A method for preparing hard carbon using polyvinyl chloride waste, coal tar and its fractions and its application
By reacting polyvinyl chloride waste and coal tar fractions under specific conditions to prepare hard carbon materials, we solve the problems of polyvinyl chloride waste treatment and coal tar refining and separation, and achieve high value-added utilization and excellent performance of hard carbon materials. Suitable for applications such as sodium-ion batteries.
Patent Information
- Application Number
- CN202310397038.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-04-13
AI Technical Summary
PVC waste treatment is difficult, and the coal tar refining and separation process is complex and energy-consuming, resulting in resource waste and environmental pollution, and a lack of high value-added utilization methods.
By reacting polyvinyl chloride waste with coal tar and its fractions under specific conditions, hard carbon materials are prepared, and dechlorination agents and surfactants are used for mixing, stirring, washing and heating to obtain high value-added hard carbon materials. .
It achieves efficient clean recovery of polyvinyl chloride waste and high value-added utilization of coal tar fractions. The prepared hard carbon material has excellent performance and is suitable for applications such as sodium-ion batteries. The process is simple and low-cost.
Smart Images

Figure CN116281949B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to a method and application of preparing hard carbon by utilizing polyvinyl chloride waste and coal tar and fractions thereof. Background Art
[0002] Polyvinyl chloride is the third largest resin product after polyethylene and polypropylene. It is widely used in industries such as construction, packaging and furniture. The treatment of a large amount of polyvinyl chloride waste has attracted widespread attention from countries around the world. At present, there are three main methods for treating organic solid waste such as plastics: landfill, incineration and mechanical recycling. Landfill treatment will waste precious land resources, and because plastics such as PVC are generally light and not easy to rot, the degradation time is long, and the degradation products will pollute the soil. When incineration is used, PVC plastics will also release harmful gases and pollute the atmosphere. When recycling and reuse methods are used, it is labor-intensive, the recycling cost is high, and there is a lack of corresponding recycling channels. At present, recycling and reuse in the world only accounts for about 15% of the total plastic consumption. However, due to the limited world oil resources, from the perspective of saving earth resources, the recycling and reuse of plastics is of great significance. To this end, countries around the world are currently investing a lot of manpower and material resources to develop key technologies for the recycling and utilization of various waste plastics, and are committed to reducing the cost of plastic recycling and developing its suitable application fields. Polyvinyl chloride waste is a halogenated hydrocarbon reaction precursor with excellent reactivity. At the same time, in the coal chemical industry, coal tar, the main by-product of coking, can be fractionated to obtain washing oil, anthracene oil, and naphthalene oil. It has the characteristics of high aromaticity, low price, and high carbon yield. However, due to its complex composition, its application is currently usually limited to low-value-added aspects such as wood preservative oil, burning carbon black, or directly used as fuel oil combustion. Its high-value-added utilization, such as use as fragrances, pharmaceutical intermediates, and dyes, requires separation and refinement of coal tar into fine chemicals. However, the refining and separation process of coal tar is complex and energy-intensive, and the product fine chemicals are small in scale and dispersed in variety. The three wastes generated in the process pollute the environment. Therefore, it is crucial to find a way to achieve high-value-added utilization by initially separating coal tar.
[0003] Therefore, the present invention utilizes the many characteristics of polyvinyl chloride and coal tar and its fractions, and proposes a method for preparing a high-value-added hard carbon material using polyvinyl chloride waste. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing hard carbon by using polyvinyl chloride waste and coal tar and its fractions and its application.
[0005] The object of the present invention is to achieve the following:
[0006] A method for preparing hard carbon using polyvinyl chloride waste and coal tar and its fractions, which mainly comprises the following steps:
[0007] The polyvinyl chloride waste is crushed into particles of 1-4 mm, added to the reaction solvent with a dechlorinating agent, a surfactant is added and magnetic stirring is performed for a period of time to fully mix the materials, coal tar or its fraction is added after mixing evenly, and after reacting at a certain temperature for a period of time, a hard carbon precursor is obtained, which is washed, filtered, dried, and heated at a certain temperature under inert gas conditions to obtain a hard carbon material.
[0008] Furthermore, the coal tar or its fraction is selected from one or a mixture of two or more of coal tar, wash oil, anthracene oil and naphthalene oil.
[0009] Furthermore, the reaction solvent is one of dichloromethane, carbon disulfide, 1,2-dichloroethane, chloroform or carbon tetrachloride.
[0010] Furthermore, the dechlorinating agent is one of ferric chloride, aluminum chloride, zinc chloride, concentrated sulfuric acid or p-toluenesulfonic acid.
[0011] Furthermore, the surfactant is one of polyacrylamide, methyl cellulose or hydroxypropyl methyl cellulose.
[0012] Furthermore, the mass ratio of the polyvinyl chloride waste to the coal tar or its fraction is 1:2 to 1:5.
[0013] Furthermore, the mass ratio of the polyvinyl chloride waste to the dechlorinating agent is 1:10 to 1:20.
[0014] Furthermore, the mass ratio of the polyvinyl chloride waste to the reaction solvent is 1:160 to 1:400.
[0015] Furthermore, the mass ratio of the polyvinyl chloride waste to the surfactant is 1:0-5.
[0016] Furthermore, the magnetic stirring time is 1-4h, and the rotation speed is 200-500r / min.
[0017] Furthermore, the reaction temperature is 60-120° C., and the reaction time is 4-8 h.
[0018] Furthermore, the drying temperature is 50-100° C. in vacuum, and the drying time is 6-24 hours.
[0019] Furthermore, the inert gas is one of nitrogen, argon and helium.
[0020] Furthermore, the inert gas flow rate is 50-250 mL min -1 .
[0021] Furthermore, the heating temperature is 800-1600°C; the heating rate is 2-10°C min -1 .
[0022] Furthermore, the heating time is 1-20h.
[0023] Another aspect of the present invention is to provide a hard carbon material prepared by the above method, wherein the d002 value of the hard carbon material is greater than 0.37 nm.
[0024] Another aspect of the present invention is to provide the use of the hard carbon material.
[0025] Furthermore, the hard carbon material can be applied to electrode materials of sodium ion batteries, lithium ion batteries and potassium ion batteries.
[0026] The beneficial effects of the present invention are as follows: a method is provided for preparing a hard carbon precursor by using coal tar fraction and polyvinyl chloride waste as raw materials under the action of a dechlorinating agent, and preparing a hard carbon material by heating. The preparation method provides a new perspective for the high-value utilization of polyvinyl chloride and coal tar fractions, can realize the high added value utilization of coal tar fractions and can efficiently and cleanly recycle waste polyvinyl chloride plastics, the preparation method is simple, the yield is high, the preparation process cost is low, and the prepared hard carbon material has excellent performance when applied to the negative electrode material of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.
[0028] Figure 1 This is the XRD spectrum of sample WO-1500-2h prepared in Example 7.
[0029] Figure 2 This is the sodium electrical cycling performance diagram of sample WO-1500-2h prepared in Example 7. DETAILED DESCRIPTION
[0030] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0031] Example 1
[0032] At room temperature, 0.75g of polyvinyl chloride waste particles (1-4mm) and 7.7g of ferric chloride were dissolved in 100mL of 1,2-dichloroethane and placed in a 250mL three-necked flask. 0.75g of polyacrylamide was added to the three-necked flask and magnetically stirred at a speed of 200r / min for 1h until completely dissolved. Then 1.5g of washing oil (WO) was added to the three-necked flask under a nitrogen atmosphere, and the temperature was raised to 80°C and heated and stirred for 6h. After the reaction was completed, the solid product was filtered and then washed with methanol and tetrahydrofuran respectively until the washing liquid was colorless and transparent, filtered, and finally dried at 80°C in a vacuum oven for 12h to obtain the reaction product. The reaction product was ground into powder, 1g was taken in a graphite boat, and the graphite boat was placed in a tube furnace at 80mL min -1 Under argon atmosphere, at 8℃min -1 The temperature was raised to 800°C at a heating rate of 1 °C, maintained for 1 h and then naturally cooled to obtain a hard carbon material.
[0033] Example 2
[0034] At room temperature, 0.75g of polyvinyl chloride waste particles (1-4mm) and 8.25g of aluminum trichloride were dissolved in 120mL of carbon disulfide and placed in a 250mL three-necked flask. 1.5g of methyl cellulose was added to the three-necked flask and magnetically stirred at a speed of 300r / min for 2h until completely dissolved. Then 2.25g of coal tar was added to the three-necked flask under a nitrogen atmosphere, and the temperature was raised to 60°C and heated and stirred for 4h. After the reaction was completed, the solid product was filtered and then washed with methanol and tetrahydrofuran respectively until the washing liquid was colorless and transparent, filtered, and finally dried in a vacuum oven at 50°C for 6h to obtain the reaction product. The reaction product was ground into powder, 1g was taken in a graphite boat, and the graphite boat was placed in a tube furnace at 50mL min -1 In a nitrogen atmosphere, the temperature was 10 °C min -1 The temperature was raised to 1100°C at a heating rate of , maintained for 4 h and then naturally cooled to obtain a hard carbon material.
[0035] Example 3
[0036] At room temperature, 0.75g of polyvinyl chloride waste particles (1-4mm) and 9g of zinc trichloride were dissolved in 140mL of dichloromethane and placed in a 250mL three-necked flask. 2.25g of hydroxypropyl methylcellulose was added to the three-necked flask and magnetically stirred at a speed of 400r / min for 2h until completely dissolved. Then 3g of anthracene oil (AO) was added to the three-necked flask. Under a nitrogen atmosphere, the temperature was raised to 70°C and heated and stirred for 5h. After the reaction was completed, the solid product was filtered and then washed with methanol and tetrahydrofuran respectively until the washing liquid was colorless and transparent, filtered, and finally dried at 70°C in a vacuum oven for 8h to obtain the reaction product. The reaction product was ground into powder, 1g was taken in a graphite boat, and the graphite boat was placed in a tube furnace at 100mL min -1 In an argon atmosphere, the temperature was 6 °C min -1 The temperature was raised to 1500°C at a heating rate of , maintained for 8 h and then naturally cooled to obtain a hard carbon material.
[0037] Example 4
[0038] At room temperature, 0.75g of polyvinyl chloride waste particles (1-4mm) and 9.75g of concentrated sulfuric acid were dissolved in 160mL of chloroform, placed in a 250mL three-necked flask, and 2.25g of hydroxypropyl methylcellulose was added to the three-necked flask, and magnetic stirring was performed at a speed of 500r / min for 1h until it was completely dissolved, and then 3.75g of naphthalene oil (NO) was added to the three-necked flask, and the temperature was raised to 90°C and heated and stirred for 7h under a nitrogen atmosphere. After the reaction was completed, the solid product was filtered and then washed with methanol and tetrahydrofuran respectively until the washing liquid was colorless and transparent, filtered, and finally dried at 90°C in a vacuum oven for 14h to obtain the reaction product. The reaction product was ground into powder, 1g was taken in a graphite boat, and the graphite boat was placed in a tube furnace at 150mL min -1 In a helium atmosphere, the temperature was 5 °C min -1 The temperature was raised to 1400°C at a heating rate of 1000 °C, maintained for 12 h and then naturally cooled to obtain a hard carbon material.
[0039] Example 5
[0040] At room temperature, 0.75g of polyvinyl chloride waste particles (1-4mm) and 10.5g of p-toluenesulfonic acid were dissolved in 180mL of carbon tetrachloride, placed in a 250mL three-necked flask, and 3g of methyl cellulose was added to the three-necked flask, and magnetic stirring was performed at a speed of 400r / min for 2h until it was completely dissolved, and then 2.25g of washing oil (WO) was added to the three-necked flask, and the temperature was raised to 100°C and heated and stirred for 8h under a nitrogen atmosphere. After the reaction was completed, the solid product was filtered and then washed with methanol and tetrahydrofuran respectively until the washing liquid was colorless and transparent, filtered, and finally dried in a vacuum oven at 100°C for 17h to obtain the reaction product. The reaction product was ground into powder, 1g was taken in a graphite boat, and the graphite boat was placed in a tube furnace at 200mL min -1 In a helium atmosphere, at 4 °C min -1 The temperature was raised to 1600°C at a heating rate of 1000 °C, maintained for 16 h and then naturally cooled to obtain a hard carbon material.
[0041] Example 6
[0042] At room temperature, 0.75g of polyvinyl chloride waste particles (1-4mm) and 13g of ferric chloride were dissolved in 140mL of 1,2-dichloroethane and placed in a 250mL three-necked flask, and 3.75g of polyacrylamide was added to the three-necked flask, and magnetic stirring was performed at a speed of 300r / min for 4h until it was completely dissolved, and then 3g of naphthalene oil (NO) was added to the three-necked flask, and the temperature was raised to 120°C and heated and stirred for 5h under a nitrogen atmosphere. After the reaction was completed, the solid product was filtered and then washed with methanol and tetrahydrofuran respectively until the washing liquid was colorless and transparent, filtered, and finally dried in a vacuum oven at 60°C for 20h to obtain the reaction product. The reaction product was ground into powder, 1g was taken in a graphite boat, and the graphite boat was placed in a tube furnace at 220mL min -1 In a nitrogen atmosphere, the temperature was 2 °C min -1 The temperature was raised to 1300°C at a heating rate of , maintained for 20 h and then naturally cooled to obtain a hard carbon material.
[0043] Example 7
[0044] At room temperature, 0.75g of polyvinyl chloride waste particles (1-4mm) and 7.7g of ferric chloride were dissolved in 100mL of 1,2-dichloroethane, placed in a 250mL three-necked flask, and magnetically stirred at 450r / min for 1h until completely dissolved. Then 1.5g of washing oil (WO) was added to the three-necked flask, and the temperature was raised to 80°C and heated and stirred for 6h under a nitrogen atmosphere. After the reaction was completed, the solid product was filtered and then washed with methanol and tetrahydrofuran respectively until the washing liquid was colorless and transparent, filtered, and finally dried in a vacuum oven at 80°C for 12h to obtain the reaction product. The reaction product was ground into powder, 1g was taken in a graphite boat, and the graphite boat was placed in a tubular furnace at 50mL min -1 In an argon atmosphere, the temperature was 5 °C min -1 The temperature was raised to 1500°C at a heating rate of 1500°C, maintained for 2 h and then naturally cooled to obtain a hard carbon material, which was recorded as WO-1500-2h.
[0045] Example 8
[0046] At room temperature, 0.75g of polyvinyl chloride waste particles (1-4mm) and 15g of p-toluenesulfonic acid were dissolved in 200mL of carbon disulfide and placed in a 250mL three-necked flask, and 1.5g of polyacrylamide was added to the three-necked flask, and magnetic stirring was carried out at a speed of 200r / min for 3h until it was completely dissolved, and then 1.5g of anthracene oil (AO) was added to the three-necked flask, and the temperature was raised to 110°C and heated and stirred for 6h under a nitrogen atmosphere. After the reaction was completed, the solid product was filtered and then washed with methanol and tetrahydrofuran respectively until the washing liquid was colorless and transparent, filtered, and finally dried in a vacuum oven at 80°C for 24h to obtain the reaction product. The reaction product was ground into powder, 1g was taken in a graphite boat, and the graphite boat was placed in a tube furnace at 250mL min -1 Under argon atmosphere, at 4℃min -1 The temperature was raised to 1300°C at a heating rate of , maintained for 2 h and then naturally cooled to obtain a hard carbon material.
[0047] Application Example 1
[0048] The sample prepared in Example 7, acetylene black and polyvinylidene fluoride were weighed in a mass ratio of 8:1:1 and placed in a mortar. N-methylpyrrolidone was used as a solvent and added into the mortar for grinding to make it evenly mixed. Then, the ground slurry was evenly coated on the copper foil with a scraper. The thickness of the coating was 50 μm. The coated film was placed in a vacuum oven and dried at 120° C. for 12 h. After drying, it was cut into discs with a diameter of 14 mm using a punching machine as the working electrode. The battery shell model was CR2016, 1M NaClO4, and a mixed solution of EC:DEC=1:1vol.% was used as the electrolyte. Whatman GF / D glass fiber was used as a diaphragm. The working electrode was used as the negative electrode material. Metal sodium was cut into discs with a diameter of 18 mm as the counter electrode, and the thickness of the gasket was 0.8 mm. The assembly process is as follows: first place the positive electrode battery shell, drip a drop of electrolyte, then put in the negative electrode material and add two drops of electrolyte, put in the diaphragm and add an appropriate amount of electrolyte, put in the cut sodium sheet, gasket, and battery negative electrode shell in turn, put the assembled battery into the battery sealing machine for packaging, and the assembled sodium ion battery is obtained. The sodium ion battery is electrochemically tested, and the electrochemical test results are shown in the attached Figure 2 As shown, at 30mA g -1 At a current density of 1.3 Å, the material's first reversible capacity is as high as 317.7 mA h g -1 The first coulombic efficiency can reach 70.83%, and after 100 cycles, there is still 284.45mA hg -1 , the capacity retention rate is as high as 89.53%.
Claims
1. A method for preparing hard carbon using polyvinyl chloride waste and coal tar and its fractions, characterized in that: The following steps are involved: The polyvinyl chloride waste is crushed into particles of 1-4 mm, added to the reaction solvent with a dechlorinating agent, a surfactant is added and magnetic stirring is performed for a period of time to fully mix the materials, coal tar or its fraction is added after mixing evenly, and after reacting at a certain temperature for a period of time, a hard carbon precursor is obtained, which is washed, filtered, dried, and heated at a certain temperature under inert gas conditions to obtain a hard carbon material.
2. The method for preparing hard carbon from polyvinyl chloride waste and coal tar and its fractions according to claim 1, characterized in that: The coal tar or its fraction is selected from one or a mixture of two or more of coal tar, washing oil, anthracene oil and naphthalene oil; the reaction solvent is one of dichloromethane, carbon disulfide, 1,2-dichloroethane, chloroform or carbon tetrachloride; the dechlorinating agent is one of ferric chloride, aluminum chloride, zinc chloride, concentrated sulfuric acid or p-toluenesulfonic acid; the surfactant is one of polyacrylamide, methyl cellulose or hydroxypropyl methyl cellulose.
3. The method for preparing hard carbon from polyvinyl chloride waste and coal tar and its fractions according to claim 1, characterized in that: The mass ratio of the polyvinyl chloride waste to coal tar or its fraction is 1:2-1:5; the mass ratio of the polyvinyl chloride waste to the dechlorinating agent is 1:10-1:20; the mass ratio of the polyvinyl chloride waste to the reaction solvent is 1:160-1:400; and the mass ratio of the polyvinyl chloride waste to the surfactant is 1:0-5.
4. The method for preparing hard carbon from polyvinyl chloride waste and coal tar and its fractions according to claim 1, characterized in that: The magnetic stirring time is 1-4h, and the rotation speed is 200-500r / min.
5. The method for preparing hard carbon from polyvinyl chloride waste and coal tar and its fractions according to claim 1, characterized in that: The reaction temperature is 60-120° C., and the reaction time is 4-8 hours.
6. The method for preparing hard carbon from polyvinyl chloride waste and coal tar and its fractions according to claim 1, characterized in that: The drying temperature is 50-100° C. in vacuum, and the drying time is 6-24 hours.
7. The method for preparing hard carbon from polyvinyl chloride waste and coal tar and its fractions according to claim 1, characterized in that: The inert gas is one of nitrogen, argon and helium; the inert gas flow rate is 50-250 mL / min -1 .
8. The method for preparing hard carbon from polyvinyl chloride waste and coal tar and its fractions according to claim 1, characterized in that: The heating temperature is 800-1600°C; the heating rate is 2-10°C min -1 ; The heating time is 1-20h.
9. The hard carbon material obtained by the method for preparing hard carbon using polyvinyl chloride waste and coal tar and its fractions as claimed in any one of claims 1 to 8, characterized in that: The d002 value of the hard carbon material is greater than 0.37 nm.
10. Use of a hard carbon material obtained by the method for preparing hard carbon using polyvinyl chloride waste and coal tar and its fractions as claimed in any one of claims 1 to 8, characterized in that: The hard carbon material is applied to electrode materials of sodium ion batteries, lithium ion batteries and potassium ion batteries.