A method for preparing arc protection coating fabric
By depositing white inorganic powder on the surface of expandable graphite and combining it with a polymer matrix, an arc protective coating is prepared, which solves the problems of damage and color inconsistency in existing arc protective clothing at high temperatures, and achieves efficient heat insulation and arc protection properties. improvement.
Patent Information
- Application Number
- CN202310336431.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing arc protective clothing is damaged at high temperatures and easily broken, and the color of the expandable graphite coating material does not meet the clothing requirements, making it unable to provide efficient protection against arc deflagration accidents.
Deposit white inorganic powders such as titanium dioxide and titanium hydroxide on the surface of expandable graphite to form white inorganic matter coating the expandable graphite, and mix it with the polymer matrix to prepare an arc protective coating to improve the thermal insulation performance and arc protection of the fabric. ability.
It achieves efficient heat insulation and arc protection of fabrics at high temperatures, and can produce coatings of various colors as needed, improving arc protection performance and color compliance.
Smart Images

Figure BDA0004156596120000061
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing arc protection coating fabric, and belongs to the technical field of arc protection fabrics. Background Art
[0002] Arc flashover accidents are one of the serious threats that power workers cannot avoid when working. Arc flashover accidents release large amounts of energy and high temperatures, often causing deep burns to the skin of power workers, leading to casualties among power workers. Anti-arc clothing is the most important protective equipment in arc flashover accidents, which can effectively reduce the damage caused by arc flashover to the human body.
[0003] The main material of arc protection clothing is intrinsically flame-retardant fabric composed of permanent flame-retardant fibers such as aramid 1313, aramid 1414, and flame-retardant nitrile chlorofiber. This type of fabric has high air permeability, poor windproof performance in cold weather, low rainproof performance, and low protective performance. The invention patent "Arc Flash Protection Material" with application number 2021800206394 and the invention patent "Expandable Graphite Modifier and Preparation Method and Application in Thermal Protection Fabric" with application number 2020103185151 both use expandable graphite and polymer composite system as the thermal insulation layer behind the fabric or between two layers of fabric, which can effectively improve the thermal insulation performance of the material. However, the surface fabric of such material has been damaged at high temperature, resulting in strength loss, and it is easy to rupture under the action of arc shock wave, resulting in its low rupture threshold energy. In addition, expandable graphite is a black powder, and the coating material containing expandable graphite is black, which often does not meet the color requirements of clothing. Summary of the invention
[0004] In view of the above problems, the present invention discloses an arc protection coating fabric and a preparation method thereof. First, inorganic powders such as titanium dioxide, titanium hydroxide, zinc oxide, zinc hydroxide, and calcium sulfate are deposited on the surface of expandable graphite to prepare white inorganic coated expandable graphite, and then the material is mixed with a polymer matrix and a pigment to coat the fabric to form an arc protection fabric. Not only can coatings of various colors be produced according to requirements, but the coating can also expand to form an effective heat insulation layer after being heated. At the same time, the expandable graphite with inorganic materials deposited on the surface also has a higher initial expansion rate, which can provide more effective protection against arc hazards.
[0005] The first object of the present invention is to provide an arc protection fabric, which comprises a base fabric and a coating, wherein the coating comprises expandable graphite and a polymer matrix, wherein the polymer matrix bonds the expandable graphite to the base fabric so that the expandable graphite is located on the outer surface of the base fabric; the base fabric comprises poly(m-phenylene isophthalamide) fiber, acrylonitrile-vinyl chloride copolymer flame-retardant fiber, low heat shrinkage fiber, permanent flame-retardant cellulose fiber and conductive fiber.
[0006] In one embodiment of the present invention, the mass percentages of the fibers in the base fabric are: 35-55% poly(m-phenylene isophthalamide) fiber, 20-35% acrylonitrile-vinyl chloride copolymer flame retardant fiber, 10-15% low heat shrinkage fiber, 25-45% permanent flame retardant cellulose fiber and 0.5-2% conductive fiber.
[0007] In one embodiment of the present invention, the low heat shrinkage fiber is one or more mixed fibers of poly(p-phenylene benzobisoxazole) fiber (PBO fiber), poly(p-benzimidazole) fiber (PBI fiber), poly(phenylene pyridine diimidazole) fiber (M5 fiber), polyimide fiber (PI fiber), and poly(p-phenylene terephthalamide) (PPTA fiber).
[0008] In one embodiment of the present invention, the permanent flame retardant cellulose fiber is a silicon-based flame retardant viscose fiber with a fineness of 1.5-1.7 dtex and a length of 51 mm.
[0009] In one embodiment of the present invention, the conductive fiber is a nylon-based filament fiber added with conductive carbon black, the fiber bundle fineness is 20D, and the number of fibers in the fiber bundle is 1-6.
[0010] In one embodiment of the present invention, the expandable graphite has a mesh size of 200-350 meshes.
[0011] In one embodiment of the present invention, the expandable graphite is common expandable graphite or modified expandable graphite with white inorganic substances deposited on the surface.
[0012] In one embodiment of the present invention, the modified expandable graphite refers to white inorganic substances such as titanium dioxide, titanium hydroxide, zinc oxide, zinc hydroxide, and calcium sulfate deposited on the surface of ordinary expandable graphite.
[0013] In one embodiment of the present invention, titanium hydroxide is deposited on the surface of expandable graphite by hydrothermal method, and the content of titanium hydroxide is 5%-8.5%, wt%; its preparation method is: expandable graphite is added to water, and a homogeneous dispersion is prepared by ultrasonic dispersion method, and heated to 60-100°C. At the same time, 10-20g / L of titanium sulfate, titanium oxysulfate, titanium chloride, titanium chloride and other titanium salt solutions and ammonia, (NH4)2CO3, Na2CO3, NaOH and other alkaline precipitants are respectively prepared, and the titanium salt solution and the precipitant are simultaneously added dropwise to the graphite dispersion, and the pH is kept constant between 1-4 during the titration process to prevent the product from agglomerating due to excessive hydrolysis. As the titanium salt is continuously hydrolyzed, the hydrolysis product Ti(OH)4 is continuously precipitated and attached to the graphite surface.
[0014] In one embodiment of the present invention, the polymer matrix used as the adhesive includes polyurethane, polyvinyl chloride, polyacrylate, and rubber.
[0015] In one embodiment of the present invention, the polyurethane is a moisture-curable polyurethane.
[0016] In one embodiment of the present invention, the mass ratio of expandable graphite to moisture-curable polyurethane in the coating is (1-2):(3-5), wherein the expandable graphite greater than this ratio will result in a greater hardness of the fabric, and the effect is not obvious below this ratio.
[0017] In one embodiment of the present invention, the coating uses DMF as a solvent, wherein the mass ratio of expandable graphite, moisture-curable polyurethane and DMF is 5-10:15-25:60-80; when DMF is lower than this ratio, the coating liquid has high viscosity and poor fluidity, and when it is higher than this ratio, it is easy to cause excessive difference between the inside and outside of the coating when curing.
[0018] In one embodiment of the present invention, the coating has a thickness of 50-70 μm.
[0019] The second object of the present invention is to provide a method for preparing the above arc protection fabric, wherein the coating process is as follows:
[0020] (1) calendering the coated surface of the base fabric;
[0021] (2) Plasma treatment of the coating surface;
[0022] (3) scraping coating agent;
[0023] (4) solidifying in a coagulation bath, wherein the coagulation bath is a 15-25% DMF solution and the coagulation temperature is 25-40° C.;
[0024] (5) Drying the coated fabric to obtain arc protection fabric.
[0025] In one embodiment of the present invention, the mass ratio of expandable graphite, moisture-curable polyurethane and DMF in the coating agent is 5-10:15-25:60-80; wherein, if the expandable graphite is greater than this ratio, the fabric will be harder, and if it is lower than this ratio, the effect is not obvious; if DMF is lower than this ratio, the coating liquid has high viscosity and poor fluidity, and if it is higher than this ratio, it is easy to cause excessive difference between the inside and outside of the coating when curing.
[0026] In one embodiment of the present invention, the base fabric processing process is as follows:
[0027] (1) Spray the antistatic agent aqueous solution on the meta-aramid fiber, and store it in a sealed container for 24-48 hours after spraying the antistatic treatment agent;
[0028] (2) mixing poly(m-phenylene isophthalamide) fiber, acrylonitrile-vinyl chloride copolymer fiber, low heat shrinkage fiber, and permanent flame retardant cellulose fiber according to a set ratio, and combing them into fiber strips (the weight ratios are all calculated based on dry weight);
[0029] (3) feeding the fiber strips into the drawing frame, and combining the three passes to form mature strips;
[0030] (4) the warp and weft of arc protection fabric are made by roving, spun yarn, winding, doubling and twisting, and the warp and weft specifications are 15-30tex×2 strands;
[0031] (5) The conductive composite yarn is embedded at intervals by warp and weft weaving, wherein the conductive composite yarn is formed by combining the above-mentioned strands with 1-4 bundles of 20D conductive yarn bundles, wherein the embedding method is to implant one strand at an interval of 5-10 mm in the warp direction and to weave one strand at an interval of 5-10 mm in the weft direction;
[0032] (6) The yarn is wound through a tube, warped, sizing, drawn in, and weaved to form the base fabric.
[0033] Beneficial effects of the present invention:
[0034] (1) The low heat shrinkage fiber shrinks less after being heated by the arc explosion. The low heat shrinkage fiber is added at 10-15%. It can be used as the skeleton material of the fabric to make the fabric have higher thermal stability. The thermal stability of the fabric is tested at a temperature of (180±2)℃ in accordance with Appendix A of GB 8965.1-2020, and the thermal stability is not more than 5%;
[0035] (2) The coating containing expandable graphite increases in thickness under the action of arc heat, which can effectively increase its thermal insulation performance; the coating has high air tightness and effectively blocks the hot gases produced by arc explosions; thereby improving the arc thermal protection performance of the fabric. The arc protection performance of the coated fabric was tested based on the American Society for Testing and Materials standard ASTM F1959 / F1959M-2014 "Standard Test Method for Determining Arc Rating of Clothing Materials". During the test, the coating surface was the explosion-facing surface. The arc thermal protection performance value (ATPV), that is, the energy value at which 50% of the incident arc energy may cause heat energy to penetrate the fabric and cause second-degree burns, was 11.5 cal / cm 2 ;
[0036] (3) When no pigment is added, the coating prepared from expandable graphite with white inorganic matter deposited on the surface is white, indicating that the white inorganic matter deposited on the surface can effectively cover the original color of expandable graphite; in addition, the edges of expandable graphite sheets also contain a certain amount of inorganic matter. When the material is heated, chemical reactions occur between the graphite sheets to produce gas, which is blocked by the inorganic matter at the edge, causing the graphite sheets to expand rapidly, with a higher initial expansion rate, which is more conducive to arc protection. Experiments show that for the same coating process, surface deposition treatment can improve the arc thermal protection performance by 0.5-1.1 cal / cm 2 . DETAILED DESCRIPTION
[0037] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0038] 1. Arc protection performance test method:
[0039] The arc protection performance of coated fabrics was tested based on the American Society for Testing and Materials standard ASTM F1959 / F1959M-2014 "Standard Test Method for Determining Arc Rating of Clothing Materials".
[0040] 2. Experimental materials:
[0041] The experimental materials in the examples are all commercially available products. Expandable graphite was purchased from Qingdao Xinghe Graphite Co., Ltd. and has a size of 325 mesh.
[0042] Example 1: Arc protection fabric
[0043] The invention discloses an arc protection fabric, which comprises a base fabric and a coating. The base fabric mainly comprises 45% poly(m-phenylene isophthalamide) fiber, 25% acrylonitrile-vinyl chloride copolymer fiber, 10% low heat shrinkage fiber, 19% permanent flame retardant cellulose fiber and 1% conductive fiber. The low heat shrinkage fiber is poly(m-phenylene isophthalamide) fiber; the permanent flame retardant cellulose fiber is silicon-based flame retardant viscose fiber with a fineness of 1.5 dtex and a length of 51 mm; and the conductive fiber is nylon-based fiber added with conductive carbon black with a specification of 20D / 3F.
[0044] The base fabric processing flow is:
[0045] (1) Spray a solution of triethanolamine oleic acid soap, isomeric alcohol polyoxyethylene ether sodium sulfate and water in a ratio of 1:2:97 onto poly(m-phenylene isophthalamide) fiber and low heat shrinkage fiber at an amount of 3% of the fiber weight, spray an antistatic treatment agent and store in a sealed container for 48 hours;
[0046] (2) Polyisophthalamide (m-phenylene diamine) fiber, acrylonitrile-vinyl chloride copolymer fiber, low heat shrinkage fiber, and permanent flame retardant cellulose fiber are mixed according to a set ratio and combed into fiber strips (weight ratios are calculated based on dry weight)
[0047] (3) feeding the fiber strips into the drawing frame, and combining the three passes to form mature strips;
[0048] (4) The arc protection yarn is made by roving-spinning-winding-drawing-twisting, the yarn is 22tex / 2 strands, the twist coefficient of single yarn is 320, and the twist coefficient of strand is 355;
[0049] (5) The conductive composite yarn is embedded at intervals by warp and weft weaving, wherein the conductive composite yarn is formed by combining the above-mentioned strands with two bundles of 20D conductive yarn bundles, wherein the embedding method is to implant one strand at an interval of 10 mm in the warp direction and to weave one strand at an interval of 10 mm in the weft direction;
[0050] (6) The yarn is wound through a process of warping, warping, sizing, drawing-in, weaving, and finishing to produce arc protection fabrics with a warp density of 280 yarns / 10 cm, a weft density of 220 yarns / 10 cm, a 2 / 1 twill weave, and a surface density of 220 g / m 2 ;
[0051] The coating is composed of expandable graphite, polyurethane and DMF. The mesh number of the expandable graphite is 325 meshes. The polyurethane is a moisture-curing polyurethane. The ratio of expandable graphite: moisture-curing polyurethane: DMF is 8:20:72. The expandable graphite is expandable graphite with titanium hydroxide deposited on the surface. The titanium hydroxide content in the expandable graphite with titanium hydroxide deposited on the surface is 6.5%. The preparation method is as follows: the expandable graphite is added to water, and a homogeneous dispersion liquid is prepared by ultrasonic dispersion method, and heated to 90°C. At the same time, a certain concentration of titanium chloride solution and an ammonia alkaline precipitant are respectively prepared, and the titanium salt solution and the precipitant are simultaneously added dropwise to the graphite dispersion liquid, and the pH is kept constant between 2-3 during the titration process. As the titanium salt is continuously hydrolyzed, the hydrolysis product Ti(OH)4 is continuously precipitated and attached to the graphite surface. The product is filtered, washed, and dried at 90°C to obtain a white powder.
[0052] The coating thickness is 60 μm;
[0053] The coating process is as follows:
[0054] (1) calendering the coated surface of the base fabric;
[0055] (2) Plasma treatment of the coating surface;
[0056] (3) scraping coating agent;
[0057] (4) solidification in a coagulation bath, the coagulation bath is a 20% DMF solution, and the coagulation temperature is 30°C;
[0058] (5) Dry the coated fabric at 95°C.
[0059] The arc protection performance of coated fabrics was tested based on the American Society for Testing and Materials standard ASTM F1959 / F1959M-2014 "Standard Test Method for Determining Arc Rating of Clothing Materials". The coating surface was the explosion-facing surface during the test. The arc thermal protection performance value (ATPV), i.e. the energy value at which 50% of the incident arc energy may cause heat energy to penetrate the fabric and cause second-degree burns, was 12.1 cal / cm 2 ; Rupture threshold (E bt ) That is, the incident arc energy has a 50% chance of causing the fabric to break, and the energy value is 22.2 cal / cm 2 . Thermal stability is 3.0%.
[0060] Example 2: Arc protection fabric
[0061] The ratio of expandable graphite: moisture-curable polyurethane: DMF in the coating of Example 1 is 5:20:72, and other conditions or parameters are consistent with those of Example 1. The arc thermal protection performance value (ATPV) of the composite fabric is 12.0 cal / cm 2 ; Rupture threshold (E bt ) is 22.0cal / cm 2 , the coating is white. The thermal stability is 3.0%.
[0062] Example 3: Arc protection fabric
[0063] The titanium hydroxide content of the expandable graphite with titanium hydroxide deposited on the surface in Example 1 was adjusted to 5%, and other conditions or parameters were consistent with those in Example 1. The arc thermal protection performance value (ATPV) of the composite fabric was 12.0 cal / cm 2 ; Rupture threshold (E bt ) is 22.1cal / cm 2 , the coating is white. The thermal stability is 3.0%.
[0064] Embodiment 4:
[0065] The surface deposition treatment of expandable graphite in Example 1 was omitted, and other conditions or parameters were consistent with those in Example 1. The arc thermal protection performance value (ATPV) of the composite fabric was 11.0 cal / cm 2 ; Rupture threshold (E bt ) is 20.2cal / cm 2 , the coating is black. The thermal stability is 3.0%.
[0066] Embodiment 5:
[0067] The titanium hydroxide content of the expandable graphite with titanium hydroxide deposited on the surface in Example 1 was adjusted to 3%, and other conditions or parameters were consistent with those in Example 1. The arc thermal protection performance value (ATPV) of the composite fabric was 11.1 cal / cm 2 ; Rupture threshold (E bt ) is 20.3cal / cm 2 , the coating is gray. The thermal stability is 3.0%.
[0068] Comparative Example 1:
[0069] The proportion of low heat shrinkage fiber in Example 1 was adjusted to 6%, and other conditions or parameters were consistent with those in Example 1. The arc heat protection performance value of the fabric was 8.8 cal / cm 2 ; The rupture threshold is 16.2cal / cm 2 , the coating is white and has a thermal stability of 6.0%.
[0070] Comparative Example 2:
[0071] The expandable graphite in the coating of Example 1 was removed, and other conditions or parameters were consistent with those of Example 1. The arc thermal protection performance value (ATPV) of the composite fabric was 9.8 cal / cm 2 ; Rupture threshold (E bt ) is 18.1cal / cm 2 , the coating is white and has a thermal stability of 3.0%.
[0072] Comparative Example 3:
[0073] In Example 1, the uncoated surface is the explosion-facing surface, the coated surface is the back surface, and the arc thermal protection performance value (ATPV) is 12.1 cal / cm 2 ; Rupture threshold (E bt ) is 20.1cal / cm 2 , thermal stability is 3.0%.
[0074] Table 1
[0075]
[0076] The coated arc protection fabric prepared according to the provisions of the present invention has good arc protection performance, such as Example 1, Example 2 and Example 3. When it exceeds the scope specified in the patent of the present invention, such as in Example 1, the proportion of low heat shrinkage fiber is too low, there is no expandable graphite in the coating, the expandable graphite is not subjected to surface deposition treatment, and the amount of white inorganic matter deposited on the surface of the expandable graphite is insufficient, all of which lead to low protection performance, insufficient improvement effect of protection performance and gray-black color.
[0077] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. An arc protection fabric, characterized in that: The fabric comprises a base fabric and a coating, wherein the coating comprises expandable graphite and a polymer matrix, wherein the polymer matrix bonds the expandable graphite to the base fabric so that the expandable graphite is located on the outer surface of the base fabric; the base fabric comprises poly(m-phenylene isophthalamide) fiber, acrylonitrile-vinyl chloride copolymer flame-retardant fiber, low heat shrinkage fiber, permanent flame-retardant cellulose fiber and conductive fiber; the expandable graphite has a mesh size of 200-350 meshes; the expandable graphite is a modified expandable graphite with white inorganic matter deposited on the surface; the modified expandable graphite refers to depositing white inorganic matter on the surface of ordinary expandable graphite, wherein the white inorganic matter is titanium hydroxide, and the titanium hydroxide content is 5%-8.5%, by weight, and titanium hydroxide is deposited on the surface of the expandable graphite by a hydrothermal method; The mass ratio of expandable graphite to polymer matrix in the coating is (1-2): (3-5); The low heat shrinkage fiber is one or more mixed fibers of poly(p-phenylene benzobisoxazole) fiber, poly(p-benzimidazole) fiber, poly(phenylene pyridine diimidazole) fiber, polyimide fiber, and poly(p-phenylene terephthalamide).
2. The arc protection fabric according to claim 1, characterized in that: The mass percentages of the fibers in the base fabric are: 35-55% of polyisophthalamide-m-phenylenediamine fibers, 20-35% of acrylonitrile-vinyl chloride copolymer flame-retardant fibers, 10-15% of low heat shrinkage fibers, 25-45% of permanent flame-retardant cellulose fibers and 0.5-2% of conductive fibers.
3. The arc protection fabric according to claim 1, characterized in that: The permanent flame-retardant cellulose fiber is a silicon-based flame-retardant viscose fiber with a fineness of 1.5-1.7 dtex and a length of 51 mm.
4. The arc protection fabric according to any one of claims 1 to 3, characterized in that: The conductive fiber is a nylon-based filament fiber added with conductive carbon black, the fiber bundle fineness is 20D, and the number of fiber strands in the fiber bundle is 1-6.
5. A method for preparing the arc protection fabric according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: (1) calendering the coated surface of the base fabric; (2) Plasma treatment of the coating surface; (3) scrape coating agent; (4) solidifying in a coagulation bath, wherein the coagulation bath is a 15-25% DMF solution and the coagulation temperature is 25-40° C.; (5) Drying the coated fabric to obtain arc protection fabric.
6. The method according to claim 5, characterized in that The mass ratio of expandable graphite, moisture-curable polyurethane and DMF in the coating agent is 5-10:15-25:60-80.
Citation Information
Patent Citations
Titanium dioxide based graphene / La<3+> carbon fibers and application thereof
CN106012109A
Permanent flame retardant deflagration and electric arc prevention fabric and manufacturing method thereof
CN106032602A
Production method of thin cotton polyamide blended flame-retardant fabric having high electric arc prevention value
CN106435931A
Anti-electric-arc flame-retardant mixture and manufacturing method thereof
CN108117750A
Preparation method of X and gamma ray protection aramid paper
CN108193549A