaOH solution for 1 h before measurement. The voltage was read from a conventional VOM (multimeter) after 20 minutes.
[0178] The PS(NaOH) of the membrane is preferably above 70%.
[0179] Infrared spectroscopy
[0180] Conventional IR measurement was used as the detection method by tracking the 910 cm -1 The peak intensity at 200 nm was used to monitor the hydrolysis of the alkyl sulfonate group (-SO2X in formula (I)) to the sulfonic acid group (-SO2OH or -SO2OM, where M is Na + , Li + or K + ). Spectra were collected in a PerkinElmer Frontier FT-IR spectrophotometer equipped with a diamond probe. Spectra were collected directly from the membranes after wiping off excess water.
[0181] NMR spectroscopy
[0182] The structures of the compounds synthesized in the examples were determined by using a Magritek Spincolve 60 carbon (60 MHz, 4 scans) NMR spectrometer. 1 H-NMR confirmation. Samples for analysis were prepared by dissolving 5 wt% of each compound in a deuterated solvent (shown in the Examples).
[0183] The following abbreviations are used in the examples:
[0184]
[0185]
[0186] Synthesis of Et-DVBS
[0187]
[0188] Step 1
[0189] A solution of 2,4-divinylbenzenesulfonic acid sodium salt (145.15 g; 0.625 mole, 1 molar equivalent) and TEMPOL (4-OH-TEMPO; 73 mg, about 500 ppm) in DMF (250 mL) was added dropwise over 1 hour to thionyl chloride (318 mL, 520 g; 4.375 mole, 7 molar equivalent) maintained at 0°C in an ice bath. After the addition was complete, the solution was slowly heated to room temperature and stirred for 16 hours. Thereafter, the reaction mixture was slowly poured into ice / water (1.5 L). Toluene (600 mL) was added and the entire mixture was filtered through Celite to remove undissolved material. The aqueous layer was extracted twice with toluene (300 mL) and the combined toluene layers were washed once with saturated KCl-solution (500 mL). The toluene solution was dried over sodium sulfate, filtered and concentrated in vacuo to give a yellow oil (about 120 g, 84%). The crude product was used in the second step without further purification. Synthesis by 1 H NMR confirmed.
[0190] Step 2
[0191] A solution of the product obtained in step 1 (120 g; 0.525 mole) and TEMPOL (4-OH-TEMPO; 60 mg, about 500 ppm) in pyridine (150 mL) was added dropwise to an ice-cooled (0°C) stirred solution of ethanol (46 mL, 36 g; 0.787 mole, 1.5 molar equivalents) in pyridine (75 mL). After stirring for two hours in an ice bath at 0°C, the reaction mixture was poured into an ice-cooled 1:1 mixture of ice and concentrated 36%-HCl (600 mL total volume). Chloroform (about 800 mL) was added and the mixture was transferred to a separation funnel. The aqueous layer was removed and the chloroform layer was washed successively with 3M HCl solution and saturated NaCl solution. The chloroform layer was dried over sodium sulfate and filtered. To the filtrate was added TEMPOL (about 25 mg; about 200 ppm) and then concentrated in vacuo to give an orange / brown oil (103 g; 82%). Synthesis by 1 H NMR confirmed.
[0192] A coating composition comprising EtSS, DVB, LiSS, a solvent and 0.5 wt% of V-65B was prepared according to the compositions CELC 1 to 4 described in Table 1. The composition was coated onto a porous substrate and laminated between two PET foils, and then thermally cured in an oven at 70°C for 16 hours. The resulting CEM precursor membranes PF1 to PF4 were then subjected to a hydrolysis process at 50°C. The hydrolysis conditions and the properties of the resulting cation exchange membranes (CEMs) are shown in Table 2.
[0193] Table 1: CEL compositions CELC 1 to 4
[0194]
[0195] Table 2: Hydrolysis of CEM precursor films PF1 to PF4 and properties of the resulting CEMs
[0196]
[0197] *All hydrolyzed solutions contain 10% IPA
[0198] Preparation of AEL
[0199] An AEL composition (AELC1) was prepared containing 58 wt% 1,4-diazabicyclo[2.2.2]octane, 1,4-bis[(4-vinylphenyl)methyl]chloride, 19 wt% water, 6 wt% IPA, 1 wt% Omnirad TM TPO-L and 1 wt% OmniradTM 1173. The AEL composition was coated on a nonwoven polyethylene fabric and cured by UV to obtain AEL.
[0200] Coat CEL and apply to AEL to produce BPM
[0201] CEL compositions were prepared according to Table 3 below. Each CEL composition was coated on the AEL prepared as above, then a second nonwoven polyethylene fabric was placed on the CEL composition layer, and the excess CEL composition was wiped off. Subsequently, the film was placed between PET sheets and cured in an oven at 80° C. for 16 hours. The resulting film was placed in a 0.1N NaOH solution containing 10% IPA for 72 hours to hydrolyze the -SO2X (ester) group to the corresponding sodium sulfonate salt to obtain BPM.
[0202] The electrochemical performance and bipolar properties of these bipolar membranes are compared with reference membranes using so-called current-voltage characteristics (IU curves), where the current density is measured as a function of the applied voltage. Typically, a given current density (i.e., 600 mA / cm 2 ) The lower the voltage (U) required, the lower the ionic resistance of one or both ion exchange layers in particular and of bipolar membranes in general. In the case of cation exchange layers, low ionic resistance leads to more energy-efficient membranes.
[0203] Table 3: CEL compositions CELC 5 to 7
[0204]
[0205] A comparative CEL composition (CExCELC1) was prepared in which the CEL layer of the BPM was obtained from a composition consisting of 30 wt% Na-AMPS (calculated on a pure material basis), 30 wt% M-11, 39 wt% water and 1 wt% V-65B. In the comparative BPM, the preparation of the AEL was exactly the same as described in the examples of the present invention.
[0206] The obtained BPM and its properties are shown in Table 4 below:
[0207] Table 4: BPMs with representative properties
[0208] Example AEL comes from: CEL comes from: Voltage* 1 AELC1 CELC5 2.92 2 AELC1 CELC6 2.78 3 AELC1 CELC7 2.67 CEx1 AELC1 CExCELC1 5.45
[0209] * Membrane at 600mA / m 2 Voltage displayed at current density.
Claims
1. A bipolar membrane comprising an anion exchange layer (AEL) and a cation exchange layer (CEL), wherein: The bipolar membrane is obtained by a method comprising the following steps: (i) applying the AEL composition to a porous support; (ii) at least partially curing the AEL composition to form the AEL; (iii) applying a CEL composition to the AEL; and (iv) curing the CEL composition to form the CEL on the AEL; Wherein, the CEL composition comprises the following components: (a) 20 to 88% by weight of a compound of formula (I): in: X is the formula -OC n H 2n+1 or -OC q H 2q-1 , wherein n has a value from 1 to 6 and q has a value of 5 or 6; and The value of m is 1 or 2; (b) 10 to 60% by weight of a compound containing at least two ethylenically unsaturated groups; (c) 0 to 30 wt % of a non-aqueous solvent; (d) 0 to 2 wt % of a free radical initiator; and (e) 0 to 15% by weight of anionic monomers containing one and only one ethylenically unsaturated group, And the average thickness of the porous support is 10 to 200 μm.
2. The bipolar membrane according to claim 1, wherein The curable composition from which the CEL is obtained comprises 20 to 60 wt % of component (b).
3. The bipolar membrane according to claim 1, wherein Component (b) contains an aromatic group.
4. The bipolar membrane according to claim 1, wherein Component (b) comprises at least two (meth)acrylic groups and / or vinyl groups.
5. The bipolar membrane according to claim 2, wherein The molar ratio of component (a) to component (b) is 2:1 to 1:
2.
6. The bipolar membrane according to claim 1, wherein The curable composition from which the CEL is obtained comprises at least 60% by weight of a curable compound.
7. The bipolar membrane of claim 1, wherein: The AEL is obtained by curing a composition containing a curable cationic compound.
8. The bipolar membrane of claim 1, wherein: The AEL is obtained by curing a composition comprising the following ingredients: (a2) 30 to 80% by weight of a curable cationic compound containing at least two ethylenically unsaturated groups; (b2) 0 to 40% by weight of a compound containing one and only one ethylenically unsaturated group; (c2) 10 to 40 wt % of a solvent; and (d2) 0.001 to 2% by weight of a free radical initiator.
9. The bipolar membrane of claim 8, wherein: The molar ratio of component (a2) to component (b2) is 9:1 to 1:
4.
10. The bipolar membrane of claim 8, wherein Component (a2) has the formula (II): in: L 1 is an alkylene group or an alkenylene group; R a , R b , R c and R d are each independently an alkyl group or an aryl group, or R a and R b , and / or R c and R d Together with the atoms to which they are attached, they form a ring; n1 and n2 each independently represent an integer from 1 to 10; and X1 - and X2 - Each independently represents an anion.
11. A method for producing a bipolar membrane according to any one of claims 1 to 10, comprising the steps of: (i) applying the AEL composition to the porous support; (ii) at least partially curing the AEL composition to form the AEL; (iii) applying the CEL composition to the AEL; and (iv) curing the CEL composition to form the CEL on the AEL; Wherein, the AEL composition comprises a curable cationic compound.
12. The method of claim 11, wherein: The method further comprises the step of hydrolyzing at least part of the -SO2X groups in the compound of formula (I) into -SO2OH groups or salts thereof.
13. The method of claim 11, wherein: The AEL composition is as defined in claim 8.
14. Use of the bipolar membrane according to claim 1 for the production of acids and bases or for the generation of electrical energy.
Citation Information
Patent Citations
Alpha-aminoacetophenones as photo initiators
EP0284561A2
Composition for forming polymeric membrane, process for producing same, polymeric membrane, separation membrane module, and ion exchange device
EP3184558A1
JP1972003981B1
JP1972006416B1
JP1972022326B1