Preparation method of tunneling oxide layer, solar cell and preparation method thereof
By adjusting the temperature and pressure in the reaction furnace tube during the chemical vapor deposition process, the problem of large thickness differences of the tunnel oxide layer between different areas and positions of the silicon wafer is solved, and a more uniform tunnel oxide layer film formation is achieved, improving the the performance of solar cells.
Patent Information
- Application Number
- CN202310244684.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-10
AI Technical Summary
In the chemical vapor deposition process, in the vertical wafer insertion method, the thickness of the tunnel oxide layer varies greatly between different areas and positions of the silicon wafer, resulting in poor uniformity of the tunnel oxide layer between the silicon wafers in the furnace tube.
By setting the temperature in the reaction furnace tube to 580°C to 610°C, introducing oxygen into the furnace tube until the pressure reaches 0.9 to 0.95 atmospheres, stopping the flow of oxygen, and maintaining the temperature for 4 to 15 minutes to grow tunnels on the silicon wafer. Wear through the oxide layer to reduce turbulence and overheating expansion caused by oxygen introduction, and improve the uniformity of oxygen distribution.
It improves the film formation uniformity of the tunnel oxide layer, reduces the local failure of the tunnel oxide layer caused by contact between adjacent silicon wafers, and ensures that the thickness difference of the tunnel oxide layer in different regions and batches of silicon wafers is small, improving the Overall uniformity.
Smart Images

Figure CN116344672B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a method for preparing a tunneling oxide layer, a solar cell and a method for preparing the same. Background Art
[0002] With the rapid development of photovoltaic technology, the conversion efficiency of crystalline silicon solar cells has increased year by year. At present, TOPCon cells and P-type IBC cells stand out with many advantages such as high efficiency and high maturity of industrial process technology. Many manufacturers in the industry have begun to increase their investment in the research and development and production of TOPCon cells and P-type IBC cells. In the mainstream industrial preparation process of the above two types of batteries, chemical vapor deposition equipment is required to prepare tunneling oxide layers and polysilicon layers. With the demand for cost reduction brought about by industrialization, chemical vapor deposition manufacturers usually use vertical insert loading boats to load silicon wafers. Specifically, multiple loading boats are arranged at intervals in the length direction of the furnace tube, and each loading boat is loaded with multiple silicon wafers arranged at intervals along the width direction of the furnace tube. In this vertical insert method, when the reaction gas is introduced along the length direction of the furnace tube, the introduction direction of the reaction gas is perpendicular to the thickness direction of each silicon wafer.
[0003] However, the tunneling oxide layer prepared by the above-mentioned inserting method will have a problem of large differences in thickness of the tunneling oxide layer between different areas on the silicon wafer and between silicon wafers located at different positions in the furnace tube, resulting in poor uniformity of the tunneling oxide layer between the silicon wafers in the furnace tube. Summary of the invention
[0004] Based on this, it is necessary to provide a method for preparing a tunneling oxide layer, a solar cell and a method for preparing the same, which can improve the uniformity of the tunneling oxide layer between silicon wafers in a reaction furnace tube.
[0005] A first aspect of an embodiment of the present application provides a method for preparing a tunneling oxide layer, the method comprising:
[0006] The temperature in the reaction furnace tube is set to 580° C. to 610° C., and oxygen is introduced into the reaction furnace tube; wherein a plurality of silicon wafers are loaded into the reaction furnace tube, and the direction in which oxygen is introduced is perpendicular to the thickness direction of each silicon wafer;
[0007] When the pressure in the reaction furnace tube reaches 0.9 to 0.95 atmospheres, the oxygen is stopped from being introduced, and the temperature in the reaction furnace tube is maintained at 580° C. to 610° C. for 4 to 15 minutes to grow a tunneling oxide layer on the silicon wafer.
[0008] In one embodiment, setting the temperature in the reaction furnace tube to 580° C. to 610° C. and introducing oxygen into the reaction furnace tube comprises:
[0009] The temperature in the reaction furnace tube is set to 590° C. to 600° C., and oxygen is introduced into the reaction furnace tube.
[0010] In one embodiment, maintaining the temperature in the reaction furnace tube at 580° C. to 610° C. for 4 min to 15 min to grow a tunnel oxide layer on a silicon wafer comprises:
[0011] The temperature in the reaction furnace tube is maintained at 590° C. to 600° C. for 4 to 15 minutes to grow a tunneling oxide layer on the silicon wafer.
[0012] In one embodiment, stopping the introduction of oxygen until the pressure in the reaction furnace tube reaches 0.9 to 0.95 atmospheres comprises:
[0013] Stop introducing oxygen when the pressure in the reaction furnace tube reaches 0.92-0.95 atmospheres.
[0014] In one embodiment, the flow rate of oxygen introduced into the reaction furnace tube is 10 slm to 40 slm.
[0015] In one embodiment, the flow rate of oxygen introduced into the reaction furnace tube is 25 slm to 40 slm.
[0016] In one embodiment, the temperature in the reaction furnace tube is set to 580° C. to 610° C., and before oxygen is introduced into the reaction furnace tube, the method further comprises:
[0017] The silicon wafers are inserted into a loading boat, and the loading boat is sent into the reaction furnace tube so that the thickness direction of the silicon wafers is perpendicular to the length direction of the reaction furnace tube.
[0018] In one embodiment, the temperature in the reaction furnace tube is set to 580° C. to 610° C., and before oxygen is introduced into the reaction furnace tube, the method further comprises:
[0019] The reaction furnace tube is evacuated to a vacuum level of 40 mTorr-60 mTorr.
[0020] A second aspect of an embodiment of the present application provides a method for preparing a solar cell, the method comprising:
[0021] Forming a tunneling oxide layer on a silicon wafer by the above-mentioned method for preparing a tunneling oxide layer;
[0022] A polysilicon layer is formed on the tunnel oxide layer.
[0023] A third aspect of an embodiment of the present application provides a solar cell, which is prepared using the above-mentioned method for preparing a solar cell.
[0024] The above-mentioned method for preparing the tunnel oxide layer, the solar cell and the method for preparing the same have the following beneficial effects:
[0025] The temperature in a reaction furnace tube is set to 580° C. to 610° C., oxygen is introduced into the reaction furnace tube, and the introduction of oxygen is stopped when the pressure in the reaction furnace tube reaches 0.9 to 0.95 atmospheres, and the temperature in the furnace tube is maintained at 580° C. to 610° C. for 4 to 15 minutes to grow a tunneling oxide layer on a silicon wafer. Compared with the related art, in the oxygen introduction process and the tube-stifling oxidation, the temperature in the reaction furnace tube is set to be relatively low, and the pressure is maintained to be lower than one atmosphere, so that the distribution uniformity of oxygen in the reaction furnace tube can be improved, which is beneficial for the reaction speeds of silicon wafers at different positions in the furnace tube to remain consistent, thereby improving the film-forming uniformity of the tunneling oxide layer of each silicon wafer.
[0026] In addition, compared with the related technology, the temperature inside the reaction furnace tube is kept low during the oxygen introduction process and the tube oxidation, which can reduce the contact between adjacent silicon wafers due to overheating expansion to a certain extent, avoid the situation where the tunneling oxide layer is not formed locally due to contact between adjacent silicon wafers, and improve the film formation uniformity between different areas on the same silicon wafer.
[0027] Further, the introduction of oxygen is stopped until the pressure in the reaction furnace tube reaches 0.9 to 0.95 atmospheres, and the temperature in the furnace tube is maintained at 580° C. to 610° C. for 4 to 15 minutes. That is, during the process of tube oxidation, the oxygen introduced in the previous stage is used as the reaction gas, and no oxygen is introduced, thereby reducing the violent fluctuations of the gas atmosphere such as the turbulence of the reaction gas caused by the introduction of oxygen in the furnace tube, not only making the film uniformity of each silicon wafer in the same batch better, but also making the thickness difference of the tunneling oxide layer between silicon wafers of different batches smaller, and also improving the uniformity of the tunneling oxide layer between silicon wafers of different batches. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A schematic diagram of the structure of a reaction furnace tube in a method for preparing a tunneling oxide layer provided in an embodiment of the present application;
[0029] Figure 2 A schematic diagram of a process for preparing a tunnel oxide layer provided in an embodiment of the present application;
[0030] Figure 3 This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 1;
[0031] Figure 4 This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 2;
[0032] Figure 5This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 3;
[0033] Figure 6 This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 4;
[0034] Figure 7 This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 5;
[0035] Figure 8 This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 6;
[0036] Fig. 9 This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 7;
[0037] Fig.10 This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 8;
[0038] Fig.11 This is a photosensitive effect diagram of a tunneling oxide layer prepared by the preparation method of Example 9;
[0039] Fig.12 A photosensitive effect diagram of a tunneling oxide layer prepared by a preparation method in the related art;
[0040] Fig.13 For Fig.12 Photosensitive effect of tunneling oxide layer on another batch of silicon wafers under the same process conditions;
[0041] Fig.14 For Fig.12 Photosensitive effect of tunneling oxide layer on another batch of silicon wafers under the same process conditions;
[0042] Fig.15 A schematic diagram of the structure of a solar cell provided in an embodiment of the present application.
[0043] Description of Figure Numbers:
[0044] 100. Chemical vapor deposition equipment; 10. Reaction furnace tube; 11. Inlet; 20. Loading boat; 30. Silicon wafer;
[0045] 200, solar cell; 201, silicon substrate; 202, tunneling oxide layer; 203, passivation layer; 204, polysilicon layer; 205, anti-reflection layer; 206, first electrode; 207, second electrode. DETAILED DESCRIPTION
[0046] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0047] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0048] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0049] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0050] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0051] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0052] The following describes the method for preparing a tunneling oxide layer, a solar cell and a method for preparing the same in accordance with the embodiments of the present application in conjunction with the accompanying drawings.
[0053] Figure 1 A schematic diagram of the structure of a reaction furnace tube in the method for preparing a tunneling oxide layer provided in an embodiment of the present application.
[0054] Reference Figure 1 In the embodiment of the present application, a tunneling oxide layer is prepared by using a chemical vapor deposition device 100. During the preparation process, the silicon wafer 30 is loaded in a loading boat 20 in a vertical inserting manner. Exemplarily, the chemical vapor deposition device 100 may include a reaction furnace tube 10 and a loading boat 20, and the loading boat 20 is sequentially arranged in the reaction furnace tube 10 along the length direction L of the reaction furnace tube 10. A plurality of silicon wafers 30 are loaded on each loading boat 20, and each silicon wafer 30 is arranged on the loading boat 20 in parallel and at intervals along the width direction W of the reaction furnace tube 10. The reaction furnace tube 10 is also provided with an inlet 11 for a reaction gas, and the inlet 11 can be arranged at the end of the length direction of the reaction furnace tube 10, so that the direction of the reaction gas (as shown by the solid arrow in the figure) is perpendicular to the thickness direction of each silicon wafer 30, and is also along the length direction L of the reaction furnace tube 10. The use of such an inserting method to load the silicon wafer 30 can greatly increase the number of silicon wafers 30 placed in the reaction furnace tube 10.
[0055] Figure 2 A schematic diagram of a process for preparing a tunnel oxide layer provided in an embodiment of the present application.
[0056] In a first aspect, the present invention provides a method for preparing a tunnel oxide layer, referring to Figure 2 , the preparation method of the tunnel oxide layer comprises:
[0057] S10, setting the temperature in the reaction furnace tube to 580° C. to 610° C., and introducing oxygen into the reaction furnace tube; wherein a plurality of silicon wafers are loaded in the reaction furnace tube, and the direction of introducing oxygen is perpendicular to the thickness direction of each silicon wafer.
[0058] S20, when the pressure in the reaction furnace tube reaches 0.9-0.95 atmospheres, stop introducing oxygen, and maintain the temperature in the reaction furnace tube at 580° C.-610° C. for 4-15 minutes to grow a tunneling oxide layer on the silicon wafer.
[0059] In the above scheme, the temperature in the reaction furnace tube is set to 580° C. to 610° C., and oxygen is introduced into the reaction furnace tube until the pressure in the reaction furnace tube reaches 0.9 to 0.95 atmospheres, then the introduction of oxygen is stopped, and the temperature in the furnace tube is maintained at 580° C. to 610° C. for 4 to 15 minutes to grow a tunneling oxide layer on the silicon wafer. Compared with the related art, in the oxygen introduction process and the tube oxidation, the temperature in the reaction furnace tube is set to be relatively low, and the pressure is maintained at a level lower than one atmosphere, so that the distribution uniformity of oxygen in the reaction furnace tube can be improved, which is beneficial for the reaction speed of silicon wafers at different positions in the reaction furnace tube to remain consistent, thereby improving the film formation uniformity of the tunneling oxide layer of each silicon wafer.
[0060] In addition, compared with the related technology, the temperature inside the reaction furnace tube is kept low during the oxygen introduction process and the tube oxidation, which can reduce the contact between adjacent silicon wafers due to overheating expansion to a certain extent, avoid the situation where the tunneling oxide layer is not formed locally due to contact between adjacent silicon wafers, and improve the film formation uniformity between different areas on the same silicon wafer.
[0061] Furthermore, when the oxygen supply is stopped, the temperature in the furnace tube is maintained at 580°C to 610°C for 4min to 15min, that is, during the tube oxidation process, the oxygen supplied in the previous stage is used as the reaction gas, and oxygen is no longer supplied, thereby reducing the violent fluctuations of the gas atmosphere such as the turbulence of the reaction gas in the furnace tube due to the supply of oxygen, which not only improves the uniformity of the film layer of each silicon wafer in the same batch, but also reduces the difference in thickness of the tunneling oxide layer between silicon wafers in different batches, thereby improving the uniformity of the tunneling oxide layer between silicon wafers in different batches.
[0062] Furthermore, in the step of setting the temperature in the reaction furnace tube to 580°C-610°C and introducing oxygen into the reaction furnace tube, the temperature in the reaction furnace tube can also be 585°C, 590°C, 595°C, 598°C, 600°C, 605°C and any value in the range between any two of the above values.
[0063] For example, the temperature in the reaction furnace tube can be set to 590° C. to 600° C., and oxygen can be introduced into the reaction furnace tube. In this way, during the introduction of oxygen, the oxygen can be further evenly distributed in the reaction furnace tube, thereby reducing the difference in uniformity between the silicon wafers in the reaction furnace tube.
[0064] Further, in the step of maintaining the temperature in the reaction furnace tube at 580° C. to 610° C. for 4 min to 15 min to grow a tunneling oxide layer on the silicon wafer, the temperature in the reaction furnace tube can also be 585° C., 590° C., 595° C., 598° C., 600° C., 605° C., and any value within the range between any two of the above values.
[0065] For example, the temperature in the reaction furnace tube can be maintained at 590°C to 600°C for 4 to 15 minutes to grow a tunneling oxide layer on the silicon wafer. In this way, during the process of tube oxidation, the uniformity of oxygen distribution in the reaction furnace tube can be further improved, and the difference in uniformity between the silicon wafers in the reaction furnace tube can be improved. Figure 1 As shown in the figure, for the silicon wafers closer to the tube wall of the reaction furnace tube, it is possible to avoid the situation where the adjacent silicon wafers are in contact with each other due to the influence of the temperature of the tube wall of the reaction furnace tube.
[0066] In the embodiment of the present application, in the step of stopping the introduction of oxygen until the pressure in the reaction furnace tube reaches 0.9 to 0.95 atmospheres, in specific implementation, the pressure in the reaction furnace tube can also be 0.91 atmosphere, 0.92 atmosphere, 0.93 atmosphere, 0.94 atmosphere, and any value within the range between any two of the above values.
[0067] For example, the introduction of oxygen may be stopped when the pressure in the reaction furnace tube reaches 0.92 to 0.95 atmospheres.
[0068] In this way, when the pressure is lower than one atmosphere, the oxygen introduced into the furnace tube can be more evenly dispersed between the silicon wafers and between the silicon wafers and the wall of the reaction furnace tube.
[0069] In the embodiment of the present application, the flow rate of oxygen introduced into the reaction furnace tube is 10 slm to 40 slm. In this way, introducing oxygen at a lower flow rate, combined with a lower temperature and a smaller pressure in the reaction furnace tube, can make the introduced oxygen more uniform in the reaction furnace tube.
[0070] Preferably, the flow rate of oxygen may be 15 slm, 20 slm, 25 slm, 28 slm, 30 slm, 32 slm, 35 slm, 38 slm, and any value within a range between any two of the above values.
[0071] For example, the flow rate of oxygen introduced into the reaction furnace tube may be 25 slm to 40 slm.
[0072] In the embodiment of the present application, in step S10, the temperature in the reaction furnace tube is set to 580° C. to 610° C., and before the step of introducing oxygen into the reaction furnace tube, the following steps are also included:
[0073] The silicon wafers are inserted into the loading boat, and the loading boat is sent into the reactor tube so that the thickness direction of the silicon wafers is perpendicular to the length direction of the reactor tube. That is, before oxygen is introduced, the silicon wafers are inserted into the loading boat and the loading boat is pushed into the reactor tube.
[0074] In the embodiment of the present application, in step S10, the temperature in the reaction furnace tube is set to 580° C. to 610° C., and before the step of introducing oxygen into the reaction furnace tube, the following steps are also included:
[0075] The reaction furnace tube is evacuated to a vacuum level of 40 mTorr to 60 mTorr, so that the air and other gases in the reaction furnace can be removed to avoid affecting the production of the tunnel oxide layer.
[0076] In a specific implementation, the method for preparing the tunnel oxide layer in the embodiment of the present application includes:
[0077] Step 1: Enter the boat
[0078] The polished silicon wafers were loaded into the loading boat, and the loading boat was pushed into the reactor tube. N 2 , the temperature inside the reactor tube is set to 400℃~500℃, N 2 The flow rate range is 10slm to 50slm, forming a positive pressure in the reactor tube to prevent external particles from entering the reactor tube and causing pollution. 2 , the reaction furnace tube is evacuated to make the vacuum degree in the reaction furnace tube be 40mTorr~60mTorr.
[0079] Step 2: Oxygenation
[0080] Heat the reaction furnace tube to 580℃~610℃, and after the temperature stabilizes, introduce oxygen to carry out SiO 2 Growth; O 2 The flow rate range is 10slm to 40slm, and the internal pressure of the reactor tube is maintained at 0.9-0.95 atmospheres after oxygenation;
[0081] Step 3: Oxidation
[0082] After the pressure reaches 0.9-0.95 atmospheres, the introduction of oxygen is stopped, and the temperature in the reaction furnace tube is maintained in the range of 580° C. to 610° C. for 4 min to 15 min to grow a tunnel oxide layer on the silicon wafer.
[0083] Several specific experimental examples are given below to illustrate the improvement effect of the method for preparing the tunnel oxide layer of the embodiment of the present application compared with the prior art.
[0084] Embodiment 1
[0085] The method for preparing the tunnel oxide layer comprises:
[0086] A) Heat the reaction furnace tube to 580°C, and after the temperature stabilizes, introduce oxygen to carry out SiO 2 Growth; O 2 The flow rate range is 10slm to 40slm, and the internal pressure of the reactor tube is maintained at 0.93 atmospheres after oxygenation;
[0087] B) After the pressure reaches 0.93 atmospheres, the introduction of oxygen is stopped and the temperature in the reaction furnace tube is maintained at 580° C. for 4 min to 15 min to grow a tunnel oxide layer on the silicon wafer.
[0088] The tunnel oxide layer produced by the above steps A) and B) is denoted as A1.
[0089] Embodiment 2
[0090] Based on the first embodiment, in further improvement, the temperature in the reaction furnace tube in step A) and step B) can also be replaced with: 590° C. At this time, the tunneling oxide layer produced by steps A) and B) is recorded as A2.
[0091] Embodiment 3
[0092] Based on the first embodiment, in further improvement, the temperature in the reaction furnace tube in step A) and step B) can also be replaced with: 595° C. At this time, the tunneling oxide layer produced by steps A) and B) is recorded as A3.
[0093] Embodiment 4
[0094] Based on the first embodiment, in further improvement, the temperature in the reaction furnace tube in step A) and step B) can also be replaced with: 600° C. At this time, the tunneling oxide layer produced by steps A) and B) is recorded as A4.
[0095] Embodiment 5
[0096] Based on the first embodiment, in further improvement, the temperature in the reaction furnace tube in step A) and step B) can also be replaced with: 610° C. At this time, the tunneling oxide layer produced by steps A) and B) is recorded as A5.
[0097] Embodiment 6
[0098] The method for preparing the tunnel oxide layer comprises:
[0099] C) Heat the reaction furnace tube to 595°C, and after the temperature stabilizes, introduce oxygen to carry out SiO 2 Growth; O 2The flow rate range is 10slm to 40slm, and the internal pressure of the reactor tube is maintained at 0.9 atmospheres after oxygenation;
[0100] D) After the pressure reaches 0.9 atmospheres, the introduction of oxygen is stopped and the temperature in the reaction furnace tube is maintained at 595° C. for 4 min to 15 min to grow a tunnel oxide layer on the silicon wafer.
[0101] The tunnel oxide layer produced by the above steps C) and D) is denoted as A6.
[0102] Embodiment 7
[0103] Based on the sixth embodiment, in further improvement, the pressure in the reaction furnace tube in step C) and step D) can also be replaced with 0.92 atmospheres. At this time, the tunnel oxide layer produced by steps C) and D) is recorded as A7.
[0104] Embodiment 8
[0105] Based on the sixth embodiment, in further improvement, the pressure in the reaction furnace tube in step C) and step D) can also be replaced with 0.93 atmospheres. At this time, the tunnel oxide layer produced by steps C) and D) is recorded as A8.
[0106] Embodiment 9
[0107] Based on the sixth embodiment, in further improvement, the pressure in the reaction furnace tube in step C) and step D) can also be replaced with 0.95 atmospheres. At this time, the tunnel oxide layer produced by steps C) and D) is recorded as A9.
[0108] Comparative Example 1
[0109] The method for preparing the tunnel oxide layer comprises:
[0110] E) Heat the reactor tube to 620°C, and after the temperature stabilizes, introduce a large amount of oxygen. 2 The flow rate is 50slm, so that the pressure in the reactor tube reaches one atmosphere after oxygenation;
[0111] F) After the pressure reaches one atmosphere, continue to introduce oxygen. 2 The flow rate range is 1slm to 10slm, and the temperature in the reaction furnace tube is maintained at 620°C for 2min to 15min to grow a tunneling oxide layer on the silicon wafer.
[0112] The tunnel oxide layer produced by the above steps E) and F) is denoted as B1.
[0113] Another batch of tunnel oxide layers prepared under the same process conditions as steps E) and F) above is denoted as B2.
[0114] Another batch of tunnel oxide layers prepared under the same process conditions as steps E) and F) above is denoted as B3.
[0115] For solar cells including tunnel oxide layers A1, A2, A3, A4, A5, A6, A7, A8, A9, and tunnel oxide layers B1, B2, B3, photoluminescence experiments are performed on these cells, and photosensitivity effect diagrams are recorded respectively, such as Figure 3-Figure 14 shown.
[0116] It should be noted that in each photosensitive effect diagram, the darker color area represents a more ideal battery passivation effect, and the more uniform the color, the better the uniformity.
[0117] exist Figure 3-Figure 11 The tunnel oxide layers A1-A9 shown in the photosensitive effect diagram have relatively uniform colors, and the darker areas have larger areas, and the uniformity and passivation are significantly better than Figure 12-14 The tunneling oxide layers B1-B3 shown in the figure indicate that the preparation method of the tunneling oxide layer according to the embodiment of the present application can not only improve the film quality of the tunneling oxide layer formed on the silicon wafer, but also significantly improve the film formation uniformity of different regions of the tunneling oxide layer on the same silicon wafer.
[0118] In a second aspect, an embodiment of the present application further provides a method for preparing a solar cell, the method comprising:
[0119] Forming a tunneling oxide layer on a silicon wafer by using the tunneling oxide layer preparation method in any of the above schemes;
[0120] A polysilicon layer is formed on the tunnel oxide layer.
[0121] Wherein, on the basis of the above step three, the step of forming a polysilicon layer on the tunnel oxide layer may specifically include:
[0122] Step 4: Vacuum
[0123] After the tunnel oxide layer is formed, the valve provided on the reaction furnace tube is opened to evacuate the reaction furnace tube, and the vacuum degree in the reaction furnace tube is maintained at 40 mTorr to 60 mTorr.
[0124] Step 5: Back Pressure
[0125] N is introduced into the reactor tube. 2 Back pressure, and maintain for a preset time; the N 2 The flow rate is 200 sccm to 5000 sccm, the back pressure range is 100 mtorr to 250 mtorr, and the holding time is 30 to 180 seconds.
[0126] Step 6: Amorphous silicon growth
[0127] After the pressure and temperature in the reactor tube are stable, SiH 4 Growth of amorphous silicon; SiH 4 The flow rate range is 200sccm to 1500sccm, the pressure in the reactor tube is maintained at 170mtorr, and the duration is 10 to 70 minutes; after the amorphous silicon growth is completed, N 2 Residual SiH in the discharge pipe 4 .
[0128] Step 7: Cool down, unload the boat and unload the film
[0129] After the temperature in the reaction furnace tube drops, the vacuum is broken and the loading boat is taken out of the reaction furnace tube. The temperature drop range is 400°C. Then the silicon wafer is taken out of the loading boat.
[0130] Step 8: After pre-processing the silicon wafer, high-temperature annealing is performed to convert the amorphous silicon layer into a polycrystalline silicon layer.
[0131] In a third aspect, the present application also provides a solar cell, which is prepared by the method for preparing a solar cell in any of the above schemes. It should be noted that the method for preparing a solar cell has been described in detail above and will not be repeated here.
[0132] Fig.15 A schematic diagram of the structure of a solar cell provided in an embodiment of the present application.
[0133] Reference Fig.15 The solar cell 200 includes: a silicon substrate 201 (ie, the aforementioned silicon wafer 30 ), a tunneling oxide layer 202 , a passivation layer 203 , a polysilicon layer 204 , an anti-reflection layer 205 , a first electrode 206 , and a second electrode 207 .
[0134] A passivation layer 203 and an anti-reflection layer 205 are sequentially provided on one side surface of the silicon substrate 201, and a tunneling oxide layer 202, a polysilicon layer 204, a passivation layer 203 and an anti-reflection layer 205 are sequentially provided on the other side surface of the silicon substrate 201, wherein the passivation layer 203 may be an aluminum oxide layer, and the anti-reflection layer 205 may include a single layer or multiple layers of silicon nitride layer.
[0135] The first electrode 206 and the second electrode 207 are disposed at intervals on one side of the silicon substrate 201 where the polysilicon layer 204 is disposed. The first electrode 206 may be an aluminum electrode, and the second electrode 207 may be a silver electrode.
[0136] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0137] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a tunneling oxide layer, characterized in that: include: The temperature in the reaction furnace tube is set to 580° C. to 610° C., and oxygen is introduced into the reaction furnace tube; wherein a plurality of silicon wafers are loaded in the reaction furnace tube, and the direction in which the oxygen is introduced is perpendicular to the thickness direction of each of the silicon wafers; When the pressure in the reaction furnace tube reaches 0.9 to 0.95 atmospheres, the introduction of oxygen is stopped, and the temperature in the reaction furnace tube is maintained at 580° C. to 610° C. for 4 to 15 minutes to grow a tunneling oxide layer on the silicon wafer.
2. The method for preparing a tunneling oxide layer according to claim 1, characterized in that: The step of setting the temperature in the reaction furnace tube to 580° C. to 610° C. and introducing oxygen into the reaction furnace tube comprises: The temperature in the reaction furnace tube is set to 590° C. to 600° C., and oxygen is introduced into the reaction furnace tube.
3. The method for preparing a tunneling oxide layer according to claim 1, characterized in that: The step of maintaining the temperature in the reaction furnace tube at 580° C. to 610° C. for 4 to 15 minutes comprises: The temperature in the reaction furnace tube is maintained at 590° C. to 600° C. for 4 min to 15 min.
4. The method for preparing a tunneling oxide layer according to claim 1, characterized in that: The step of stopping the introduction of oxygen until the pressure in the reaction furnace tube reaches 0.9 to 0.95 atmospheres comprises: The oxygen supply is stopped when the pressure in the reaction furnace tube reaches 0.92-0.95 atmospheres.
5. The method for preparing a tunneling oxide layer according to any one of claims 1 to 4, characterized in that: The flow rate of oxygen introduced into the reaction furnace tube is 10slm to 40slm.
6. The method for preparing a tunneling oxide layer according to claim 5, characterized in that: The flow rate of oxygen introduced into the reaction furnace tube is 25slm to 40slm.
7. The method for preparing a tunneling oxide layer according to any one of claims 1 to 4, characterized in that: The step of setting the temperature in the reaction furnace tube to 580° C. to 610° C. and introducing oxygen into the reaction furnace tube further comprises: The silicon wafers are inserted into a loading boat, and the loading boat is sent into the reaction furnace tube, so that the thickness direction of the silicon wafers is perpendicular to the length direction of the reaction furnace tube.
8. The method for preparing a tunneling oxide layer according to any one of claims 1 to 4, characterized in that: The step of setting the temperature in the reaction furnace tube to 580° C. to 610° C. and introducing oxygen into the reaction furnace tube further comprises: The reaction furnace tube is subjected to a vacuum treatment so that the vacuum degree in the reaction furnace tube is 40 mTorr-60 mTorr.
9. A method for preparing a solar cell, characterized in that: include: Forming a tunneling oxide layer on a silicon wafer by the method for preparing a tunneling oxide layer according to any one of claims 1 to 8; A polysilicon layer is formed on the tunnel oxide layer.
10. A solar cell, characterized in that: The solar cell is prepared by the method for preparing a solar cell according to claim 9.