A kind of alloy and its preparation method and application
By developing specific alloy compositions in food contact steels to form ferrite and TiC phases, the problem of heavy metal ions migration in existing food contact steels is solved, high strength and toughness and low harmful metal mobility are achieved, and safety and Corrosion resistance, meets the performance requirements of steel for food contact.
Patent Information
- Application Number
- CN202211581535.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Among the existing food contact steel products, especially stainless steel and low alloy steel, there are problems of heavy metal ions dissolution and migration in acid, alkali, salt and high temperature environments, resulting in health risks, and the corrosion resistance of low alloy steel is insufficient. Lack of security.
Develop an alloy with a content of C: 0.03-0.08%, Si≤0.01%, Mn≤0.04%, P≤0.005%, S≤0.005%, Als≤0.005%, Ti: 0.003-0.015%, N≤0.002 %, O≤0.005%, Cr+Ni+As+Sn+Bi+Sb+Pb≤0.05%, the balance is Fe and inevitable impurities. By forming ferrite and TiC phases, the strength and toughness are improved and harmful metals are reduced. ion mobility.
It achieves low mobility and high strength and toughness of harmful metal ions, meets the performance indicators of steel plates for food contact, provides good safety and corrosion resistance, and is far lower than the hazardous metal migration concentration required by national standards.
Smart Images

Figure CN116377338B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an alloy, and in particular to an alloy that can be used in steel products for contact with food. Background Art
[0002] With the improvement of people's quality of life and safety awareness, the safety issues caused by food contact steel products have gradually attracted people's attention. Food contact steel can generally be divided into two categories: stainless steel and low alloy steel (carbon steel). Stainless steel is a steel system with a wide range of applications and excellent cost performance in the world today. Because of its good metallic properties, corrosion resistance, beauty and durability, it is widely used in food-related fields such as tableware containers, tools and equipment for food production and operation. Affected by the steel system and preparation process, stainless steel contains a large amount of alloy elements such as chromium (Cr), nickel (Ni), and manganese (Mn). For example, Cr, as the main alloy element of stainless steel, is generally higher than 10.5% to ensure the corrosion resistance of steel. Since stainless steel tableware containers have to undergo cooking processes such as steaming, boiling, frying, and frying during food processing, they have to be in contact with food for a long time under specific acid, alkali, salt, high temperature and other environments, which can easily cause the dissolution and migration of heavy metals.
[0003] In addition, these tableware containers need to be cleaned with detergents after use, and detergents generally contain alkaline substances, which may destroy the high-chromium dense passivation film on the metal surface, resulting in the dissolution of chromium. These dissolved heavy metal ions are very likely to enter the human body through food, endangering health. For example, if the human body ingests too much Cr, it will accumulate in the liver, kidneys and endocrine glands, causing health problems such as stomach pain and internal organ damage. Its high-valent ion - hexavalent chromium is also highly oxidizing, which can cause toxic side effects such as mutagenicity, teratogenicity, carcinogenicity and genotoxicity in organisms.
[0004] In addition, excessive intake of Ni can cause central circulation disorders, edema, hemorrhage and degeneration of the myocardium, brain, lungs and kidneys. Ni is also closely related to a variety of cancers (lung cancer, nasopharyngeal cancer and leukemia). Data show that drinking water with high nickel content every day will increase the incidence of cancer, especially cancer patients must avoid contact with nickel-containing products during radiotherapy and chemotherapy; excessive intake of Mn in the human body may cause damage to the extrapyramidal tract of the nervous system and the corresponding Parkinson's disease syndrome, and severe cases may cause symptoms of mental illness.
[0005] On the other hand, low alloy steel (carbon steel) is generally considered to have a higher safety factor and will not cause harm to the human body because of the low content of other metal elements added to the steel itself. Therefore, it is also widely used to make food-related products such as knives and cookware. According to incomplete statistics, low alloy steel accounts for about 60,000 tons of steel used for food contact in my country each year. The safety of steel in this field is bound to receive more and more attention and concern. However, low alloy steel (carbon steel) generally has low corrosion resistance. Whether heavy metals dissolve and migrate under specific acid, alkali, salt and high temperature conditions and exceed a certain content is still lacking in relevant research. Summary of the invention
[0006] To overcome at least one defect of the above-mentioned prior art, on the one hand, an embodiment of the present invention provides an alloy, which comprises the following components, by mass percentage: C: 0.03-0.08%; Si≤0.01%; Mn≤0.04%; P≤0.005%; S≤0.005%; Als≤0.005%; Ti: 0.003-0.015%; N≤0.002%; O≤0.005%; Cr+Ni+As+Sn+Bi+Sb+Pb≤0.05%; the balance is Fe and unavoidable impurities.
[0007] According to one embodiment of the present invention, the alloy includes the following components: C: 0.05-0.08%; Si≤0.01%; Mn≤0.04%; P≤0.005%; S≤0.005%; Als≤0.005%; Ti: 0.006-0.012%; N≤0.002%; O≤0.002%; Cr+Ni+As+Sn+Bi+Sb+Pb≤0.05%; the balance is Fe and unavoidable impurities.
[0008] According to one embodiment of the present invention, the mass content of Fe in the alloy is 99.0% to 99.6%; and / or,
[0009] The mass percentage of C is expressed as C%, the mass percentage of Ti is expressed as Ti%, the mass percentage of S is expressed as S%, and the mass percentage of N is expressed as N%. The mass percentages of the above elements have the following relationship: 3C%>20Ti%>34N%+30S%.
[0010] According to one embodiment of the present invention, the mass percentage of C is expressed as C%, the mass percentage of Si is expressed as Si%, the mass percentage of Mn is expressed as Mn%, and the mass percentage of Ti is expressed as Ti%. The mass percentages of the above elements have the following relationship: 5(3 / 5Si%+5 / 7Mn%) 1 / 2 +2Ti%≥3C%.
[0011] According to an embodiment of the present invention, the microstructure of the alloy includes a first phase and a second phase, the first phase is ferrite, and the second phase includes Ti and C elements.
[0012] According to one embodiment of the present invention, the mass percentage of the second phase is 0.28-0.35%; and / or,
[0013] The average grain size of the ferrite is ≤10 μm; and the two-dimensional size of the second phase is 3 to 10 nm.
[0014] According to one embodiment of the present invention, the yield strength of the alloy is ≥230 MPa, the tensile strength is ≥300 MPa, the elongation after fracture is ≥40%, and the reduction of area is ≥70%.
[0015] In a second aspect, an embodiment of the present invention provides a method for preparing the above alloy, comprising preparing raw materials into continuous casting billets to obtain the alloy.
[0016] According to one embodiment of the present invention, the method comprises subjecting the continuously cast billet to hot rolling; or subjecting the continuously cast billet to cold rolling.
[0017] In a third aspect, an embodiment of the present invention provides a food contact utensil made of the above alloy.
[0018] The alloy of one embodiment of the present invention has a low content of harmful metal ions and a low harmful metal ion mobility; at the same time, it has high strength and toughness, meets the performance indicators of food contact steel plates, is used for preparing food contact products, and has good safety.
[0019] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings are only for the purpose of illustrating particular embodiments and are not to be construed as limiting the invention.
[0021] in:
[0022] Figure 1 This is a metallographic structure morphology diagram of the steel tool obtained in Example 1 of the present invention;
[0023] Figure 2 This is a metallographic structure morphology diagram of the hot-rolled coil prepared in Example 2 of the present invention;
[0024] Figure 3A , 3B This is a comparison chart of harmful ion migration concentrations of the coil prepared in Example 3 of the present invention and the Q235 steel plate of Comparative Example 4 in a standard 4% acetic acid aqueous solution;
[0025] Figure 3C A photo of a cookware made of the rolled plate obtained in Example 3 of the present invention;
[0026] Figure 4 This is a metallographic structure morphology of the cold-rolled coil after annealing obtained in Example 4 of the present invention. DETAILED DESCRIPTION
[0027] The preferred embodiments of the present invention are described in detail below, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0028] An embodiment of the present invention provides an alloy, which includes the following components, by mass percentage: C: 0.03-0.08%; Si≤0.01%; Mn≤0.04%; P≤0.005%; S≤0.005%; Als≤0.005%; Ti: 0.003-0.015%; N≤0.002%; O≤0.005%; Cr+Ni+As+Sn+Bi+Sb+Pb≤0.05%; the balance is Fe and unavoidable impurities.
[0029] The alloy according to one embodiment of the present invention is a low alloy steel.
[0030] In one embodiment, the microstructure of the alloy includes a first phase and a second phase, the first phase is ferrite, and the second phase is formed by a combination of C and Ti, such as a TiC phase; the formation of the second phase can play a role in grain refinement and strengthening.
[0031] In one embodiment, the mass percentage of the first phase in the alloy can be 99.65-99.72%, such as 99.66%, 99.67%, 99.68%, 99.69%, 99.7%, 99.71%; the mass percentage of the second phase can be 0.28-0.35%, such as 0.29%, 0.3%, 0.31%, 0.32%, 0.33%, 0.34%. The above mass percentages are obtained by simulation calculation based on the alloy component content, and the calculation software used can be, for example, Thermo-Calc material thermodynamic software simulation.
[0032] In one embodiment, the average grain size of ferrite is ≤10 μm; the two-dimensional size of the second phase may be between 3 and 10 nm, that is, the size of the second phase in any direction on the two-dimensional surface is between 3 and 10 nm.
[0033] In one embodiment, the alloy includes the following components: C: 0.05-0.08%; Si≤0.01%; Mn≤0.04%; P≤0.005%; S≤0.005%; Als≤0.005%; Ti: 0.006-0.012%; N≤0.002%; O≤0.002%; Cr+Ni+As+Sn+Bi+Sb+Pb≤0.05%; the balance is Fe and unavoidable impurities.
[0034] In one embodiment, the mass content of Fe is 99.0% to 99.6%, for example, 99.1%, 99.2%, 99.3%, 99.4%, or 99.5%.
[0035] In one embodiment, carbon (C) is an essential element for improving strength, but too high a carbon content will affect the plasticity and toughness of the alloy, bringing adverse effects on forming. Taking all aspects into consideration, the C content needs to be controlled within 0.03-0.08%, such as 0.04%, 0.05%, 0.06%, 0.07%.
[0036] In one embodiment, silicon (Si) is a deoxidizing element and also a solid solution strengthening element, which can improve the strength of the alloy to a certain extent. The content of silicon exceeding a certain amount will affect the toughness and plasticity of the alloy. The alloy of one embodiment of the present invention mainly focuses on precipitation strengthening and fine grain strengthening of the second phase. In order to avoid affecting the subsequent processing and use of the alloy, the Si content is controlled to ≤ 0.01%, such as 0.001%, 0.002%, 0.005%, 0.008%.
[0037] In one embodiment, manganese (Mn) is an essential element to ensure the strength and toughness of the alloy. A certain content of Mn can refine the ferrite grains and produce MnS to reduce the harmful effects of S in the alloy. However, manganese is a harmful element and can cause harm to the human body if it migrates into food, so the Mn content is controlled to ≤ 0.04%, such as 0.01%, 0.02%, and 0.03%.
[0038] In one embodiment, acid-soluble aluminum (Als) is an excellent deoxidizer for the alloy and an effective element for grain refinement. Al is easy to form aluminum oxide inclusions, which is not conducive to the forming of the alloy and also brings certain harm to the corrosion resistance of the alloy. Therefore, under the premise of ensuring the deoxidation of the alloy, the amount of acid-soluble aluminum in the alloy can be controlled to be ≤0.005%, such as 0.001%, 0.002%, 0.003%, 0.004%.
[0039] In one embodiment, titanium (Ti) is a key controlled element and a strengthening element that controls the precipitation of the second phase in the alloy. Titanium and carbon form fine precipitates that can be pinned at the grain boundaries to refine the grains, and can also be dissolved in the solid solution of iron to play a certain strengthening role. When the titanium content in the alloy exceeds a certain value, its strength and toughness will decrease to a certain extent, so the Ti content is controlled at 0.003-0.015%, such as 0.005%, 0.006%, 0.008%, 0.01%, 0.012%, 0.014%.
[0040] In one embodiment, the mass percentage of C in the alloy is expressed as C%, the mass percentage of Ti is expressed as Ti%, the mass percentage of S is expressed as S%, and the mass percentage of N is expressed as N%. The mass percentages of Ti, C, N, and S elements have the following relationship: 3C%>20Ti%>34N%+30S%; under this content relationship, it can be ensured that a certain amount of precipitation phase (second phase) is generated without exceeding the Ti content, thereby ensuring the strength and toughness of the alloy.
[0041] In one embodiment, nitrogen (N) can form a second phase carbonitride with C, V, and Ti to improve the toughness of the alloy. However, nitrogen will preferentially form coarse titanium carbonitride with C and Ti, which affects the precipitation of TiC, deteriorates the strengthening effect, and reduces the effective strengthening titanium content in the alloy. Therefore, the N content is controlled to ≤ 0.002%, such as 0.001%, 0.0015%.
[0042] In the alloy of one embodiment of the present invention, a certain amount of C and Ti can form a relatively fine second phase, which plays a role in grain refinement and strengthening. After a relatively systematic study and theoretical analysis, combined with the individual contents of C and Ti, if the contents of C and Si, Mn, Ti and other elements satisfy the following relationship: 5 (3 / 5Si% + 5 / 7Mn%) 1 / 2 +2Ti%≥3C%, then the precipitation of the second phase can be guaranteed without exceeding the carbon content. Too high a carbon content will lead to a decrease in plasticity. Here, the carbon content not exceeding the standard refers to the carbon content that will not lead to a decrease in plasticity. If the carbon content is reduced, the strength of the alloy cannot be guaranteed. In one embodiment of the present invention, by limiting the above-mentioned element content, the precipitation strengthening and fine grain strengthening effects of the second phase can improve the strength, thereby improving the strength of the alloy while maintaining its plasticity. Wherein, in the above formula, the mass percentage of C is expressed as C%, the mass percentage of Si is expressed as Si%, the mass percentage of Mn is expressed as Mn%, and the mass percentage of Ti is expressed as Ti%.
[0043] In one embodiment, phosphorus (P) is an impurity element in the alloy, which will damage the toughness and plasticity of the alloy. Therefore, the P content is controlled to be less than 0.005%, such as 0.001%, 0.002%, 0.003%, 0.004%.
[0044] In one embodiment, sulfur (S) is an impurity element in the alloy, which forms sulfide inclusions and becomes the starting point of corrosion, thereby avoiding competitive precipitation of S and Ti. Therefore, the S content is controlled to be below 0.005%, such as 0.001%, 0.002%, 0.003%, and 0.004%.
[0045] In one embodiment, oxygen (O) is an impurity element in the alloy, and its presence is not conducive to casting and will deteriorate the casting performance of the alloy. Therefore, the O content is controlled to be ≤ 0.005%, such as 0.001%, 0.002%, 0.003%, 0.004%.
[0046] In one embodiment, Cr, Ni, As, Sn, Bi, Sb, and Pb are all harmful elements in the alloy and should be controlled at a relatively low level, and their total should not exceed 0.05%, for example, 0.01%, 0.02%, 0.03%, and 0.04%.
[0047] In one embodiment, the alloy has a yield strength of ≥230 MPa, a tensile strength of ≥300 MPa, an elongation after fracture of ≥40%, and a reduction of area of ≥70%.
[0048] In one embodiment, the yield strength of the alloy is 230-250 MPa, for example, 231 MPa, 235 MPa, 240 MPa, 245 MPa; the tensile strength is 300-345 MPa, for example, 305 MPa, 310 MPa, 315 MPa, 317 MPa, 320 MPa, 323 MPa, 325 MPa, 327 MPa, 330 MPa, 335 MPa, 340 MPa; the elongation after fracture is 40-45%, for example, 41%, 42%, 43%, 44%; the reduction of area is 70-80%, for example, 72%, 74%, 75%, 76%, 78%.
[0049] The concentration of harmful metal migration of the alloy according to one embodiment of the present invention is tested in a 4% acetic acid aqueous solution, a mixed solution of 3% sodium chloride and 4% acetic acid, and a high-temperature environment heated to 800° C., and the content is more than 5 times lower than the requirement of GB / T 4336-2016.
[0050] The alloy of one embodiment of the present invention has a harmful metal migration concentration that is more than 5 times lower than the requirement of GB / T4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", and can have excellent plasticity and strength while ensuring a low harmful metal migration concentration.
[0051] The alloy according to one embodiment of the present invention improves the strength and toughness of high-purity iron by microalloying the harmless metal element Ti to form a second phase, so that the alloy meets the performance indicators of a steel sheet for food contact.
[0052] The alloy of one embodiment of the present invention has good strength and plasticity and can be used for preparing food contact utensils by deep drawing, spinning and other forming methods. The concentration of harmful ion migration in different use environments is far lower than the national standard requirements and has good food contact safety.
[0053] The alloy of one embodiment of the present invention controls the content of harmful heavy metals and inclusions, thereby significantly reducing the concentration of harmful metal migration; further, by adjusting the addition amounts of elements such as C, Ti, N, and S, it is able to meet the strength and plasticity requirements of products such as steel plates or coils.
[0054] One embodiment of the present invention provides a steel plate or a coil, which is made of the above alloy and meets the performance index of a food contact steel plate. The thickness of the steel plate or the coil can be 0.2 to 4 mm, and further can be 0.2 to 3 mm, such as 0.5 mm, 0.8 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3.5 mm.
[0055] An embodiment of the present invention provides a method for preparing the above alloy, comprising: according to the ratio of the above components, preparing a continuous casting billet with raw materials in a specific ratio to obtain the alloy.
[0056] In one embodiment, the raw material can be made into a continuous casting billet by an existing process or device.
[0057] In one embodiment, the microstructure of the alloy is mainly determined by the type and content of each component, and the obtained continuous casting billet has the aforementioned microstructure, namely, the ferrite phase and the second phase composed of Ti and C.
[0058] In one embodiment, a converter is used for smelting, and refining methods such as LF furnace, VD furnace or RH furnace vacuum are used to control the content of impurity elements such as P and S in the molten steel, reduce inclusions, and control the content of harmful elements in the molten iron, such as heavy metals such as Cr, Ni, As, Cd, and Pb.
[0059] In one embodiment, the method for preparing the alloy comprises the following steps:
[0060] Hot metal smelting;
[0061] Hot metal pretreatment; and
[0062] The steel is made in a converter according to the composition ratio of the above alloys. The process route adopted is converter, LF, VD or RH refining and vacuum treatment. The content of harmful elements in the molten steel is strictly controlled, and the gas content is controlled to ensure the inclusion content in the steel. Finally, the dead flow of the molten steel is prevented by feeding the Ti wire to prevent the formation of large titanium oxides in the high temperature process.
[0063] Among them, impurity elements in steel can be reduced through molten iron pretreatment. After desulfurization and dephosphorization, the sulfur content is less than 0.002% and the phosphorus content is less than 0.002%. During the smelting process, the refining treatment time of LF and RH is not less than 20 minutes, the superheat of the ladle is controlled to be ≤20°C, and protective casting is adopted throughout the process.
[0064] In one embodiment, the purity of the molten iron can be improved by pre-treating the molten iron to remove impurities; the molten iron pre-treatment may include steps such as desulfurization, dephosphorization, and desiliconization.
[0065] In one embodiment, the continuously cast slab may be processed to further refine its microstructure.
[0066] In one embodiment, the continuous casting billet can be directly cast into a shape (as-cast) after being melted to obtain a desired product.
[0067] In one embodiment, the continuously cast slab may be hot rolled (hot rolled state) or cold rolled (cold rolled state).
[0068] In one embodiment, the steel material may be cast, hot rolled or cold rolled according to the use environment.
[0069] In one embodiment, the hot rolling treatment includes: reheating the continuous casting billet to 1100-1250°C, and then continuously rolling, and the heating temperature can be, for example, 1150°C or 1200°C. During the continuous rolling process, the final rough rolling deformation temperature is 900-950°C, for example, 910°C, 920°C, 930°C, or 940°C; the roughing deformation is ≥30%, and can further be 30-65%, for example, 35%, 40%, 45%, 50%, 55%, 60%, or 65%; the final rolling temperature is 800-850°C, for example, 810°C, 820°C, 830°C, or 840°C; and the coiling temperature is ≤400°C, and can further be 300-400°C, for example, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, or 390°C. The thickness of the steel obtained after continuous rolling can be 2 to 3 mm. The steel can be derusted according to actual needs.
[0070] In one embodiment, the cold rolling treatment includes: the hot rolled coil can be directly used, and multiple cold rolling (for example, the number of passes ≥ 2) is performed after shearing, and the rolling speed is controlled to be 0.5-2 m / s, for example, 1 m / s, 1.5 m / s. Further, annealing treatment is performed after the cold rolling treatment. After cold rolling, due to the high dislocation density, the yield strength of the steel will increase to a certain extent, and the elongation will decrease. The above effects can be weakened or eliminated through annealing treatment. The temperature of the annealing treatment can be 600-700°C, for example, 620°C, 650°C, 660°C, 680°C; the holding time can be ≥10h, and further can be 10-20h, for example, 12h, 14h, 15h, 16h, 17h, 18h; the furnace temperature can be ≤80°C, and further can be 50-80°C, for example, 55°C, 60°C, 65°C, 70°C, 75°C. After the cold-rolled and annealed steel is taken out of the furnace, it can be further flattened before use. The thickness of the steel obtained after the cold-rolled and annealed treatment can be 0.2 to 1.5 mm.
[0071] The alloy of one embodiment of the present invention has a simple preparation process and low cost, can be applied to various food contact steel environments, and is suitable for the manufacturing requirements of steel plates / coils with a specification of 0.2 to 3 mm.
[0072] The steel plate or rolled plate according to one embodiment of the present invention can simultaneously meet the processing and forming processes, and the processing state has little effect on strength and plasticity.
[0073] The preparation of alloy and steel materials according to one embodiment of the present invention is further described below in conjunction with the accompanying drawings and specific examples. The tests involved in the examples are all carried out in accordance with relevant national standards. Chemical analysis of the chemical composition of the finished product C, Si, Mn, P, S, Ni, Cr, Mo, N, and Nb is carried out in accordance with GB / T 223, GB11261, GB / T 11170, GB / T 20123, and GB / T20124; the yield strength, tensile strength, elongation after fracture, and cross-sectional shrinkage are obtained by taking standard tensile specimens for tensile testing in accordance with GB / T228.1-2010 standard.
[0074] Example 1
[0075] Selected iron ore is used to pre-treat the molten iron and then obtain the continuous casting billet through the process of molten steel purification smelting - LF - RH refining vacuum - continuous casting billet; the refining treatment time of LF and RH during the smelting process is 20 minutes, and the superheat of the ladle is controlled at 20℃.
[0076] The obtained continuous casting billet is cut into small pieces, melted in an electric furnace and directly sand cast into steel tools with a thickness of 3±0.5mm. The obtained steel tools are tested and the metallographic structure diagram is shown in Figure 1 , and the rest of the test results are as follows.
[0077] The components of the steelware and the mass percentage of each component are measured as follows:
[0078] C: 0.07%; Si: 0.01%; Mn: 0.04%; P: 0.003%; S: 0.004%; Als: 0.005%; Ti: 0.010%; N: 0.002%; O: 0.002%; Cr: 0.010%; Ni: 0.020%; As≤0.001%; Sn≤0.001%; Bi≤0.001%; Sb≤0.001%; Pb≤0.001, the remainder is Fe and other inevitable impurities.
[0079] The yield strength of the steel tool was measured to be 245 MPa, the tensile strength was 345 MPa, the elongation after fracture was 40%, and the cross-sectional shrinkage was 70%.
[0080] According to the requirements of GB / T 4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", the steel utensils prepared in Example 1 were subjected to a metal ion migration test, wherein the concentration of harmful ions migrated in a 4% acetic acid aqueous solution was: Cr: 0.081 mg / L; Mn: 0.165 mg / L; Ni < 0.0001 mg / L; As < 0.0001 mg / L; Sn < 0.0001 mg / L; Bi < 0.0001 mg / L; Sb < 0.0001 mg / L; Pb < 0.0001 mg / L;
[0081] The concentration of harmful ions in a mixed solution of 3% sodium chloride and 4% acetic acid is: Cr: 0.0753mg / L; Mn: 0.0697mg / L; Ni < 0.0001mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0082] The concentrations of harmful ions migrated in a high temperature environment of 800°C are: Cr: 0.0982 mg / L; Mn: 0.490 mg / L; Ni: 0.041 mg / L; As<0.0001 mg / L; Sn<0.0001 mg / L; Bi<0.0001 mg / L; Sb<0.0001 mg / L; Pb<0.0001 mg / L.
[0083] Example 2
[0084] Selected iron ore is used to pre-treat the molten iron and then obtain the continuous casting billet through the process of molten steel purification smelting - LF - RH refining vacuum - continuous casting billet; the refining treatment time of LF and RH during the smelting process is 20 minutes, and the superheat of the ladle is controlled at 20℃.
[0085] The continuous casting billet is heated to 1100°C and then continuously rolled. The deformation amount of the roughing pass is 60%, and the deformation temperature of the final roughing pass is 950°C. The rolling speed is 0.8m / s. Laminar cooling is used during the rolling process. The final rolling temperature is 800°C and the coiling temperature is 350°C.
[0086] The thickness of the produced coil is 2±0.02mm. The coil is tested and the metallographic structure diagram is shown in Figure 2 , and the rest of the test results are as follows.
[0087] The measured components of the coil and the mass percentage of each component are as follows:
[0088] C: 0.07%; Si: 0.01%; Mn: 0.04%; P: 0.004%; S: 0.004%; Als: 0.003%; Ti: 0.005%; N: 0.002%; O: 0.002%; Cr: 0.010%; Ni: 0.004%; As≤0.001%; Sn≤0.001%; Bi≤0.001%; Sb≤0.001%; Pb≤0.001%; the balance is Fe and other unavoidable impurities.
[0089] The yield strength of the coil was measured to be 231 MPa, the tensile strength was 323 MPa, the elongation after fracture was 41%, and the cross-sectional shrinkage was 70%.
[0090] According to the requirements of GB / T 4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", the metal ion migration test was carried out on the coil prepared in Example 2, wherein the concentration of harmful ions migrated in 4% acetic acid aqueous solution was: Cr: 0.091 mg / L; Mn: 0.203 mg / L; Ni < 0.0001 mg / L; As < 0.0001 mg / L; Sn < 0.0001 mg / L; Bi < 0.0001 mg / L; Sb < 0.0001 mg / L; Pb < 0.0001 mg / L;
[0091] The concentration of harmful ions in a mixed solution of 3% sodium chloride and 4% acetic acid is: Cr: 0.0853mg / L; Mn: 0.0970mg / L; Ni < 0.0001mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0092] The concentrations of harmful ions migrated in a high temperature environment of 800°C are: Cr: 0.0882 mg / L; Mn: 0.590 mg / L; Ni: 0.021 mg / L; As<0.0001 mg / L; Sn<0.0001 mg / L; Bi<0.0001 mg / L; Sb<0.0001 mg / L; Pb<0.0001 mg / L.
[0093] Example 3
[0094] Selected iron ore is used to pre-treat the molten iron and then obtain the continuous casting billet through the process of molten steel purification smelting - LF - RH refining vacuum - continuous casting billet; the refining treatment time of LF and RH during the smelting process is 20 minutes, and the superheat of the ladle is controlled at 20℃.
[0095] The continuous casting billet is heated to 1100°C and then continuously rolled. The deformation amount of the roughing pass is 65%, and the deformation temperature of the final roughing pass is 900°C. The rolling speed is 0.9m / s. Laminar cooling is used during the rolling process. The final rolling temperature is 850°C and the coiling temperature is 400°C.
[0096] The thickness of the coil is 2.0±0.02mm. The coil is tested and the concentration of harmful ions migrated by Q235 in a standard 4% acetic acid aqueous solution is compared as shown in the figure below. Figures 3A to 3B As shown in the figure, it can be seen that the Cr ion concentration of the rolled plate of Example 3 is ≤0.25mg / L, and the Mn ion concentration is ≤1.8mg / L, which meet the international standards, while the above ion concentrations of Q235 do not meet the standards. Figure 3C As shown, it shows that the prepared alloy has good formability; the other test results are as follows.
[0097] The measured components of the coil and the mass percentage of each component are as follows:
[0098] C: 0.05%; Si: 0.01%; Mn: 0.04%; P: 0.003%; S: 0.001%; Als: 0.003%; Ti: 0.006%; N: 0.002%; Cr: 0.020%; Ni: 0.004%; O: 0.0015%; As≤0.001%; Sn≤0.001%; Bi≤0.001%; Sb≤0.001%; Pb≤0.001%; the balance is Fe and other unavoidable impurities.
[0099] The yield strength of the coil was measured to be 235 MPa, the tensile strength was 327 MPa, the elongation after fracture was 42%, and the cross-sectional shrinkage was 75%.
[0100] According to the requirements of GB / T 4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", the coil prepared in Example 3 was subjected to a metal ion migration test, wherein:
[0101] The concentration of harmful ions in 4% acetic acid aqueous solution is: Cr: 0.107mg / L; Mn: 0.197mg / L; Ni<0.0001mg / L; As<0.0001mg / L; Sn<0.0001mg / L; Bi<0.0001mg / L; Sb<0.0001mg / L; Pb<0.0001mg / L;
[0102] The concentration of harmful ions in a mixed solution of 3% sodium chloride and 4% acetic acid is: Cr: 0.0991mg / L; Mn: 0.1070mg / L; Ni < 0.0001mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0103] The concentrations of harmful ions migrated in a high temperature environment of 800°C are: Cr: 0.0882 mg / L; Mn: 0.590 mg / L; Ni: 0.021 mg / L; As<0.0001 mg / L; Sn<0.0001 mg / L; Bi<0.0001 mg / L; Sb<0.0001 mg / L; Pb<0.0001 mg / L.
[0104] Example 4
[0105] Selected iron ore is used to pre-treat the molten iron and then obtain the continuous casting billet through the process of molten steel purification smelting - LF - RH refining vacuum - continuous casting billet; the refining treatment time of LF and RH during the smelting process is 20 minutes, and the superheat of the ladle is controlled at 20℃.
[0106] The continuous casting billet is heated to 1100°C and then continuously rolled. The deformation amount of the roughing pass is 65%, and the deformation temperature of the final roughing pass is 900°C. The rolling speed is 0.9m / s. Laminar cooling is used during the rolling process. The final rolling temperature is 850°C and the coiling temperature is 400°C.
[0107] After the steel is uncoiled, it is pickled to remove the iron oxide scale on the surface of the coil, and then cold rolled and annealed. The relevant parameters of the cold rolling process are shown in Table 1:
[0108] Table 1
[0109] Rolling pass Thickness(left) / mm Thickness(right) / mm Reduction rate / % Rolling speed / m / s Rolling force / ton one 2.01 1.62 18.6 0.76 870 two 1.02 1.62 37.0 1.52 1030
[0110] The relevant parameters of the annealing process are shown in Table 2:
[0111] Table 2
[0112] Heating temperature / ℃ Insulation time / h Hood temperature / ℃ Water cooling temperature / ℃ Oven temperature / ℃ 650 17 600 350 70(air cooling)
[0113] The thickness of the produced coil is 2.0±0.02mm. The coil is tested and the metallographic structure diagram is shown in Figure 4 , and the rest of the test results are as follows.
[0114] The measured components of the coil and the mass percentage of each component are as follows:
[0115] C: 0.05%; Si: 0.01%; Mn: 0.04%; P: 0.003%; S: 0.001%; Als: 0.003%; Ti: 0.005%; N: 0.002%; Cr: 0.020%; Ni: 0.004%; O: 0.001%; As≤0.001%; Sn≤0.001%; Bi≤0.001%; Sb≤0.001%; Pb≤0.001%; the balance is Fe and other unavoidable impurities.
[0116] The yield strength of the prepared coil is 230 MPa, the tensile strength is 317 MPa, the elongation after fracture is 44%, and the cross-sectional shrinkage is 80%.
[0117] According to the requirements of GB / T 4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", the coil prepared in Example 4 was subjected to a metal ion migration test, wherein:
[0118] The harmful ion migration concentrations of 4% acetic acid aqueous solution are Cr: 0.098 mg / L; Mn: 0.203 mg / L; Ni < 0.0001 mg / L; As < 0.0001 mg / L; Sn < 0.0001 mg / L; Bi < 0.0001 mg / L; Sb < 0.0001 mg / L; Pb < 0.0001 mg / L.
[0119] The concentration of harmful ions in a mixed solution of 3% sodium chloride and 4% acetic acid is: Cr: 0.0789mg / L; Mn: 0.0791mg / L; Ni < 0.0001mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0120] The concentrations of harmful ions migrated in a high temperature environment of 800°C are: Cr: 0.0803 mg / L; Mn: 0.483 mg / L; Ni: 0.021 mg / L; As<0.0001 mg / L; Sn<0.0001 mg / L; Bi<0.0001 mg / L; Sb<0.0001 mg / L; Pb<0.0001 mg / L.
[0121] Comparative Example 1
[0122] Selected iron ore is used to pre-treat the molten iron and then obtain the continuous casting billet through the process of molten steel purification smelting - LF - RH refining vacuum - continuous casting billet; the refining treatment time of LF and RH during the smelting process is 20 minutes, and the superheat of the ladle is controlled at 20℃.
[0123] The continuous casting billet is heated to 1100°C and then continuously rolled. The deformation amount of the roughing pass is 65%, and the deformation temperature of the final roughing pass is 900°C. The rolling speed is 0.9m / s. Laminar cooling is used during the rolling process. The final rolling temperature is 850°C and the coiling temperature is 400°C.
[0124] The thickness of the produced coil is 2.0±0.02 mm, and the other test results are as follows.
[0125] The measured components of the coil and the mass percentage of each component are as follows:
[0126] C: 0.07%; Si: 0.01%; Mn: 0.05%; P: 0.004%; S: 0.006%; Als: 0.003%; Ti: 0.02%; N: 0.003%; Cr: 0.02%; Ni: 0.040%; O: 0.0015%; As≤0.001%; Sn≤0.001%; Bi≤0.001%; Sb≤0.001%; Pb≤0.001%; the balance is Fe and other inevitable impurities.
[0127] The yield strength of the coil was measured to be 255 MPa, the tensile strength was 375 MPa, the elongation after fracture was 35%, and the cross-sectional shrinkage was 68%.
[0128] According to the requirements of GB / T 4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", the coil prepared in Comparative Example 1 was subjected to a metal ion migration test, wherein:
[0129] The concentration of harmful ions in 4% acetic acid aqueous solution is: Cr: 0.125mg / L; Mn: 0.228mg / L; Ni: 0.0042mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0130] The concentration of harmful ions in a mixed solution of 3% sodium chloride and 4% acetic acid is: Cr: 0.0998mg / L; Mn: 0.218mg / L; Ni < 0.0001mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0131] The concentrations of harmful ions migrating under high temperature environment of 800℃ are: Cr: 0.0803mg / L; Mn: 0.483mg / L; Ni: 0.035mg / L; As<0.0001mg / L; Sn<0.0001mg / L; Bi<0.0001mg / L; Sb<0.0001mg / L; Pb<0.0001mg / L.
[0132] Comparative Example 2
[0133] Selected iron ore is used to pre-treat the molten iron and then obtain the continuous casting billet through the process of molten steel purification smelting - LF - RH refining vacuum - continuous casting billet; the refining treatment time of LF and RH during the smelting process is 20 minutes, and the superheat of the ladle is controlled at 20℃.
[0134] The continuous casting billet is heated to 1100°C and then continuously rolled. The deformation amount of the roughing pass is 65%, and the deformation temperature of the final roughing pass is 900°C. The rolling speed is 0.9m / s. Laminar cooling is used during the rolling process. The final rolling temperature is 850°C and the coiling temperature is 400°C.
[0135] The thickness of the produced coil is 2.0±0.02 mm, and the other test results are as follows.
[0136] The measured components of the coil and the mass percentage of each component are as follows:
[0137] C: 0.05%; Si: 0.02%; Mn: 0.04%; P: 0.006%; S: 0.003%; Als: 0.003%; Ti: 0.02%; N: 0.002%; Cr: 0.05%; Ni: 0.035%; O: 0.0016%; As≤0.001%; Sn≤0.001%; Bi≤0.001%; Sb≤0.001%; Pb≤0.001%; the balance is Fe and other unavoidable impurities.
[0138] The yield strength of the coil was measured to be 248 MPa, the tensile strength was 367 MPa, the elongation after fracture was 32%, and the cross-sectional shrinkage was 75%.
[0139] According to the requirements of GB / T 4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", the coil prepared in Comparative Example 2 was subjected to a metal ion migration test, wherein:
[0140] The concentration of harmful ions in 4% acetic acid aqueous solution is: Cr: 0.579mg / L; Mn: 0.209mg / L; Ni<0.0001mg / L; As<0.0001mg / L; Sn<0.0001mg / L; Bi<0.0001mg / L; Sb<0.0001mg / L; Pb<0.0001mg / L;
[0141] The concentration of harmful ions in a mixed solution of 3% sodium chloride and 4% acetic acid is: Cr: 0.487mg / L; Mn: 0.195mg / L; Ni < 0.0001mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0142] The concentrations of harmful ions migrating under high temperature environment of 800℃ are: Cr: 0.605mg / L; Mn: 0.499mg / L; Ni<0.0001mg / L; As<0.0001mg / L; Sn<0.0001mg / L; Bi<0.0001mg / L; Sb<0.0001mg / L; Pb<0.0001mg / L.
[0143] Comparative Example 3
[0144] Selected iron ore is used to pre-treat the molten iron and then obtain the continuous casting billet through the process of molten steel purification smelting - LF - RH refining vacuum - continuous casting billet; the refining treatment time of LF and RH during the smelting process is 20 minutes, and the superheat of the ladle is controlled at 20℃.
[0145] The continuous casting billet is heated to 1100°C and then continuously rolled. The deformation amount of the roughing pass is 65%, and the deformation temperature of the final roughing pass is 900°C. The rolling speed is 0.9m / s. Laminar cooling is used during the rolling process. The final rolling temperature is 850°C and the coiling temperature is 400°C.
[0146] The thickness of the produced coil is 2.0±0.02 mm, and the other test results are as follows.
[0147] The measured components of the coil and the mass percentage of each component are as follows:
[0148] C: 0.07%; Si: 0.02%; Mn: 0.06%; P: 0.005%; S: 0.007%; Als: 0.005%; Ti: 0.015%; N: 0.003%; Cr: 0.03%; Ni: 0.02%; O: 0.002%; As≤0.001%; Sn≤0.001%; Bi≤0.001%; Sb≤0.001%; Pb≤0.001%; the balance is Fe and other unavoidable impurities.
[0149] The yield strength of the coil was measured to be 265 MPa, the tensile strength was 380 MPa, the elongation after fracture was 33%, and the cross-sectional shrinkage was 64%.
[0150] According to the requirements of GB / T 4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", the coil prepared in Comparative Example 3 was subjected to a metal ion migration test, wherein:
[0151] The concentration of harmful ions in 4% acetic acid aqueous solution is: Cr: 0.393mg / L; Mn: 0.303mg / L; Ni: 0.107mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0152] The concentration of harmful ions in a mixed solution of 3% sodium chloride and 4% acetic acid is: Cr: 0.283mg / L; Mn: 0.299mg / L; Ni: 0.0931mg / L; As < 0.0001mg / L; Sn < 0.0001mg / L; Bi < 0.0001mg / L; Sb < 0.0001mg / L; Pb < 0.0001mg / L;
[0153] The concentrations of harmful ions migrated in a high temperature environment of 800°C are: Cr: 0.401 mg / L; Mn: 0.481 mg / L; Ni: 0.152 mg / L; As<0.0001 mg / L; Sn<0.0001 mg / L; Bi<0.0001 mg / L; Sb<0.0001 mg / L; Pb<0.0001 mg / L.
[0154] Comparative Example 4
[0155] This example is a 3mm thick Q235 steel plate purchased from the market in a common hot-rolled state. After inspection, its components and the mass percentage of each component are as follows:
[0156] C: 0.22%; Si: 0.35%; Mn: 0.85%; P: 0.035%; S: 0.04%; Ti: 0.1%; N: 0.005%; Cr: 0.034%; Ni: 0.0012%; O: 0.031%; As≤0.001%; Sn≤0.001%; Bi≤0.001%; Sb≤0.001%; Pb≤0.001%; the balance is Fe and other inevitable impurities.
[0157] The yield strength of the steel plate was measured to be 345 MPa, the tensile strength was 435 MPa, the elongation after fracture was 32%, and the cross-sectional shrinkage was 65%.
[0158] According to the requirements of GB / T 4336-2016 "National Food Safety Standard - Metal Materials and Products for Food Contact", the metal ion migration test was carried out on Q235 steel plate.
[0159] The concentration of harmful ions in 4% acetic acid aqueous solution is: Cr: 0.402mg / L; Mn: 4.5mg / L; Ni: <0.0001mg / L; As <0.0001mg / L; Sn <0.0001mg / L; Bi <0.0001mg / L; Sb <0.0001mg / L; Pb <0.0001mg / L;
[0160] The concentration of harmful ions in a mixed solution of 3% sodium chloride and 4% acetic acid is: Cr: 0.399mg / L; Mn: 4.639mg / L; Ni: <0.0001mg / L; As <0.0001mg / L; Sn <0.0001mg / L; Bi <0.0001mg / L; Sb <0.0001mg / L; Pb <0.0001mg / L;
[0161] The concentrations of harmful ions migrated in a high temperature environment of 800°C are: Cr: 0.481 mg / L; Mn: 5.103 mg / L; Ni: 0.0093 mg / L; As<0.0001 mg / L; Sn<0.0001 mg / L; Bi<0.0001 mg / L; Sb<0.0001 mg / L; Pb<0.0001 mg / L.
[0162] According to the description of the above embodiments and comparative examples, the alloy component content of comparative example 1 has a small change compared with that of embodiment 1, and the N and S elements have a certain change. The test results of the prepared alloy plate show that although the concentration of harmful ion migration of the alloy plate of comparative example 1 is also low, its mechanical properties cannot meet the index requirements. The main changes of comparative examples 2 and 3 are trace elements such as Cr and Ni compared with embodiments 2 and 3. The test results show that the tensile properties of the alloy plates of comparative examples 2 and 3 do not meet the requirements, and the migration amount of harmful elements is significantly increased, which cannot meet the use requirements of international standards.
[0163] Therefore, the embodiments of the present invention can achieve an overall optimized balance between the harmful metal ion mobility and the mechanical properties of the alloy by limiting the content of the alloy components.
[0164] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. An alloy, comprising the following components, by mass percentage: C: 0.03-0.08%; 0.001%≤Si≤0.01%; 0.01%≤Mn≤0.04%; P≤0.005%; S≤0.005%; Als≤0.005%; Ti: 0.003-0.015%; N≤0.002%; O≤0.005%; Cr+Ni+As+Sn+Bi+Sb+Pb≤0.05%; the balance being Fe and unavoidable impurities; The mass percentage of C is expressed as C%, the mass percentage of Ti is expressed as Ti%, the mass percentage of S is expressed as S%, and the mass percentage of N is expressed as N%. The mass percentages of the above elements have the following relationship: 3C%>20Ti%>34N%+30S%; The mass percentage of C is expressed as C%, the mass percentage of Si is expressed as Si%, the mass percentage of Mn is expressed as Mn%, and the mass percentage of Ti is expressed as Ti%. The mass percentages of the above elements have the following relationship: 5 (3 / 5Si% + 5 / 7Mn%) 1 / 2 +2Ti%≥3C%; The yield strength of the alloy is ≥230MPa, the tensile strength is ≥300MPa, the elongation after fracture is ≥40%, the cross-sectional shrinkage is ≥70%, and the harmful metal migration concentration of the alloy is more than 5 times lower than the requirement of GB / T4336-2016.
2. The alloy according to claim 1 comprises the following components: C: 0.05-0.08%; 0.001%≤Si≤0.01%; 0.01%≤Mn≤0.04%; P≤0.005%; S≤0.005%; Als≤0.005%; Ti: 0.006-0.012%; N≤0.002%; O≤0.002%; Cr+Ni+As+Sn+Bi+Sb+Pb≤0.05%; the balance is Fe and unavoidable impurities.
3. The alloy according to claim 1, wherein The mass percentage of Fe is 99.0% to 99.6%. 4 . The alloy according to claim 1 , wherein the microstructure of the alloy comprises a first phase and a second phase, wherein the first phase is ferrite, and the second phase comprises Ti and C.
5. The alloy according to claim 4, wherein The mass percentage of the second phase is 0.28-0.35%; and / or, The average grain size of the ferrite is ≤10 μm; and the two-dimensional size of the second phase is 3 to 10 nm.
6. A method for preparing the alloy according to any one of claims 1 to 5, comprising preparing raw materials into continuous casting billets to obtain the alloy.
7. The method according to claim 6 comprises subjecting the continuously cast slab to hot rolling; or subjecting the continuously cast slab to cold rolling.
8. A food contact utensil made from the alloy according to any one of claims 1 to 5.
Citation Information
Patent Citations
Cold-rolled steel plate and preparation method thereof
CN104060070A
Low-carbon low-nitrogen and high-oxygen industrial pure iron and production method thereof
CN104451385A
Porcelain oven rack
US20030172921A1
High-strength hot rolled steel sheet and method for manufacturing the same
US20140363696A1
Non-ageing low-alloy hot-rolled strip-form formable steel
US4985090A
Cited By
Preparation method of food contact baking tray steel, food contact baking tray steel and baking tray
CN117187510A
Method for producing a food contact baking tray steel, food contact baking tray steel and baking tray
CN117187510B