A flexible ceramic non-stick coating containing an aqueous high temperature resistant toughening component and a preparation method thereof
By introducing water-dispersible polyester modified silicone into ceramic coatings, the organic-inorganic interpenetrating structure is solved, and the high temperature flexibility and adhesion of ceramic coatings are achieved. Focus on improving.
Patent Information
- Application Number
- CN202211743627.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-29
AI Technical Summary
Ceramic non-stick coatings are fragile, easy to break at high temperatures, poor adhesion, and existing toughening methods such as the use of organic resins or emulsion systems have problems with insufficient heat resistance.
Use water-dispersible polyester modified silicone as a high-temperature toughening component to form an organic-inorganic interpenetrating structure through sol-gel reaction, buffering the shrinkage stress of the ceramic coating, and passing through polyester segments and silicone chains The segment improves adhesion and recoating properties.
It significantly improves the flexibility and adhesion of the ceramic coating, adapts to high temperature environments, maintains the hardness and heat resistance of the ceramic coating, and improves the recoating performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of new materials, and in particular to a flexible ceramic non-stick coating containing an aqueous high-temperature resistant toughening component and a preparation method thereof. Background Art
[0002] Since its invention, Teflon non-stick coating has been widely used in non-stick coatings, but its curing temperature is high (400℃), the coating hardness is low, it is easy to be scratched, the coating life is not long, and it will release harmful decomposition products at high temperatures (above 260℃). In addition, the health effects of GenX, a PFOA substitute used in the production process, are still uncertain. With the strengthening of people's environmental awareness and the gradual implementation of safety and health standards, the research and development of water-based inorganic ceramic non-stick coatings has regained attention. Compared with Teflon non-stick coatings, ceramic non-stick coatings have abundant raw material sources and low VOCs content; low curing temperature, energy saving; no toxic and harmful substances are produced during manufacturing and use, healthy and environmentally friendly; high hardness, scratch resistance, long service life, and resource saving.
[0003] However, the disadvantage of ceramic coatings is that they are very brittle and have poor toughness compared to organic coatings. The coatings are prone to collapse when colliding with some hard objects, and their adhesion to metal substrates is poor. Their applications are also greatly limited, and their market share in non-stick coatings has never been expanded. Therefore, it is necessary to solve these problems by toughening ceramic coatings. Studies have found that by dispersing ceramic powders in organic resins, flexible ceramic coating products can be obtained. The coatings formed by such products are non-continuous inorganic phase fillings and continuous organic phase structures. Macroscopically, they show impact resistance, flexibility, and good adhesion to the substrate, but their hardness is lower than that of ceramic coatings (pencil hardness is less than 4H), and their scratch resistance is relatively poor. There are also studies that use acrylic emulsions, polyurethane emulsions and ceramic coating systems to enhance the flexibility of ceramic coatings, but these emulsions have poor heat resistance. When ceramic coatings are applied to non-stick pans, the heating conditions during use are relatively complex, and obvious yellowing and coking of the coatings will occur. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a flexible ceramic non-stick coating containing an aqueous high-temperature resistant toughening component and a preparation method thereof. In the present invention, a water-dispersible polyester-modified silicone is added as a high-temperature resistant toughening component after the sol-gel reaction of the ceramic coating reaches a certain degree, and the water present in the system is used as a dispersion medium. Under the action of shear, it penetrates into the inorganic network structure formed by the sol-gel reaction of the ceramic coating to form a molecular-level three-dimensional composite of an organic-inorganic interpenetrating structure. The addition of water-dispersible polyester-modified silicone can buffer the shrinkage stress generated during the curing or bending of the ceramic coating through the change of its own volume, improve the flexibility of the ceramic coating, and at the same time improve the adhesion and recoating performance of the ceramic coating through the self-stratification phenomenon of the polyester segment and the silicone segment.
[0005] The specific technical scheme of the present invention is:
[0006] In the first aspect, the present invention provides a flexible ceramic non-stick coating containing an aqueous high-temperature resistant toughening component, which is made from the following raw materials in parts by weight: 4-10 parts of water-dispersible polyester-modified silicone, 10-30 parts of methyl silane, 3-6 parts of phenyl silane, 2-4 parts of solvent, 10-30 parts of nano-silica sol, 40-60 parts of high-temperature resistant pigments and fillers, 0.3-0.7 parts of additives, 0.2-0.4 parts of acid catalysts, and 50-70 parts of water.
[0007] The ceramic non-stick coating of the present invention is composed of water-dispersible polyester modified silicone, methyl silane, phenyl silane, solvent, nano silica sol, high temperature resistant pigment filler, auxiliary agent, acid catalyst and water. The water-dispersible polyester modified silicone is prepared by polymerization, end-capping, modification and neutralization of neopentyl glycol, isophthalic acid, trimethylolpropane, trimellitic anhydride, silicone intermediate and N, N-dimethylethanolamine. The addition of water-dispersible polyester modified silicone can buffer the shrinkage stress generated when the ceramic coating is cured or bent through the change of its own volume, improve the flexibility of the ceramic coating, and at the same time improve the adhesion and recoating performance of the ceramic coating through the self-stratification phenomenon of polyester segments and silicone segments.
[0008] Preferably, the water-dispersible polyester-modified silicone is prepared by the following preparation method: 1-2 mole parts of neopentyl glycol, 2.5-6 mole parts of trimethylolpropane, and 2-5 mole parts of isophthalic acid are added into a reactor, the temperature is raised to 170-185°C for esterification for 1-2 hours, and then the temperature is raised to 210-225°C, and the reaction is continued for 2-4 hours until the acid value drops below 10 mgKOH / g, the reaction is stopped, the temperature is lowered to 145-165°C, propylene glycol butyl ether and 0.7-1.5 mole parts of trimellitic anhydride are added, the reaction is continued until the acid value is 65-75 mgKOH / g, the temperature is lowered to 105-115°C, tetrabutyl titanate and silicone intermediate are added, the reaction is continued for 1-2 hours until transparent, the temperature is lowered to 70-80°C, and 1.2-2.5 mole parts of N, N-dimethylethanolamine are added for neutralization.
[0009] The invention uses neopentyl glycol, isophthalic acid and trimethylolpropane as monomers to prepare a hyperbranched polyester, which is then capped by trimellitic anhydride to synthesize a carboxyl-terminated hyperbranched polyester, and then the hydroxyl groups on the hyperbranched polyester react with the alkoxy groups on the organosilicon intermediate, and finally N,N-dimethylethanolamine is used to neutralize the carboxyl groups on the hyperbranched polyester to form salts, so as to obtain a water-dispersible polyester-modified organosilicon.
[0010] Preferably, the amount of propylene glycol butyl ether is 50-60wt% of trimethylolpropane; the amount of tetrabutyl titanate is 0.05-0.1wt% of trimethylolpropane; and the amount of the organosilicon intermediate is 150-200wt% of trimethylolpropane.
[0011] The present invention found that the amount of the above three substances is crucial to the performance of water-dispersible polyester-modified silicone. Specifically: the addition of propylene glycol butyl ether is used to dilute the hyperbranched polyester. Since the hyperbranched polyester has a regular structure and good solubility, it does not need to add a large amount of solvent to reduce the viscosity. Therefore, the amount of propylene glycol butyl ether is set at 50-60wt% of trimethylolpropane (triol); the polyester-modified silicone is produced by dealcoholization of the hydroxyl groups on the hyperbranched polyester and the alkoxy groups on the silicone intermediate. Since the silicone intermediate will also undergo a dehydration polycondensation reaction between the alkoxy groups, a catalyst needs to be added to enhance the selectivity of the reaction. Tetrabutyl titanate is a highly efficient catalyst for the reaction. When a small amount is added, it can promote the reaction very well. However, if the amount is too large, it will affect the performance of the subsequent cured coating. Therefore, the addition amount is selected to be 0.05-0.1wt% of trimethylolpropane. In theory, as the content of the organosilicon intermediate increases, the heat resistance will be better. However, when the organosilicon content is too high, the organosilicon intermediate that is not grafted onto the hyperbranched polyester will self-polymerize to produce by-products, affecting the stability of the system. Therefore, it is set to 150-200wt% of trimethylolpropane.
[0012] Preferably, the methylsilane is selected from methyltrimethoxysilane, methyltriethoxysilane and dimethyldimethoxysilane.
[0013] Preferably, the phenylsilane is selected from phenyltrimethoxysilane, phenyltriethoxysilane and diphenyldimethoxysilane.
[0014] Preferably, the solvent is selected from isopropyl alcohol, propylene glycol butyl ether, and propylene glycol methyl ether acetate.
[0015] Preferably, the nano silica sol is selected from the acidic silica sol Levasil CT30DH, Levasil CT20DH and Levasil CT8 DH produced by Nouryon.
[0016] Preferably, the heat-resistant color filler is composed of a mixture of heat-resistant pigment and heat-resistant filler in any ratio, the pigment is a heat-resistant pigment commonly used in the art, and can be an inorganic heat-resistant pigment such as carbon black and red iron oxide, or an organic heat-resistant pigment such as phthalocyanine blue. The filler is a heat-resistant filler commonly used in the art, and can be silicon carbide or aluminum oxide.
[0017] Preferably, the additive includes one or more of a dispersant, a leveling agent, and a defoaming agent; the dispersant is selected from UNIQ-690W, BYK-190, and AFCONA-4595; the leveling agent is selected from UNIQ-495U, BYK-333, and TEGO-450; the defoaming agent is selected from UNIQ-265W, BYK-028, and SURFYNOL-440.
[0018] Preferably, the acid catalyst is selected from formic acid, acetic acid and hydrochloric acid.
[0019] In a second aspect, the present invention provides a method for preparing the above-mentioned flexible ceramic non-stick coating containing an aqueous high temperature resistant toughening component, which specifically comprises the following steps:
[0020] (1) Mix nano silica sol, high temperature resistant pigment filler, additives and deionized water evenly, grind to a fineness of ≤10 μm to obtain a color paste.
[0021] (2) Adding a mixture of methylsilane, phenylsilane and solvent to the color paste prepared in step (1), mixing evenly, adding an acidic catalyst, stirring, and then adding a water-dispersible polyester-modified silicone, stirring at high speed, and filtering to obtain a flexible ceramic non-stick coating containing an aqueous high-temperature resistant toughening component.
[0022] The ceramic non-stick coating of the present invention is prepared through a sol-gel reaction: methylsilane and phenylsilane are dissolved in a solvent to form a uniform mixture, and then mixed with nano silica sol, high temperature resistant pigments and fillers, additives, and water through grinding to obtain a color paste. Under the catalysis of an acid, methylsilane and phenylsilane undergo a sol-gel reaction of hydrolysis and polycondensation, and components undergo a reaction between silanol hydroxyl groups, a reaction between silanol and siloxy groups, a reaction between silanol and the surface hydroxyl groups of nano silica, a reaction between silanol and the surface hydroxyl groups of pigments and fillers, and coordination bonds between molecules, and finally a ceramic-like hard coating is formed in the curing stage. Methylsilane can improve the hardness and self-cleaning effect of the ceramic coating, and phenylsilane helps to improve the flexibility, gloss, fullness and compatibility of the ceramic coating with other organic resins.
[0023] In addition, the timing of adding the water-dispersible polyester modified silicone in the present invention is particularly important. The water-dispersible polyester modified silicone in the present invention is added as a high-temperature resistant toughening component after the sol-gel reaction of the ceramic coating reaches a certain degree, with the water present in the system as the dispersion medium. Under the action of shear, it penetrates into the inorganic network structure formed by the sol-gel reaction of the ceramic coating to form a molecular-level three-dimensional composite of an organic-inorganic interpenetrating structure. The addition of polyester modified silicone can buffer the shrinkage stress generated when the ceramic coating is cured or bent through the change of its own volume, improve the flexibility of the ceramic coating, and also improve the adhesion and recoating performance of the ceramic coating through the self-stratification phenomenon of the polyester segment and the silicone segment.
[0024] Compared with the prior art, the present invention has the following technical effects:
[0025] (1) The present invention uses water-dispersible polyester-modified silicone as a toughening component of the ceramic non-stick coating, which has excellent high temperature resistance and is suitable for various high temperature heating environments.
[0026] (2) The present invention controls the order of adding raw materials so that the water-dispersible polyester-modified silicone and the ceramic inorganic network form an organic-inorganic interpenetrating molecular-level three-dimensional composite, which significantly improves the flexibility of the ceramic coating and improves the adhesion and recoating performance of the ceramic coating through a gradient self-stratification mechanism. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the embodiments.
[0028] Overall embodiment
[0029] A flexible ceramic non-stick coating containing an aqueous high temperature resistant toughening component is prepared from the following raw materials in parts by weight:
[0030] 4-10 parts of water-dispersible polyester modified silicone, 10-30 parts of methyl silane, 3-6 parts of phenyl silane, 2-4 parts of solvent, 10-30 parts of nano silica sol, 40-60 parts of high temperature resistant pigments and fillers, 0.3-0.7 parts of additives, 0.2-0.4 parts of acid catalysts, and 50-70 parts of water.
[0031] Wherein, methylsilane is selected from methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane. Phenylsilane is selected from phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane. Solvent is selected from isopropyl alcohol, propylene glycol butyl ether, propylene glycol methyl ether acetate. Nano silica sol is selected from acidic silica sol Levasil CT30 DH, Levasil CT20 DH, Levasil CT8 DH of Nouryon. High temperature resistant color filler is composed of high temperature resistant pigment and high temperature resistant filler mixed in any ratio. The pigment is a high temperature resistant pigment commonly used in the art, which can be an inorganic high temperature resistant pigment such as carbon black and iron oxide red, or an organic high temperature resistant pigment such as phthalocyanine blue. The filler is a high temperature resistant filler commonly used in the art, which can be silicon carbide or aluminum oxide. The additives include one or more of dispersants, leveling agents, and defoamers; the dispersants are selected from UNIQ-690W, BYK-190, and AFCONA-4595; the leveling agents are selected from UNIQ-495U, BYK-333, and TEGO-450; the defoamers are selected from UNIQ-265W, BYK-028, and SURFYNOL-440. The acid catalyst is selected from formic acid, acetic acid, and hydrochloric acid.
[0032] The water-dispersible polyester modified silicone is prepared by the following preparation method: 1-2 mole parts of neopentyl glycol, 2.5-6 mole parts of trimethylolpropane, and 2-5 mole parts of isophthalic acid are added into a reaction kettle, the temperature is raised to 170-185°C, and the esterification is carried out for 1-2 hours, and then the temperature is raised to 210-225°C, and the reaction is continued for 2-4 hours until the acid value drops below 10 mgKOH / g, and the reaction is stopped, and the temperature is lowered to 145-165°C, propylene glycol butyl ether (50% of trimethylolpropane) is added, and the reaction is carried out. -60wt%) and 0.7-1.5 mol parts of trimellitic anhydride, continue to react until the acid value is 65-75mgKOH / g, cool to 105-115°C, add tetrabutyl titanate (0.05-0.1wt% of trimethylolpropane) and silicone intermediate (150-200wt% of trimethylolpropane), react for 1-2h until transparent, cool to 70-80°C, add 1.2-2.5 mol parts of N,N-dimethylethanolamine for neutralization.
[0033] The method for preparing the above-mentioned flexible ceramic non-stick coating containing an aqueous high temperature resistant toughening component specifically comprises the following steps:
[0034] (1) Mix nano silica sol, high temperature resistant pigment filler, additives and deionized water evenly, grind to a fineness of ≤10 μm to obtain a color paste.
[0035] (2) Adding a mixture of methylsilane, phenylsilane and solvent to the color paste prepared in step (1), mixing evenly, adding an acidic catalyst, stirring, and then adding a water-dispersible polyester-modified silicone, stirring at high speed, and filtering to obtain a flexible ceramic non-stick coating containing an aqueous high-temperature resistant toughening component.
[0036] Preparation Example of Water-Dispersible Polyester Modified Silicone
[0037] Example 1
[0038] 1 mol part of neopentyl glycol, 2.5 mol parts of trimethylolpropane and 2 mol parts of isophthalic acid are put into a reactor, the temperature is raised to 170°C for esterification for 2 hours, then the temperature is raised to 210°C, the reaction is continued for 4 hours until the acid value drops to 8.2 mgKOH / g, the reaction is stopped, the temperature is lowered to 145°C, 50 wt% of propylene glycol butyl ether of trimethylolpropane and 0.7 mol parts of trimellitic anhydride are added, the reaction is continued until the acid value is 71.5 mgKOH / g, the temperature is lowered to 105°C, 0.05 wt% of trimethylolpropane tetrabutyl titanate and 150 wt% of trimethylolpropane organosilicon intermediate DC-3074 are added, the reaction is continued for 2 hours until it becomes transparent, the temperature is lowered to 70°C, and 1.2 mol parts of N,N-dimethylethanolamine are added for neutralization.
[0039] The reaction process is schematically shown below:
[0040]
[0041] Example 2
[0042] 2 mol parts of neopentyl glycol, 6 mol parts of trimethylolpropane and 5 mol parts of isophthalic acid are put into a reactor, the temperature is raised to 185°C for esterification for 1 hour, then the temperature is raised to 225°C, the reaction is continued for 2 hours until the acid value drops to 9.0 mgKOH / g, the reaction is stopped, the temperature is lowered to 165°C, 60 wt% of trimethylolpropane propylene glycol butyl ether and 1.5 mol parts of trimellitic anhydride are added, the reaction is continued until the acid value is 69.7 mgKOH / g, the temperature is lowered to 115°C, 0.1 wt% of trimethylolpropane tetrabutyl titanate and 200 wt% of trimethylolpropane organosilicon intermediate DC-3074 are added, the reaction is continued for 1 hour until it becomes transparent, the temperature is lowered to 80°C, and 2.5 mol parts of N,N-dimethylethanolamine are added for neutralization.
[0043] Coating Preparation Example
[0044] Example 3
[0045] (1) 10 parts by weight of nano silica sol Levasil CT30 DH, 15 parts by weight of carbon black, 25 parts by weight of silicon carbide, 0.2 parts by weight of dispersant UNIQ-690W, 0.1 parts by weight of leveling agent UNIQ-495U, and 50 parts by weight of deionized water were mixed evenly and ground to a fineness of ≤10 μm to obtain a black color paste.
[0046] (2) A mixture consisting of 10 parts by weight of methyltrimethoxysilane, 3 parts by weight of phenyltrimethoxysilane, and 2 parts by weight of isopropanol was added to the black color paste prepared in step (1), and after mixing evenly, 0.2 parts by weight of formic acid was added, and stirred for 2 hours. Then, 4 parts by weight of the water-dispersible polyester-modified silicone prepared in Example 1 was added, and high-speed shear stirring was performed at 3000 rpm for 1 hour. After filtering, a flexible ceramic non-stick coating containing an aqueous high-temperature resistant toughening component was obtained.
[0047] Example 4
[0048] (1) 30 parts by weight of nano silica sol Levasil CT20DH, 15 parts by weight of red iron oxide, 45 parts by weight of aluminum oxide, 0.4 parts by weight of dispersant BYK-190, 0.2 parts by weight of BYK-333, 0.1 parts by weight of defoamer BYK-028, and 70 parts by weight of deionized water were mixed and evenly ground to a fineness of ≤10 μm to obtain a red color paste.
[0049] (2) A mixture consisting of 20 parts by weight of methyltriethoxysilane, 10 parts by weight of dimethyldimethoxysilane, 6 parts by weight of phenyltriethoxysilane, and 4 parts by weight of propylene glycol butyl ether was added to the red color paste prepared in step (1), and after mixing evenly, 0.4 parts by weight of acetic acid was added, and stirred for 5 hours. Then, 10 parts by weight of the water-dispersible polyester-modified silicone prepared in Example 2 was added, and high-speed shear stirring was performed at 3000 rpm for 0.5 hours. After filtering, a flexible ceramic non-stick coating containing an aqueous high-temperature resistant toughening component was obtained.
[0050] Example 5
[0051] (1) 25 parts by weight of nano silica sol Levasil CT8 DH, 15 parts by weight of phthalocyanine blue, 30 parts by weight of aluminum oxide, 0.3 parts by weight of dispersant AFCONA-4595, 0.1 parts by weight of leveling agent TEGO-450, 0.1 parts by weight of defoaming agent SURFYNOL-440, and 60 parts by weight of deionized water were mixed and evenly ground to a fineness of ≤10 μm to obtain a blue color paste.
[0052] (2) A mixture consisting of 20 parts by weight of methyltrimethoxysilane, 3 parts by weight of phenyltriethoxysilane, 2 parts by weight of diphenyldimethoxysilane, and 3 parts by weight of propylene glycol methyl ether acetate was added to the blue color paste prepared in step (1). After mixing evenly, 0.3 parts by weight of hydrochloric acid was added and stirred for 4 hours. Then, 6 parts by weight of the water-dispersible polyester-modified silicone prepared in Example 2 was added and stirred at 3000 rpm for 0.5 hours. The mixture was filtered to obtain a flexible ceramic non-stick coating containing an aqueous high temperature resistant toughening component.
[0053] Example 6
[0054] (1) 15 parts by weight of nano silica sol Levasil CT30 DH, 20 parts by weight of carbon black, 30 parts by weight of alumina, 0.3 parts by weight of dispersant UNIQ-690W, 0.2 parts by weight of leveling agent UNIQ-495U, 0.1 parts by weight of defoamer UNIQ-265W, and 60 parts by weight of deionized water were mixed evenly and ground to a fineness of ≤10 μm to obtain a black color paste.
[0055] (2) A mixture consisting of 15 parts by weight of methyltrimethoxysilane, 5 parts by weight of phenyltrimethoxysilane, and 3 parts by weight of isopropanol was added to the black color paste prepared in step (1), and after mixing evenly, 0.3 parts by weight of formic acid was added, and stirred for 4 hours. Then, 6 parts by weight of the water-dispersible polyester-modified silicone prepared in Example 1 was added, and high-speed shear stirring was performed at 3000 rpm for 0.5 hours. The flexible ceramic non-stick coating containing an aqueous high-temperature resistant toughening component was obtained by filtering.
[0056] Comparative Example 1
[0057] The only difference from Example 3 is that water-dispersible polyester-modified silicone is not added in step (2), and the remaining steps, materials and compositions are consistent with Example 3.
[0058] Comparative Example 2
[0059] The only difference from Example 3 is that in step (2), water-dispersible polyester-modified silicone is not added, but is replaced by the same weight portion of commercially available polyurethane emulsion, and the remaining steps, materials and composition are consistent with Example 3.
[0060] Comparative Example 3
[0061] The only difference from Example 3 is that in step (2), the water-dispersible polyester-modified silicone is first subjected to high-speed shear stirring at 3000 rpm in water for 1 hour before being added, and the remaining steps, materials and composition are consistent with Example 3.
[0062] Performance Testing
[0063] The flexible ceramic non-stick coatings containing water-based high temperature toughening components prepared in Examples 3-6 and the coatings prepared in Comparative Examples 1-3 were coated on aluminum substrates (the coating thickness was controlled to be 20 μm), and then their hardness, adhesion, heat resistance, impact resistance, recoatability and other properties were tested, wherein the hardness test was carried out according to GB / T 6739, and the results were evaluated as follows: the paint film was scratched; the adhesion test was carried out according to GB / T 9286, with a spacing of 2 mm; the heat resistance was measured according to the standard of GB / T 1735, and the test conditions were: 200°C*30min, and the results were evaluated as follows: the color difference ≤2 was qualified; the impact resistance test was carried out according to GB / T 1732, and it was qualified by passing the positive impact of 50 cm / kg; the recoatability test was carried out by grinding the ceramic coating with 1000 mesh sandpaper, and then spraying a layer of the same ceramic coating again, and testing the interlayer adhesion, and ≤1 level was qualified. The test results are shown in Table 1.
[0064] Table 1 Performance test results of products of Examples 3-6 and Comparative Examples 1-3:
[0065] hardness Adhesion Heat resistance Impact resistance Recoatability Example 3 6H Level 0 qualified qualified qualified Example 4 6H Level 0 qualified qualified qualified Example 5 6H Level 0 qualified qualified qualified Example 6 6H Level 0 qualified qualified qualified Comparative Example 1 6H Level 1 qualified Failure Failure Comparative Example 2 6H Level 0 Failure qualified qualified Comparative Example 3 6H Level 1 qualified qualified Failure
[0066] From the above data comparison, we can see that:
[0067] In Comparative Example 1, no toughening component, water-dispersible polyester modified silicone, was added, the adhesion of the ceramic coating decreased, and the impact resistance and recoatability were unqualified.
[0068] Comparative Example 2 uses commercially available polyurethane emulsion instead of water-dispersible polyester modified silicone, which can also achieve toughening effect, but the heat resistance is unsatisfactory.
[0069] In comparative example 3, the water-dispersible polyester modified silicone was first subjected to high-speed shear stirring at 3000 rpm in water for 1 hour before being added, which had a certain toughening effect. However, since it failed to form an effective three-dimensional composite with the inorganic network structure, the chain segments were entangled with each other, affecting the gradient self-stratification, and thus the recoatability was poor.
[0070] Compared with comparative examples 1-3, the flexible ceramic non-stick coatings containing aqueous high-temperature resistant toughening components of Examples 3-6 can not only maintain the original high-temperature resistance, high hardness and other properties of the ceramic coating, but also improve the flexibility of the coating and have excellent impact resistance. At the same time, the adhesion and recoating performance of the ceramic coating can be improved through the self-stratification phenomenon of the polyester segment and the silicone segment.
[0071] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0072] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. Application of water-dispersible polyester modified silicone in improving the recoating performance of flexible ceramic non-stick coatings on aluminum substrate surfaces, Features: The preparation method of the flexible ceramic non-stick coating comprises: (1) Mix 10-30 parts of nano silica sol, 40-60 parts of high temperature resistant pigments and fillers, 0.3-0.7 parts of additives, and 50-70 parts of water, and grind to obtain a color paste; (2) adding a mixture of 10-30 parts of methylsilane, 3-6 parts of phenylsilane, and 2-4 parts of solvent to the color paste, mixing evenly, adding 0.2-0.4 parts of acid catalyst, stirring, and then adding 4-10 parts of water-dispersible polyester modified silicone, shearing and stirring, filtering, and obtaining a flexible ceramic non-stick coating; The above raw materials are all parts by weight; The preparation of water-dispersible polyester-modified silicone is as follows: neopentyl glycol, trimethylolpropane and isophthalic acid are put into a reactor for esterification reaction, the temperature is lowered, propylene glycol butyl ether and trimellitic anhydride are added to continue the reaction, the temperature is lowered, tetrabutyl titanate and silicone intermediate are added, the reaction is carried out until transparent, the temperature is lowered, and N,N-dimethylethanolamine is added for neutralization.
2. The use according to claim 1, Features: The preparation method of the water-dispersible polyester-modified silicone comprises: adding 1-2 molar parts of neopentyl glycol, 2.5-6 molar parts of trimethylolpropane and 2-5 molar parts of isophthalic acid into a reaction kettle, heating to 170-185° C. for esterification for 1-2 hours, then heating to 210-225° C., continuing to react for 2-4 hours until the acid value drops below 10 mgKOH / g, stopping the reaction, cooling to 145-165° C., adding propylene glycol butyl ether and 0.7-1.5 molar parts of trimellitic anhydride, continuing to react until the acid value reaches 65-75 mgKOH / g, cooling to 105-115° C., adding tetrabutyl titanate and silicone intermediate, reacting for 1-2 hours until transparent, cooling to 70-80° C., and adding 1.2-2.5 molar parts of N,N-dimethylethanolamine for neutralization.
3. The use according to claim 2, Features: The amount of propylene glycol butyl ether is 50-60wt% of trimethylolpropane; The amount of tetrabutyl titanate is 0.05-0.1wt% of trimethylolpropane; The amount of the organosilicon intermediate used is 150-200wt% of trimethylolpropane.
4. The use according to any one of claims 1 to 3, Features: The methylsilane is selected from methyltrimethoxysilane, methyltriethoxysilane and dimethyldimethoxysilane.
5. The use according to any one of claims 1 to 3, Features: The phenylsilane is selected from phenyltrimethoxysilane, phenyltriethoxysilane and diphenyldimethoxysilane.
6. The use according to any one of claims 1 to 3, Features: The solvent is selected from isopropyl alcohol, propylene glycol butyl ether, and propylene glycol methyl ether acetate.
7. The use according to any one of claims 1 to 3, Features: The nano silica sol is acidic silica sol.
8. The use according to any one of claims 1 to 3, Features: The high temperature resistant color and filler are composed of a mixture of high temperature resistant pigment and high temperature resistant filler in any ratio.
9. The use according to any one of claims 1 to 3, Features: The auxiliary agent includes one or more of a dispersant, a leveling agent, and a defoaming agent.
Citation Information
Patent Citations
Flexible ceramic non-sticking coating composition and application method thereof
CN104059398A
Organic-silicon-modified aqueous polyester resin and preparation method of same
CN104829819A
Wearproof Teflon non-stick coating with good thermal conductivity
CN105295715A
High-thermal-conductivity and high-wear-resistance organosilicon non-stick coating
CN105602418A
Hydrophobic heat-resistant silicone modified polyester resin and preparation method thereof
CN106220838A