A method and device for producing olefins by catalytic cracking of waste plastics
By directly performing a catalytic cracking reaction between heated and melted waste plastics and recycled pyrolysis oil under the action of a catalyst, the problems of low propylene selectivity and complex dechlorination treatment in the catalytic cracking of waste plastics are solved, and efficient production of low-carbon olefins and cost reduction effect.
Patent Information
- Application Number
- CN202310230896.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-11
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-11
AI Technical Summary
In the existing technology, the catalytic cracking of waste plastics to produce low-carbon olefins has low propylene selectivity and requires separate dechlorination treatment, which increases the cost and operational complexity.
The heated and melted waste plastics and recycled cracked oil are used to perform catalytic cracking reaction under the action of a catalyst. The reaction product is steam stripped and regenerated to obtain cracked gas and liquid phase products. Olefins are obtained through gas-liquid separation and oil-water separation, and are utilized The bifunctional catalyst directly catalyzes cracking to generate ethylene, propylene, and butylene, and converts hydrogen chloride into metal chloride in situ during the reaction to avoid the generation of chlorinated alkane to pollute the product.
It realizes the direct production of high value-added chemical products, simplifies the process flow, reduces investment and operating costs, improves the yield of propylene and the activity stability of the catalyst, and reduces chloride pollution.
Smart Images

Figure CN116240042B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste plastic treatment, and in particular relates to a method and a device for producing olefins by catalytic cracking of waste plastics. Background Art
[0002] With the rapid development of the plastics industry and the increasing demand for plastic products, the proportion of used plastic solid waste in urban solid waste is also increasing day by day. Conventional methods for the treatment of waste plastics include landfill, incineration, physical recycling and chemical conversion. Landfill is the most commonly used method for treating solid waste, but it wastes land resources, and as time goes by, harmful substances such as additives and plasticizers in the waste plastics after landfill will dissolve, causing secondary pollution to the environment; incineration is currently a more commonly used treatment method. The combustion calorific value of waste plastics is equivalent to that of fuel oil, and it can be converted into heat energy after incineration, but harmful gases such as CO2 and dioxins will be produced during the incineration process, which will increase carbon emissions and pollute the atmosphere; physical recycling is to clean the waste plastics, granulate them, melt them and reuse them, which has certain economic benefits, but due to the variety of recycled waste plastics, the composite recycled plastics obtained after melting and regeneration are unstable, and can only produce some low-end plastic products, and the quality and value are far lower than new plastics.
[0003] The chemical conversion method is to convert waste plastics into fuel oil or chemical raw materials through thermal cracking or catalytic cracking. It can not only alleviate the problem of resource shortage, but also will not cause secondary pollution to the environment. It is the best choice for reducing the amount of waste plastics and recycling them. At present, waste plastics, whether thermal cracking or catalytic cracking, are still mainly used to generate oil products. However, with the increasing number of new energy vehicles in China, the demand for oil products is on a downward trend, and chemicals such as low-carbon olefins still need to be imported. Therefore, the production of chemicals from waste plastics is an effective way to utilize waste plastics. In addition, since waste plastics contain polyvinyl chloride, the products generated by thermal cracking or catalytic cracking contain chlorides that affect product quality. The conventional method is to remove chlorides through hydrofining, but hydrofining and removal of chlorides require the construction of special equipment, which increases investment and operating costs, and seriously affects economic benefits.
[0004] In addition, ethylene and propylene in low-carbon olefins are both important chemical raw materials. Among them, propylene is one of the basic raw materials of the three major synthetic materials, and its largest amount is used to produce polypropylene. In addition, propylene can be used to prepare acrylonitrile, propylene oxide, isopropanol, phenol, acetone, butanol, octanol, acrylic acid and its esters, propylene glycol, epichlorohydrin and synthetic glycerol. If waste plastics can be converted into products such as propylene, huge economic benefits will be generated. In the prior art, patent document CN113398982B discloses a catalyst for preparing low-carbon olefins from waste plastics, which has a high liquefied gas yield, but the main products are propylene and butene, and the selectivity of propylene is relatively low; patent document CN112316986A provides a catalyst for producing low-carbon olefins and aromatics from waste plastics, and the low-carbon olefins are mainly ethylene.
[0005] In general, in the prior art, the selectivity of propylene in the product distribution of low-carbon olefins produced from waste plastics still needs to be further improved, and the overall process for producing olefins requires separate dechlorination, which is relatively costly.
[0006] In view of this, a method and device for producing olefins by catalytic cracking of waste plastics are proposed in the present invention. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method and device for producing olefins by catalytic cracking of waste plastics. The waste plastics do not need dechlorination pretreatment and can be directly contacted with a catalyst for catalytic cracking to produce high value-added chemical products such as low-carbon olefins, with a short process flow and low operating costs.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] In a first aspect, a method for producing olefins by catalytic cracking of waste plastics comprises: mixing heated and molten waste plastics with recycled cracking oil and then performing a catalytic cracking reaction under the action of a catalyst to obtain a reaction product; after the reaction is completed, the catalyst after the reaction is regenerated after steam stripping, the reaction product is subjected to gas-liquid separation to obtain cracking gas and liquid products, the liquid product is subjected to oil-water separation to obtain the cracking oil, and a part of the cracking oil is recycled; the obtained cracking gas is further separated to obtain olefins.
[0010] As a further preferred embodiment of the technical solution of the present invention, the catalytic cracking reaction conditions are: reactor outlet temperature 450-650°C, reaction pressure 0.05-0.5MPa, reaction time 0.1-3s, catalyst-oil ratio 5-25, and water vapor injection amount 5-50% of the mass of the waste plastic feed.
[0011] As a further preferred embodiment of the technical solution of the present invention, the catalyst comprises, by mass fraction: 41-65% of the first active component, 3-9% of the second active component, 1-9% of the auxiliary active component, and the remainder being a carrier and a binder;
[0012] Wherein, the first active component is ZSM-5 molecular sieve;
[0013] Wherein, the second active component is selected from one or both of calcium oxide and magnesium oxide.
[0014] As a further preferred embodiment of the technical solution of the present invention, the silicon-aluminum ratio of the ZSM-5 molecular sieve is 75-300; preferably, the silicon-aluminum ratio is 90-150.
[0015] As a further preferred embodiment of the technical solution of the present invention, the auxiliary active component is selected from a combination of one or more of rare earth metal oxides, phosphorus oxide, and boron oxide.
[0016] As a further preferred embodiment of the technical solution of the present invention, the rare earth oxide is cerium oxide.
[0017] As a further preferred embodiment of the technical solution of the present invention, the cerium oxide is obtained by decomposing cerium chloride or cerium nitrate; the calcium oxide is obtained by decomposing calcium chloride or calcium nitrate; and the magnesium oxide is obtained by decomposing magnesium chloride or magnesium nitrate.
[0018] As a further preferred embodiment of the technical solution of the present invention, the binder is selected from one or both of aluminum sol and silica sol; the carrier is selected from one or more of silicon oxide, kaolin, attapulgite, bentonite and diatomaceous earth.
[0019] As a further preferred embodiment of the technical solution of the present invention, the preparation of the catalyst comprises the following steps:
[0020] After deionized water and a binder are stirred evenly, a carrier is added and stirred evenly again; then, a ZSM-5 molecular sieve is added and stirred evenly again to obtain a sol, and then an auxiliary active component is added to the sol and stirred to obtain a solution 1;
[0021] Add the second active component to deionized water and stir evenly to obtain solution 2;
[0022] Solution 2 is added to solution 1, and after stirring, the mixture is filtered and ground to obtain solution 3;
[0023] The solution 3 is molded, dried and calcined to obtain a finished catalyst.
[0024] As a further preferred embodiment of the technical solution of the present invention, the specific steps of molding, drying and calcining are: sending the obtained solution 3 into a spray drying tower for treatment to obtain a molded catalyst, with a furnace temperature of 350-550°C, an outlet temperature of 150-350°C, and a spray pressure of 2-5MPa; then, drying the molded catalyst at 150-250°C for 2-6h, and after drying, calcining at 450-600°C for 2-6h to obtain a finished catalyst.
[0025] As a further preferred embodiment of the technical solution of the present invention, the conditions for catalyst regeneration are: regeneration pressure 0.05-0.5 MPa, regeneration temperature 450-650°C.
[0026] In a second aspect, a device for realizing the above-mentioned method for producing olefins by catalytic cracking of waste plastics is provided, comprising: a waste plastic feeder, a riser reactor, a catalyst settler, a stripper for regenerated catalyst, and a catalyst regenerator;
[0027] The waste plastic feeder is connected to the riser reactor through a pipeline, and the riser reactor is connected to the catalyst settler through a pipeline; a catalytic cracking oil and gas outlet is provided at one end of the catalyst settler; the other end of the catalyst settler is located inside the catalyst regenerator, the catalyst stripper to be regenerated is located inside the catalyst regenerator, and the catalyst settler and the catalyst stripper to be regenerated are arranged in an upper and lower overlapping manner; the catalyst regenerator is connected to the riser reactor through a pipeline.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The process of the present invention can directly catalytically crack waste plastics to produce chemicals such as ethylene, propylene, and butene, without the need to separately dechlorinate the waste plastics. The process is simple, with low investment cost and low processing cost.
[0030] (2) The process of the present invention can convert the hydrogen chloride generated during the processing of waste plastics into metal chlorides in situ, effectively preventing the generation of chlorinated alkanes to contaminate the product.
[0031] (3) The present invention is applicable to a fluidized bed process with a continuous reaction-regeneration cycle, and the activity of the catalyst is maintained by regenerating the catalyst by burning it and continuously adding and discharging the catalyst.
[0032] (4) In the process provided by the present invention, the content of active components of the bifunctional catalyst molecular sieve is high, and the yield of directly catalytically cracking waste plastics to produce ethylene, propylene, butene, etc. is high, and the maximum yield of propylene can reach 31%+.
[0033] (5) The bifunctional catalyst of the present invention has good hydrothermal stability and a long service life due to modification of the biactive components.
[0034] (6) In the process provided by the present invention, aluminum sol is used as a binder in the catalyst preparation process, and a catalyst carrier such as composite kaolin is used. When the catalyst molecular sieve content is high, the catalyst still has good anti-wear performance, effectively reducing the consumption cost of the catalyst.
[0035] (7) In the process method provided by the present invention, the raw materials of the bifunctional catalyst are cheap and easily available, the production process is simple, and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The present invention provides a process flow diagram of a method for producing olefins by catalytic cracking of waste plastics.
[0037] Figure 2 This is a schematic diagram of the device for producing olefins by catalytic cracking of waste plastics provided by the present invention.
[0038] Among them, 1. waste plastic feeder; 2. riser reactor; 3. catalytic cracking oil and gas; 4. catalyst settler; 5. catalyst regeneration flue gas; 6. stripper for regenerated catalyst; 7. catalyst regenerator; 8. catalyst regeneration air. DETAILED DESCRIPTION
[0039] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Meanwhile, it should be emphasized that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturers are not specified, are all conventional products that can be purchased commercially.
[0041] See also Figure 1 A method for producing olefins by catalytic cracking of waste plastics, comprising: mixing heated and molten waste plastics with recycled cracking oil, and then performing a catalytic cracking reaction under the action of a catalyst to obtain a reaction product; after the reaction is completed, the catalyst after the reaction is regenerated after steam stripping, the reaction product is subjected to gas-liquid separation to obtain cracking gas and liquid products, the liquid product is subjected to oil-water separation to obtain the cracking oil, and a part of the cracking oil is recycled; the obtained cracking gas is further separated to obtain olefins.
[0042] In the above technical scheme, the heated and molten waste plastics are mixed with the recycled pyrolysis oil and enter the fluidized bed catalytic cracking reactor, and a catalytic cracking reaction occurs under the action of the catalytic cracking catalyst. The oil and gas generated by the catalytic cracking reaction of the waste plastics are cooled and separated into pyrolysis gas and liquid products. The pyrolysis gas is further separated to obtain gas products such as ethylene, propylene, butene, etc. The obtained liquid products are separated by oil and water to obtain pyrolysis oil. A part of the obtained pyrolysis oil is recycled, and the remaining part is directly discharged from the device. The catalyst in the fluidized bed reactor needs to be transferred to the fluidized bed catalyst regenerator for charring and regeneration due to coking deactivation, and the charred and regenerated catalyst is returned to the fluidized bed reactor. In addition, since the catalyst reacts with hydrogen chloride for a long time, the catalyst deactivation will also be caused. This deactivated catalyst cannot be restored by charring and regeneration, and the catalyst needs to be regularly unloaded, and fresh catalyst is regularly added to maintain the dechlorination activity of the catalyst. It should be particularly emphasized that the devices used to obtain ethylene, propylene, butene and other gases by further separation of pyrolysis gas are all mature process devices in the prior art. The specific structure or device is not limited in the present invention, which is subject to the ability of those skilled in the art to implement.
[0043] In some embodiments, the catalytic cracking reaction conditions are: reactor outlet temperature 450-650°C, reaction pressure 0.05-0.5MPa, reaction time 0.1-3s, agent-oil ratio 5-25, and atomized water vapor injection amount 5-50% (accounting for the amount of waste plastic feed); preferably, the reactor outlet temperature is 480-550°C, the reaction time is 0.5-1.5s, the agent-oil ratio is 10-15, the reaction pressure is 0.1-0.2MPa, and the atomized water vapor injection amount is 15-40%. It can be understood that the reactor outlet temperature can be any specific value among 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, or any value within the range of 480-550°C; the reaction pressure can be any specific value among 0.1MPa, 0.11MPa, 0.12MPa, 0.13MPa, 0.14MPa, 0.15MPa, 0.16MPa, 0.17MPa, 0.18MPa, 0.19MPa, 0.2MPa, or any value within the range of 0.1-0.2MPa; the reaction time can be 0.5s, 0.6s, 0.7s, 0.8s, 0.9s, 1 s, 1.1s, 1.2s, 1.3s, 1.4s, 1.5s, or any value in the range of 0.5-1.5s; the agent-oil ratio can be any specific value among 10, 11, 12, 13, 14, 15, or any value in the range of 10-15; the water vapor injection amount can be any specific value among 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, or any value in the range of 15-40%. It should be emphasized that in the present invention, a certain amount of water vapor is injected during the catalytic cracking reaction because: adding water vapor into the catalytic cracking reactor can not only increase the olefin yield of the catalytic cracking reaction of waste plastics to produce olefins, but also reduce the coking of the catalyst during the catalytic cracking process and alleviate the deactivation of the catalyst.
[0044] In some embodiments, the catalyst comprises, by mass fraction: 41-65% of a first active component, 3-9% of a second active component, 1-9% of an auxiliary active component, and the remainder being a carrier and a binder;
[0045] Wherein, the first active component is ZSM-5 molecular sieve;
[0046] Wherein, the second active component is selected from one or both of calcium oxide and magnesium oxide.
[0047] In the above technical scheme, the catalyst is a bifunctional catalyst, one of the active components is ZSM-5 molecular sieve, and the cracking reaction of waste plastics such as polyethylene (PE) and polypropylene (PP) on ZSM-5 molecular sieve solid acid catalyst follows the classic carbon ion reaction mechanism. First, the long-chain olefins produced by thermal cracking of the polymer obtain protons H from the B acid site on the catalyst surface. + The carbon ions are generated, which then undergo β-cleavage to generate smaller molecular olefins, or the carbon ions act as intermediates in other secondary reactions to undergo isomerization, cyclization, aromatization and other reactions to generate alkanes, olefins, aromatics and other compounds.
[0048] PVC waste plastics also undergo similar reactions on ZSM-5 molecular sieve solid acid catalysts, but hydrogen chloride is also generated at the same time. Hydrogen chloride reacts with olefin molecules generated by catalytic cracking of waste plastics to produce addition reactions, resulting in both gaseous and liquid products containing chloroalkanes, which seriously affects product quality.
[0049] Another active component of the bifunctional catalyst is a metal oxide (selected from one or both of calcium oxide and magnesium oxide), which can react in situ with hydrogen chloride generated by catalytic cracking of waste plastics to generate metal chloride, thereby blocking the reaction of hydrogen chloride with olefins to generate chloroalkane polluting products.
[0050] In the catalyst of the present invention, the ZSM-5 molecular sieve has the function of catalytically cracking waste plastics to generate low-carbon olefins; the function of the second active component metal oxide is to convert hydrogen chloride generated in the process of catalytic cracking of waste plastics into metal salts in situ to remove hydrogen chloride; the auxiliary active components rare earth metal oxide, phosphorus oxide, boron oxide and the like can improve the hydrothermal stability of the active component ZSM-5 molecular sieve in the process of high-temperature regeneration, because the molecular sieve modified with oxides such as rare earth metal oxide, phosphorus oxide, boron oxide and the like has a crystal volume shrinkage tendency greatly slowed down in a high-temperature water vapor environment, and the modification can weaken the strong acid center of the molecular sieve and is also conducive to improving the selectivity of low-carbon olefins; at the same time, the rare earth metal oxide, phosphorus oxide and boron oxide can form a weak binding force with the second active component metal oxide, can effectively alleviate the aggregation of the high-content second active component metal oxide in the process of high-temperature regeneration, retain its dispersion to the maximum extent, and play a role in effectively capturing hydrogen chloride; the function of the carrier is to provide a good dispersion matrix for the catalyst and provide suitable wear strength and particle shape, etc., to meet the needs of normal fluidization of the catalyst in the fluidized bed reactor.
[0051] In some embodiments, in the above catalyst, the content of each component is as follows, by mass fraction: 41-65% ZSM-5 molecular sieve, 3-9% second active component, 1-9% co-active component, and the remainder is carrier and binder. Preferably, the content of ZSM-5 molecular sieve is 45-55%. It can be understood that its content can be any specific value among 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, or any value within the range of 45-55%. Preferably, the amount of the second active component is 5-7.5%. It can be understood that its content can be any specific value among 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, or any value within the range of 5-7.5%.
[0052] In some embodiments, the silicon-aluminum ratio of the ZSM-5 molecular sieve is 75 to 300; preferably, the silicon-aluminum ratio is 90 to 150. It is understood that the silicon-aluminum ratio can be any specific value of 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, 150 or any value within the range of 90 to 150.
[0053] In some embodiments, the auxiliary active component is selected from a combination of one or more of rare earth metal oxides, phosphorus oxide, and boron oxide. Preferably, the rare earth metal oxide is cerium oxide; preferably, the auxiliary active component is a combination of cerium oxide and phosphorus oxide; further preferably, the content of cerium oxide is 1-5%; the content of phosphorus oxide is 0.5-3.5%; more preferably, the content of cerium oxide is 2-3.5%, and the content of phosphorus oxide is 1-2%. It can be understood that the content of cerium oxide can be any specific value among 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, or any value within the range of 2 to 3.5%; the content of phosphorus oxide can be any specific value among 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, or any value within the range of 1 to 2%.
[0054] In some embodiments, the source of the cerium oxide can be directly cerium oxide, or it can be obtained by decomposing cerium chloride or cerium nitrate; calcium oxide can be directly calcium oxide, or it can be obtained by decomposing calcium chloride or calcium nitrate; magnesium oxide can be directly magnesium oxide, or it can be obtained by decomposing magnesium chloride or magnesium nitrate.
[0055] In some embodiments, the binder is selected from one or both of aluminum sol or silica sol, preferably aluminum sol; the carrier is selected from one or more of silicon oxide, kaolin, attapulgite, bentonite, diatomaceous earth, preferably kaolin. The content of the binder is 15-30%, preferably 20-25%; the content of the carrier is 10-30%, preferably 15-20%. It is understood that the content of the binder can be any specific value of 20%, 21%, 22%, 23%, 24%, 25% or any value in the range of 20-25%; the content of the carrier can be any specific value of 15%, 16%, 17%, 18%, 19%, 20% or any value in the range of 15-20%.
[0056] In some embodiments, a method for preparing the above catalyst is also provided, comprising the following steps:
[0057] After deionized water and a binder are stirred evenly, a carrier is added and stirred evenly again; then, a ZSM-5 molecular sieve is added and stirred evenly again to obtain a sol, and then an auxiliary active component is added to the sol and stirred to obtain a solution 1;
[0058] Add the second active component to deionized water and stir evenly to obtain solution 2;
[0059] Solution 2 is added to solution 1, and after stirring, the mixture is filtered and ground to obtain solution 3;
[0060] The solution 3 is molded, dried and calcined to obtain a finished catalyst.
[0061] In some embodiments, the specific steps of molding, drying and calcining are: sending the obtained solution 3 into a spray drying tower for treatment to obtain a molded catalyst, with a furnace temperature of 350-550°C, an outlet temperature of 150-350°C, and a spray pressure of 2-5MPa; then, drying the molded catalyst at 150-250°C for 2-6 hours, and after drying, calcining at 450-600°C for 2-6 hours to obtain a finished catalyst. It can be understood that the furnace temperature can be any specific value of 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C or any value in the range of 350-550°C; the outlet temperature can be 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, Any specific value among 220℃, 230℃, 240℃, 250℃, 260℃, 270℃, 280℃, 290℃, 300℃, 310℃, 320℃, 330℃, 340℃, 350℃ or any value within the range of 150-350℃; the spray pressure can be 2MPa, 2.2MPa, 2.4MPa, 2.6MPa, 2.8MPa, 3MPa, 3.2MPa, 3.4MPa, 3.6MPa, 3.8MPa, 4MPa, 4.2MPa, 4.4MPa , 4.6MPa, 4.8MPa, 5MPa, or any value in the range of 2-5MPa; the catalyst drying temperature can be any specific value among 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, or any value in the range of 150-250°C; the drying time can be any specific value among 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, or any value in the range of 2- The calcination temperature may be any specific value among 450℃, 460℃, 470℃, 480℃, 490℃, 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, 600℃, or any value within the range of 450~600℃; the calcination time may be any specific value among 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, or any value within the range of 2~6h.
[0062] In some embodiments, the catalyst regeneration conditions are: regeneration pressure 0.05-0.5 MPa (gauge pressure), regeneration temperature 450-650° C. Preferably, the pressure is 0.1-0.2 MPa. It can be understood that the regeneration pressure (gauge pressure) can be any specific value among 0.1MPa, 0.11MPa, 0.12MPa, 0.13MPa, 0.14MPa, 0.15MPa, 0.16MPa, 0.17MPa, 0.18MPa, 0.19MPa, 0.2MPa, or any value within the range of 0.1-0.2MPa; the regeneration temperature can be any specific value among 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 510°C, 620°C, 630°C, 640°C, 650°C, or any value within the range of 450-650.
[0063] In the above production process, the main parts of the waste plastic catalytic cracking olefin production device are the fluidized bed reactor, the fluidized bed catalyst regeneration reactor and other facilities. The fluidized bed reactor includes a fluidized bed reactor and a riser reactor. In view of the short reaction time of the waste plastic catalytic cracking and the need to prevent the polymerization of the generated olefins and reduce the olefin yield, the riser reactor is preferred.
[0064] The deactivated catalyst fluidized bed regeneration reactor is a fluidized bed reactor. The regeneration process requires the use of regeneration gas, which is an oxygen-containing gas, preferably air.
[0065] Based on the above selection principles, see Figure 2 , a device for realizing the above-mentioned method of producing olefins by catalytic cracking of waste plastics, comprising: a waste plastic feeder 1 (including atomized water vapor feed), a riser reactor 2, a catalyst settler 4, a stripper for regenerated catalyst 6, and a catalyst regenerator 7;
[0066] The waste plastic feeder 1 is connected to the riser reactor 2 through a pipeline, and the riser reactor 2 is connected to the catalyst settler 4 through a pipeline; a catalytic cracking oil and gas outlet is opened at one end of the catalyst settler 4; the other end of the catalyst settler 4 is located inside the catalyst regenerator 7, the catalyst stripper 6 to be regenerated is located inside the catalyst regenerator 7, and the catalyst settler 4 and the catalyst stripper 6 to be regenerated are arranged in an upper and lower overlapped manner; the catalyst regenerator 7 is connected to the riser reactor 2 through a pipeline.
[0067] In the above technical scheme, the high-temperature liquid obtained after the raw material waste plastic is heated and melted, together with the recycled cracking oil and atomized steam, enters the riser reactor 2 in the reaction-regeneration unit through the plastic feeder 1, and then contacts the regenerated catalyst, moves upward in the riser reactor 2 and undergoes a cracking reaction. The catalyst and the cracking oil gas are separated in the catalyst settler 4, and the catalytic cracking oil gas 3 leaves the catalyst settler 4 and is separated from the gas and liquid to obtain cracking gas and cracking oil (containing water). The cracking gas is further separated to obtain olefin products such as ethylene, propylene, and butene; the cracking oil (containing water) is separated from the oil and water to obtain cracking oil and process water. The cracking oil is rich in aromatics, and light aromatics such as benzene, toluene, and xylene can be obtained by separation, and the process water is treated by decontamination. It can be understood that the catalyst regenerator 7 is provided with a feed port for catalyst regeneration air 8 and an outlet for catalyst regeneration flue gas 5.
[0068] The catalyst needs to be regenerated after participating in the reaction deactivation in the riser reactor 2. The catalyst to be regenerated (called the catalyst to be regenerated) enters the catalyst regenerator 7 after being stripped by water vapor in the catalyst stripper 6 to be regenerated under the action of the catalyst regeneration air 8. The regenerated catalyst returns to the riser reactor 2 through the delivery pipeline to continue to participate in the catalytic cracking reaction of the waste plastics, and the obtained catalyst regeneration flue gas 5 is subsequently treated. It should be particularly emphasized that the internal components of each of the above-mentioned devices are not specifically described or limited in the present invention, and those skilled in the art can choose according to actual needs. At the same time, it can also be understood that the above-mentioned device is a necessary process device part for realizing the waste plastic to olefin of the present invention, and can also include necessary devices for treating catalytic cracking oil and gas 3 such as gas-liquid separation device, oil-water separator, etc. The gas-liquid separation device is used to process the catalytic cracking oil and gas 3 to obtain cracking gas and liquid phase products. The cracking gas is further separated by the separation device to obtain products such as ethylene, propylene, butene, etc.; the liquid phase product is separated by the oil-water separation device to obtain process wastewater and cracking oil.
[0069] It should be particularly emphasized that the waste plastics mentioned in the present invention may be hydrocarbon plastics, generally one or more of polyethylene, polypropylene, polyvinyl chloride, ethylene-propylene copolymer, ethylene-octene copolymer, ethylene-butene copolymer, ethylene-cycloolefin copolymer, polydicyclopentadiene, cyclopentadiene copolymer, and polystyrene.
[0070] The method and device for producing olefins by catalytic cracking of waste plastics of the present invention are further described below in conjunction with specific embodiments.
[0071] Example 1
[0072] A method for preparing a catalyst for producing olefins by catalytic cracking of waste plastics, comprising:
[0073] 8000 kg of deionized water and 11900 kg of aluminum sol were stirred for 1 hour, and then 2700 kg of kaolin was added, and the mixture was stirred for another 4 hours; then 5000 kg of ZSM-5 molecular sieve with a silicon-aluminum ratio of 120 was added, and the mixture was stirred for another 6 hours to obtain a sol, and then 240 kg of 85% phosphoric acid and 750 kg of cerium nitrate hexahydrate were added to the sol, and the mixture was stirred for another 4 hours to obtain a solution 1;
[0074] Add 1500 kg of magnesium nitrate to 5000 kg of deionized water and stir for 2 hours to obtain solution 2;
[0075] Solution 2 was added to solution 1, and the mixture was stirred for 2 h, filtered, and ground to obtain solution 3;
[0076] The above solution 1 is sent to a spray drying tower for treatment to obtain a shaped catalyst, with a furnace temperature of 450°C, an outlet temperature of 180°C, and a spray pressure of 4MPa; then, the shaped catalyst is dried at 150°C for 4h, and after drying, it is calcined at 550°C for 6h to obtain a finished catalyst.
[0077] Example 2
[0078] A method for preparing a catalyst for producing olefins by catalytic cracking of waste plastics, comprising:
[0079] 5000 kg of deionized water and 11900 kg of aluminum sol were stirred for 1 hour, and then 2000 kg of kaolin was added, and the mixture was stirred for another 4 hours; then 5000 kg of ZSM-5 molecular sieve with a silicon-aluminum ratio of 120 was added, and the mixture was stirred for another 6 hours to obtain a sol, and then 240 kg of 85% phosphoric acid and 750 kg of cerium nitrate hexahydrate were added to the sol, and the mixture was stirred for another 4 hours to obtain a solution 1;
[0080] Add 1500 kg of calcium nitrate to 5000 kg of deionized water and stir for 2 hours to obtain solution 2;
[0081] Solution 2 was added to solution 1, and the mixture was stirred for 2 h, filtered, and ground to obtain solution 3;
[0082] The above solution 3 is sent to a spray drying tower for treatment to obtain a shaped catalyst, with a furnace temperature of 450°C, an outlet temperature of 180°C, and a spray pressure of 4MPa; then, the shaped catalyst is dried at 150°C for 4h, and after drying, it is calcined at 550°C for 6h to obtain a finished catalyst.
[0083] Example 3
[0084] A method for preparing a catalyst for producing olefins by catalytic cracking of waste plastics, comprising:
[0085] 5000 kg of deionized water and 11900 kg of aluminum sol were stirred for 1 hour, and then 1800 kg of kaolin was added, and the mixture was stirred for another 4 hours; then 5000 kg of ZSM-5 molecular sieve with a silicon-aluminum ratio of 120 was added, and the mixture was stirred for another 6 hours to obtain a sol; then 240 kg of 85% phosphoric acid and 750 kg of cerium nitrate hexahydrate were added to the sol, and the mixture was stirred for another 4 hours to obtain a solution 1;
[0086] Add 2000 kg of calcium nitrate to 5000 kg of deionized water and stir for 2 h to obtain solution 2;
[0087] Solution 2 was added to solution 1, and the mixture was stirred for 2 h, filtered, and ground to obtain solution 3;
[0088] The above solution 3 is sent to a spray drying tower for treatment to obtain a shaped catalyst, with a furnace temperature of 450°C, an outlet temperature of 180°C, and a spray pressure of 4MPa; then, the shaped catalyst is dried at 150°C for 4h, and after drying, it is calcined at 550°C for 6h to obtain a finished catalyst.
[0089] The product properties of the catalysts prepared in Examples 2 to 3 are as follows:
[0090] Table 1 Physical properties of catalysts
[0091]
[0092] As can be seen from Table 1, the catalyst prepared by the present invention has a suitable bulk density and particle size distribution as well as a high specific surface area and pore volume, and can be well adapted to the fluidization requirements of the reaction process of the fluidized bed reactor; when the catalyst molecular sieve content is about 50%, it still has good wear resistance (industrial applications generally require a wear index of ≤3%), which can ensure that the catalyst has a low loss during the fluidization process.
[0093] Example 4
[0094] A device for realizing the above-mentioned method of producing olefins by catalytic cracking of waste plastics, comprising: a waste plastic feeder 1, a riser reactor 2, a catalyst settler 4, a stripper for regenerated catalyst 6, and a catalyst regenerator 7;
[0095] The waste plastic feeder 1 is connected to the riser reactor 2 through a pipeline, and the riser reactor 2 is connected to the catalyst settler 4 through a pipeline; a catalytic cracking oil and gas outlet is opened at one end of the catalyst settler 4; the other end of the catalyst settler 4 is located inside the catalyst regenerator 7, the catalyst stripper 6 to be regenerated is located inside the catalyst regenerator 7, and the catalyst settler 4 and the catalyst stripper 6 to be regenerated are arranged in an upper and lower overlapped manner; the catalyst regenerator 7 is connected to the riser reactor 2 through a pipeline.
[0096] Application Example 5
[0097] The catalyst prepared in Example 2 was used to produce olefins from waste plastics. The specific test method is as follows: The test was carried out on the device described in Example 4, the raw materials were polypropylene particles plus about 1% polyvinyl chloride particles, and the overall chlorine content was 0.5%. The test results are shown in Table 2 below.
[0098] Table 2 Test results of olefin production by catalytic cracking of plastics
[0099]
[0100] As can be seen from Table 2, catalytic cracking of polypropylene (containing a small amount of polyvinyl chloride) can produce low-carbon olefins such as ethylene, propylene, butene, etc., with a total olefin yield of more than 60%; the oil product yield is greater than 20%, mainly aromatics; in addition, the dechlorination rate of the catalytic cracking process of polypropylene (containing a small amount of polyvinyl chloride) is greater than 97%, and both the gaseous and liquid products after dechlorination can be directly used.
[0101] In summary, the waste plastic catalytic cracking method of the present invention can directly produce chemicals such as ethylene, propylene, butene, and directly dechlorinate. Under appropriate process conditions, the waste plastic catalytic cracking can produce more than 60% of low-carbon olefins, and the catalyst dechlorination rate exceeds 97%. The process flow is short, the production device is simple, and the practicability is strong.
[0102] The present invention illustrates the technical concept of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of individual raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for producing olefins by catalytic cracking of waste plastics, characterized in that: include: The heated and melted waste plastics are mixed with the recycled pyrolysis oil and then subjected to catalytic pyrolysis reaction under the action of a catalyst to obtain a reaction product; After the reaction is completed, the catalyst after the reaction is regenerated after steam stripping, the reaction product is subjected to gas-liquid separation to obtain cracked gas and liquid phase product, the liquid phase product is subjected to oil-water separation to obtain the cracked oil, a part of the cracked oil is recycled; the cracked gas obtained is further separated to obtain olefins; The catalytic cracking reaction conditions are as follows: reactor outlet temperature 450-550°C, reaction pressure 0.05-0.5MPa, reaction time 0.1-3s, catalyst-oil ratio 5-25, and water vapor injection amount 5-50% of the mass of the waste plastic feed; The catalyst comprises, by mass fraction, 41-65% of a first active component, 3-9% of a second active component, 1-9% of an auxiliary active component, and the remainder being a carrier and a binder; Wherein, the first active component is ZSM-5 molecular sieve; Wherein, the second active component is selected from one or both of calcium oxide and magnesium oxide; The waste plastic contains polyvinyl chloride; Wherein, the auxiliary active components are rare earth metal oxide and phosphorus oxide; the rare earth metal oxide is cerium oxide; Wherein, the binder is selected from one or both of aluminum sol and silica sol; the carrier is selected from one or more of silicon oxide, kaolin, attapulgite, bentonite and diatomaceous earth; The preparation of the catalyst comprises the following steps: After deionized water and a binder are stirred evenly, a carrier is added and stirred evenly again; then, a ZSM-5 molecular sieve is added and stirred evenly again to obtain a sol, and then an auxiliary active component is added to the sol and stirred to obtain a solution 1; Add the second active component to deionized water and stir evenly to obtain solution 2; Solution 2 is added to solution 1, and after stirring, the mixture is filtered and ground to obtain solution 3; The solution 3 is molded, dried and calcined to obtain a finished catalyst; Among them, the specific steps of molding, drying and calcining treatment are: sending the obtained solution 3 into a spray drying tower for treatment to obtain a molded catalyst, with a furnace temperature of 350~550℃, an outlet temperature of 150~350℃, and a spray pressure of 2~5MPa; then, drying the molded catalyst at 150~250℃ for 2~6h, and after drying, calcining at 450~600℃ for 2~6h to obtain a finished catalyst.
2. The method for producing olefins by catalytic cracking of waste plastics according to claim 1, characterized in that: The silicon-aluminum ratio of ZSM-5 molecular sieve is 90~150.
3. The method for producing olefins by catalytic cracking of waste plastics according to claim 1, characterized in that: The cerium oxide is obtained by decomposing cerium chloride or cerium nitrate; the calcium oxide is obtained by decomposing calcium chloride or calcium nitrate; and the magnesium oxide is obtained by decomposing magnesium chloride or magnesium nitrate.