A preparation method for enhanced colored transparent wood
By delectin, oxidation and metal ion cross-linking treatment of wood, combined with hot pressing technology, color transparent wood without dyes and resin is prepared, which solves the problems of environmental protection and insufficient strength in the existing technology and achieves high transparency Preparation of colored transparent wood with lightness, mechanical strength and color uniformity has a wide range of application prospects.
Patent Information
- Application Number
- CN202310169062.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-02-27
AI Technical Summary
The existing transparent wood preparation methods destroy the natural degradability advantages of wood, and there are problems such as complex operation, harmful gas generation, uneven dyeing and insufficient mechanical strength. The traditional dye and resin impregnation process is not environmentally friendly.
By delignification, oxidation and metal ion cross-linking treatment of gas-dry wood, combined with hot pressing technology, colored transparent wood without dye dyeing and resin impregnation is prepared, and the wood strength is improved by washing with metal ion solutions and pure water. and color uniformity.
It has achieved green and environmentally friendly, low-cost, simple and easy-to-use high light transmittance, high mechanical strength and multi-color color transparent wood preparation, and can adjust the tensile strength, transparency and color depth through ion concentration, which has great application prospects.
Smart Images

Figure CN116277349B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of enhanced colored transparent wood. Background Art
[0002] Wood is a widely distributed natural renewable building material, which is widely used in construction, furniture, decoration and other fields. In order to increase the added value of wood, most of the methods used now are polymer impregnation or pore compression to modify the wood, improve its strength, and use wood dyeing technology to increase the added value of wood.
[0003] Transparent wood is the product of wood pore impregnation and compression modification. Wood transparency is to give wood light transmittance. In recent years, transparent wood has gradually entered the fields of building decoration due to its advantages such as biodegradability, anisotropic high light transmittance, and mechanical strength superior to native wood. The existing method for preparing transparent wood is mainly to impregnate wood with resin, etc., but this destroys the natural advantage of wood itself as a degradable material. Its preparation process will produce harmful gases, the operation is complicated, and there are certain requirements for polymer ratio, impregnation pressure, and curing temperature. In addition, in order to expand its scope of application, the mechanical strength of transparent wood also needs to be further enhanced.
[0004] From the perspective of wood dyeing, the existing dyeing technology is mostly to dye the veneer and then laminate it or directly dye the surface and inside of the wood. The process parameters such as dye concentration, ratio, dyeing temperature, time, and the amount of accelerator and fixative directly affect the dyeing effect of the wood. Secondly, synthetic dyes are highly toxic, have low utilization rates, and a large amount of waste liquid is difficult to degrade. The more environmentally friendly plant dyes have problems such as uneven dyeing.
[0005] Therefore, the development of a green, environmentally friendly, low-cost, simple and easy method for preparing enhanced colored wood with high light transmittance, excellent mechanical strength and multiple colors has huge market potential. Summary of the invention
[0006] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing enhanced colored transparent wood, which does not require dyeing and resin impregnation, is green and environmentally friendly, low cost, simple and easy to operate, and has the advantages of high light transmittance, uniform color, and high mechanical strength.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0008] A method for preparing enhanced colored transparent wood comprises delignifying air-dried wood, oxidizing the delignified wood and performing metal ion cross-linking treatment on the oxidized delignified wood. The metal ion cross-linking treatment is to put the oxidized delignified wood into a metal ion solution and soak it at room temperature for 12 to 96 hours. The mass ratio of metal ions to solution in the metal ion solution is 0.002 to 6:100.
[0009] As a preferred technical solution of the present invention, the metal ions are any one or a mixture of several water-soluble metal ions.
[0010] As a preferred technical solution of the present invention, the corresponding metal ion solution produces colored transparent wood of corresponding colors.
[0011] As a preferred technical solution of the present invention, the corresponding metal ion concentration will produce colored transparent wood with corresponding color effects.
[0012] As a preferred technical solution of the present invention, the strength of the corresponding ion-crosslinked colored transparent wood also changes accordingly.
[0013] A method for preparing enhanced colored transparent wood comprises the following steps:
[0014] (1) Weigh a certain amount of air-dried wood, place it in a 1 wt % sodium chlorite aqueous solution, adjust the pH to 4.6 with acetic acid, place it in an oil bath, perform delignification treatment on the wood at 80° C. and 200 rpm for 6 to 12 hours, take out the wood and wash the residual liquid thereon with pure water to obtain delignified wood;
[0015] (2) preparing 200 mL of a phosphate buffer solution with a pH of 6.8 containing 0.032 g of TEMPO, 2.26 g of sodium chlorite powder, and 0.6447 mL of a sodium hypochlorite solution with an effective chlorine content of 10%, and stirring to fully dissolve the mixture to obtain a reaction solution;
[0016] (3) preparing 200 mL of reaction solution per 1 g of wood, immersing the delignified wood in the reaction solution, reacting in an oil bath at 60 to 80° C. for 20 to 70 hours, and then washing away the residual solution with pure water to obtain oxidative delignified wood;
[0017] (4) 200 mL of 0.1-200 MM metal ion solution or a metal ion solution having a mass ratio of metal ions to solution of 0.002-6:100 is placed in 1 g of the original mass of oxidatively delignified wood, and the mixture is immersed at room temperature for 12-96 hours to obtain metal ion cross-linked wood;
[0018] (5) placing the metal ion cross-linked wood between two steel plates and hot pressing at 10 to 60 MPa and 30 to 100° C. for 1 to 36 hours;
[0019] (6) After the pressure is released and the steel plate is cooled, a colored transparent wood is obtained.
[0020] As a preferred technical solution of the present invention, the pure water is distilled water, and the water temperature is 10-80°C.
[0021] As a preferred technical solution of the present invention, the oxidized wood is placed between two steel plates by first pressurizing the oxidized wood between the two steel plates to 10-60 MPa, then heating it to 30-100° C., and maintaining hot pressing for 1-36 hours.
[0022] As a preferred technical solution of the present invention, the preparation order of the reaction solution is to first add sodium chlorite to the PBS buffer, add TEMPO powder after it is dissolved, and then add sodium hypochlorite to the solution after it is fully dissolved.
[0023] As a preferred technical solution of the present invention, the air-dried wood is coniferous wood, broad-leaved wood or bamboo, and has a moisture content of less than 12%.
[0024] Compared with the prior art, the present invention can achieve the following beneficial effects:
[0025] 1. The present invention uses chemical reagents to remove lignin from wood, then undergoes oxidation treatment, washes with pure water, and then is placed in a metal ion solution for cross-linking to improve strength and color, and then undergoes heat pressing to obtain enhanced colored transparent wood. The method of the present invention is simple and easy to implement, avoids the harm to the human body and environmental pollution caused by the volatilization of toxic substances during resin impregnation and curing and dye coloring, and has the advantages of being green and environmentally friendly, low cost, high light transmittance, uniform color, and high mechanical strength.
[0026] 2. The colored transparent wood prepared by the present invention can change the color of the wood by simply replacing the ion solution, and the color is uniform.
[0027] 3. The enhanced colored transparent wood prepared by the present invention can adjust the tensile strength, transparency and color depth of the multi-color wood by simply adjusting the ion concentration.
[0028] 4. The present invention first delignifies the wood, then oxidizes the delignified wood, and then washes the chemically treated wood with pure water and soaks it in an ion solution, and then performs hot pressing to obtain enhanced colored transparent wood. Taking poplar as an example, the tensile strength of the enhanced colored transparent poplar prepared by the method of the present invention is as high as 820MPa, which is increased by more than 8 times; according to Figure 3 The lowest value / log in Example 1 is 9 times, and the highest value is 13 times.
[0029] 5. The ionic solution used for cross-linking in the present invention is different from traditional wood dyes, does not contain toxic and difficult-to-handle organic dyes, and has the advantages of being easily recyclable and reusable.
[0030] 6. The enhanced colored transparent wood prepared by the present invention on the basis of multi-color, transparency and high strength has great application prospects in the field of architectural decoration. In addition to giving the transparent wood color and high strength, the incorporation of ions can also give the enhanced colored transparent wood a variety of additional functions such as sterilization, catalysis, shielding, and conductivity, and has great potential in the preparation of special functional building materials and even energy-saving heat storage, optoelectronics, batteries, smart devices and other aspects. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The transparent effect picture of the colored transparent wood prepared by the present invention;
[0032] Figure 2 Another color transparent wood transparent effect prepared by the present invention;
[0033] Figure 3 A comparison diagram of the improvement of the tensile strength of wood of the present invention and the prior art;
[0034] Figure 4 This is a comparison diagram of the adjustability of the metal ion concentration to the product strength of the present invention. DETAILED DESCRIPTION
[0035] In order to make the technical means, creative features, purpose and efficacy of the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments, but the following embodiments are only preferred embodiments of the present invention, not all. Based on the embodiments in the implementation mode, other embodiments obtained by those skilled in the art without creative work all belong to the protection scope of the present invention. The experimental methods in the following embodiments, unless otherwise specified, are conventional methods, and the materials, reagents, etc. used in the following embodiments, unless otherwise specified, can all be obtained from commercial channels.
[0036] like Figure 1As shown, Example 1: A method for preparing enhanced colored transparent wood, comprising the following steps: using poplar wood as raw material, cutting the size into 6*6cm, thickness into 0.8mm, weighing 7 pieces of the poplar wood, totaling 10g, the wood mass refers to the air-dried mass. Weighing 25g of sodium chlorite (80%) to prepare 2000mL of aqueous solution, adjusting the pH to 4.6 with acetic acid; putting the weighed poplar wood into the above solution, heating in an oil bath pot at 80℃, 200rmp / min for 9h, washing with pure water until the pH is neutral, the pure water is distilled water, and the washing water temperature is 50℃, to obtain delignified wood. Prepare 2000mL of phosphate buffered saline solution with a pH value of 6.8 containing 0.32g of TEMPO, 22.6g of sodium chlorite powder, and 6.447mL of sodium hypochlorite solution with an effective chlorine content of 10%, stir to fully dissolve, and obtain a reaction solution. The preparation order of the reaction solution is to first add sodium chlorite to the PBS buffer, add tempo powder after it is dissolved, and then add sodium hypochlorite to the solution after it is fully dissolved; prepare 200mL of reaction solution for every 1g of wood, immerse the delignified wood in the reaction solution, react in an oil bath at 60-80°C for 20-70h, and then wash away the residual liquid with pure water to obtain oxidized delignified wood; put the above oxidized delignified wood into 2000mL of an aqueous solution containing 1.62g of FeCl3, and soak it at room temperature for 96h to obtain metal ion cross-linked wood. The ion-impregnated wood is placed between two steel plates and hot-pressed at 60°C for 3 hours under 20 MPa. The hot pressing is to first pressurize the wood to densify it and then start heating. After the pressure is released and the steel plates are cooled, enhanced reddish-brown transparent wood is obtained.
[0037] Reinforced reddish brown transparent wood, after testing, its tensile strength is as high as 661MPa, the transmittance is 80%, the haze is 73%, and it is reddish brown.
[0038] Example 2: A method for preparing enhanced colored transparent wood, which is different from Example 1 in that: the oxidatively delignified wood is placed in 2000 mL of an aqueous solution containing 0.648 g of FeCl3 and soaked at room temperature for 96 hours; that is, the content of FeCl3 in the aqueous solution is reduced to 0.648 g; the remaining steps are the same as those in Example 1, so they are not repeated. Finally, enhanced brown-yellow transparent wood is obtained.
[0039] It can be seen that as the iron ion concentration decreases, the color of the colored wood changes from the reddish brown of Example 1 to the brownish yellow of this embodiment, and the macroscopic transparency is also improved. After testing, its tensile strength is as high as 820 MPa, the transmittance is 82%, and the haze is 70%.
[0040] Example 3: A method for preparing enhanced colored transparent wood, which is different from Example 1 in that: the oxidized wood is placed in 1920 mL of an aqueous solution containing 0.498 g of CoCl2 and soaked at room temperature for 96 hours; that is, the metal ions in the aqueous solution are replaced with CoCl2, with a content of 0.498 g; the remaining steps are the same as those in Example 1, so they are not repeated. Finally, enhanced pink transparent wood is obtained.
[0041] The test shows that its tensile strength is as high as 754MPa, the transmittance is 83%, the haze is 68%, and it is pink in color.
[0042] like Figure 2 As shown, Example 4: A method for preparing enhanced colored transparent wood comprises the following steps:
[0043] (1) Take bamboo as raw material, cut into pieces with a size of 6*1.5cm and a thickness of 0.8mm, weigh 10 pieces of the above bamboo pieces, totaling 3g; (2) Weigh 25g of sodium chlorite (80%) to prepare 2000mL of aqueous solution, and adjust the pH to 4.6 with acetic acid. (3) Put the weighed bamboo pieces into the above solution, heat them in an oil bath at 80℃ and 200rmp / min for 10h, and then wash them with pure water until the pH is neutral to obtain delignified bamboo. (4) Prepare 600mL of phosphate buffered saline solution with a pH of 6.8 containing 0.096g of TEMPO, 6.78g of sodium chlorite powder, and 1.93mL of sodium hypochlorite solution with 10% effective chlorine. The preparation order of the solution is to first add sodium chlorite to the PBS buffer, add tempo powder after it is dissolved, and then add sodium hypochlorite to the solution after it is fully dissolved, and stir to fully dissolve. (5) Place the above-mentioned delignified bamboo in the above-mentioned solution, react in an oil bath at 60°C for 24 hours, and then wash with distilled water. (6) Place the above-mentioned oxidized bamboo in 600mL of an aqueous solution containing 0.19g of FeCl3 and soak at room temperature for 72 hours. (7) Place the above-mentioned ion-soaked bamboo between two steel plates and hot press at 60°C for 3 hours under 10MPa. (8) After unloading the pressure and waiting for the steel plates to cool, a reinforced light yellow transparent bamboo is obtained.
[0044] The test shows that its tensile strength is as high as 815MPa, the transmittance is 83%, the haze is 65%, and it is light yellow.
[0045] like Figure 3 As shown, it is a comparative diagram of the improvement of the tensile strength of the transparent wood prepared in Examples 1 to 3 of the present invention and the original wood, which illustrates that the tensile strength of the enhanced colored transparent poplar wood prepared by the method of the present invention is improved by more than 6 times compared with the original wood.
[0046] like Figure 4As shown, the adjustability of the metal ion concentration in the transparent wood prepared in Examples 1 to 3 of the present invention to the product strength, and the strength of the corresponding ion-crosslinked colored transparent wood also changes accordingly. The metal ion is any one or a mixture of several water-soluble metal ions. The mass ratio of the metal ion to the solution in the metal ion solution can be in the range of 0.002 to 6:100.
[0047] The corresponding metal ion solution produces colored transparent wood of the corresponding color. The corresponding metal ion concentration will produce colored transparent wood with the corresponding color effect. For example, when the concentration of FeCl3 metal ion aqueous solution is high, enhanced reddish brown transparent wood will be obtained; when the concentration of FeCl3 aqueous solution is reduced, enhanced light yellow transparent wood will be obtained; and the metal ion aqueous solution of CoCl2 will eventually obtain enhanced pink transparent wood.
[0048] The tensile strength data of the transparent wood prepared by each embodiment of the present invention, the existing common transparent materials and the existing transparent wood are as follows:
[0049]
[0050] The above index data show that the tensile strength (MPa) index of the colored transparent wood prepared by the present invention is better than various indexes of common transparent materials and some publicly available transparent woods. The tensile strength (MPa) of the colored transparent wood prepared by the present invention is more than 3 times that of sapphire, and more than 4 times that of some existing transparent woods.
[0051] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing enhanced colored transparent wood, characterized in that: The steps include: (1) Weigh a certain amount of air-dried wood, place it in a 1 wt % sodium chlorite aqueous solution, adjust the pH to 4.6 with acetic acid, place it in an oil bath, perform delignification treatment on the wood at 80° C. and 200 rpm for 6 to 12 hours, take out the wood and wash the residual liquid thereon with pure water to obtain delignified wood; (2) preparing 200 mL of a phosphate buffer solution with a pH of 6.8 containing 0.032 g of TEMPO, 2.26 g of sodium chlorite powder, and 0.6447 mL of a sodium hypochlorite solution with an effective chlorine content of 10%, and stirring to fully dissolve the mixture to obtain a reaction solution; The preparation order of the reaction solution is to first add sodium chlorite to the PBS buffer, add TEMPO powder after it is dissolved, and then add sodium hypochlorite to the solution after it is fully dissolved; (3) preparing 200 mL of reaction solution per 1 g of wood, immersing the delignified wood in the reaction solution, reacting in an oil bath at 60 to 80° C. for 20 to 70 hours, and then washing away the residual solution with pure water to obtain oxidative delignified wood; (4) 200 mL of 0.1-200 MM metal ion solution is placed per 1 g of the original mass of oxidative delignified wood, wherein the mass ratio of metal ions to solution in the metal ion solution is 0.002-6:100, and the wood is immersed at room temperature for 12-96 hours to obtain metal ion cross-linked wood; The metal ion solution is an aqueous solution of CoCl2 and FeCl3; the corresponding metal ion solution produces colored transparent wood of corresponding color, the corresponding metal ion concentration produces colored transparent wood of corresponding color effect, and the strength of the corresponding ion-crosslinked colored transparent wood also changes accordingly; (5) placing the metal ion cross-linked wood between two steel plates and hot pressing at 10 to 60 MPa and 30 to 100° C. for 1 to 36 hours; (6) After the pressure is released, the steel plate is cooled to obtain colored transparent wood; The pure water is distilled water, and the water temperature is 10-80°C; The oxidized wood is placed between two steel plates, and the oxidized wood between the two steel plates is firstly pressurized to 10-60 MPa, and then heated to 30-100° C. and kept hot pressed for 1-36 hours.
2. The method according to claim 1, characterized in that: The air-dried wood is coniferous wood, broad-leaved wood or bamboo, and has a moisture content of less than 12%.