Resin composition and power cable
By using a phenol skeleton monomer as a resistance-imparting agent in the propylene resin insulating layer, the problem of uneven insulation caused by metal impurities is solved, and high insulation and electrical stability are achieved.
Patent Information
- Application Number
- CN202180071423.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-21
- Filing Date
- 2021-10-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-10-26
AI Technical Summary
When acrylic resin is used as the insulation material of power cables, it is easy to cause uneven insulation due to the mixing of metal impurities, which affects the performance of the cable.
Using a monomer with a phenol skeleton and a specific alkyl group in the phenol skeleton as a resistance-imparting agent, it suppresses the influence of metal impurities on insulation through a chemical structure with high affinity for metal impurities and a specified molecular weight and melting point. The resin composition is coated with metal impurities to mitigate resistance changes and electric field concentration.
It effectively improves the insulation of the propylene resin composition, ensures the high insulation and stability of the insulation layer, and avoids the decrease in insulation caused by metal impurities.
Smart Images

Figure CN116390979B_ABST
Abstract
Description
Technical Field
[0001] This application claims priority based on Japanese application No. 2020-211491 filed on December 21, 2020, and cites all the contents described in the aforementioned Japanese application.
[0002] The present disclosure relates to a resin composition and a power cable. Background Art
[0003] Cross-linked polyethylene is excellent in insulating properties and is therefore widely used as a resin component constituting an insulating layer in power cables and the like (for example, Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 57-69611 Summary of the invention
[0007] According to one embodiment of the present disclosure, a resin composition is provided, the resin composition containing a resin component containing a propylene unit and a resistance-imparting agent, the resistance-imparting agent being a monomer having a phenolic skeleton and having a hydrogen or an alkyl group having 1 to 3 carbon atoms bonded to at least one of the ortho positions of a hydroxyl group in the phenolic skeleton, the melting point being 215° C. or lower, and the molecular weight being 200 or higher and 500 or lower, the content of the resistance-imparting agent being 0.4 or higher and 10 or lower parts by mass relative to 100 parts by mass of the resin component, and the content ratio of metal impurities being 0.02% or lower by volume ratio.
[0008] According to another embodiment of the present disclosure, there is provided a power cable, comprising: a conductor; and an insulating layer coated on the outer periphery of the conductor, wherein the insulating layer is formed of a resin composition, wherein the resin composition contains a resin component containing a propylene unit and a resistance-imparting agent, wherein the resistance-imparting agent is a monomer having a phenolic skeleton and having a hydrogen or an alkyl group having 1 to 3 carbon atoms bonded to at least one of the ortho positions of the hydroxyl group in the phenolic skeleton, wherein the melting point is 215° C. or less, and the molecular weight is 200 to 500, wherein the content of the resistance-imparting agent is 0.4 to 10 parts by mass relative to 100 parts by mass of the resin component, and the content ratio of metal impurities is 0.02% or less by volume. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 1 is a schematic cross-sectional view perpendicular to the axial direction of a power cable according to an embodiment of the present disclosure. DETAILED DESCRIPTION
[0010] [Problems to be Solved by the Present Disclosure]
[0011] Cross-linked polyethylene cannot be recycled after years of degradation and can only be incinerated, so there are concerns about the impact on the environment.
[0012] Therefore, in recent years, as a resin component constituting the insulating layer, a resin containing propylene (hereinafter also referred to as "propylene resin") has attracted attention. Even if the propylene resin is non-crosslinked, it can achieve high insulation. That is, it can take both insulation and recyclability into account. In addition, by using propylene resin, it is possible to improve operability, processability, and ease of manufacturing.
[0013] However, when a propylene resin is used as a resin component constituting the insulating layer, the insulating properties inherent to the propylene resin may not be obtained.
[0014] An object of the present disclosure is to provide a technology for improving the insulation properties of a resin composition containing a propylene resin.
[0015] [Effects of the present disclosure]
[0016] According to the present disclosure, the insulation properties of a resin composition containing a propylene resin can be improved.
[0017] [Description of Embodiments of the Present Disclosure]
[0018] <Insights Obtained by the Inventors>
[0019] First, the findings obtained by the inventors are briefly described.
[0020] Generally, propylene resin has a large amount of crystals and is prone to form coarse crystals. Therefore, when the insulating layer is formed using only propylene resin, there is a tendency for the insulating layer to become hard. Therefore, when using propylene resin as a resin component constituting the insulating layer, it is necessary to mix a low-crystalline resin to control the crystallinity of the propylene resin.
[0021] The present inventors formed an insulating layer by low-crystallizing a propylene-based resin. As a result, when a power cable was produced, the insulating properties were sometimes uneven, and the insulating properties inherent to the propylene-based resin could not be obtained.
[0022] This point has been studied, and it is found that the unevenness of insulation is caused by foreign matter mixed into the resin composition during the manufacturing process of the power cable. As the foreign matter, for example, there are metal impurities such as metal powders from metal conductors, and carbides (amber) generated by the burning of resin components. Among the foreign matter, especially metal impurities will have an impact on insulation, and depending on the amount of mixing, the insulation of the power cable is sometimes greatly uneven.
[0023] The metal impurities have poor adhesion to the resin component, so a sharp resistance change occurs at the interface with the resin component, which reduces the insulation. In addition, when the metal impurities have a protruding shape, the electric field is easily concentrated, so the insulation is easily reduced.
[0024] As described above, in the insulating layer made of acrylic resin, uneven insulation may occur due to metal impurities mixed in during the manufacturing stage.
[0025] The inventors of the present invention have studied the above problem and found that the use of a specific additive can suppress the unevenness of insulation. The additive is a substance used as an antioxidant, a monomer having a phenolic skeleton and a hydrogen or carbon 1-3 alkyl group bonded to at least one of the ortho positions of the hydroxyl group in the phenolic skeleton, a molecular weight of 200 to 500, and a melting point of 215° C. or less, which is lower than the heating mixing temperature of the propylene resin.
[0026] The above-mentioned monomers have been generally used as antioxidants so far, but according to the research of the inventors, it is found that by having a chemical structure with high affinity for metal impurities and a specified molecular weight and melting point, the surface of the metal impurities can be melted and coated during the heating and mixing of the resin composition. In addition, by coating the surface, it acts in a manner that alleviates the rapid resistance change at the interface between the metal impurities and the resin component, and also alleviates the electric field concentration to the metal impurities. As a result, the decrease in insulation caused by metal impurities can be suppressed. That is, the above-mentioned monomers not only act as antioxidants, but also act as resistance-imparting agents that impart resistance to the decrease in insulation caused by metal impurities to the insulating layer.
[0027] Furthermore, the inventors have found that by adding a predetermined amount of the above-mentioned compound to a resin composition containing a propylene resin, a decrease in insulation properties due to metal impurities mixed into the resin composition can be suppressed.
[0028] The present disclosure has been completed based on the above-mentioned findings found by the inventors.
[0029] <Embodiments of the present disclosure>
[0030] Next, embodiments of the present disclosure will be described by way of examples.
[0031] [1] A resin composition according to one embodiment of the present disclosure contains a resin component containing propylene units and a resistance-imparting agent, wherein the resistance-imparting agent is a monomer having a phenolic skeleton and having a hydrogen or carbon 1 to 3 alkyl group bonded to at least one of the ortho positions of the hydroxyl group in the phenolic skeleton, the melting point being 215° C. or lower and the molecular weight being 200 to 500, the content of the resistance-imparting agent being 0.4 to 10 parts by mass based on 100 parts by mass of the resin component, and the content of metal impurities being 0.02% or less by volume.
[0032] According to this configuration, the insulation properties of the resin composition containing the propylene resin can be improved.
[0033] [2] Another embodiment of the present invention provides a power cable comprising: a conductor; and an insulating layer covering the outer periphery of the conductor, wherein the insulating layer is formed of a resin composition, the resin composition comprising a resin component containing propylene units and a resistance-imparting agent, the resistance-imparting agent being a monomer having a phenolic skeleton and having a hydrogen or carbon 1 to 3 alkyl group bonded to at least one of the ortho positions of the hydroxyl group in the phenolic skeleton, the melting point being 215° C. or less, and the molecular weight being 200 to 500, the content of the resistance-imparting agent being 0.4 to 10 parts by mass based on 100 parts by mass of the resin component, and the content of metal impurities being 0.02% or less by volume.
[0034] According to this configuration, the insulation properties of the power cable can be improved.
[0035] [3] In the power cable described in [2] above, the resin component contains at least one of an ethylene unit and a styrene unit.
[0036] According to this configuration, excessive crystal growth of the acrylic resin can be suppressed, and high insulation and desired flexibility can be obtained in the insulating layer.
[0037] [4] In the power cable described in [2] or [3] above, the resistance-imparting agent has a linear carbon chain structure having 5 to 10 carbon atoms.
[0038] According to this configuration, electrical stability can be imparted to the insulating layer.
[0039] [5] In the electric power cable described in any one of [2] to [4] above, the resistance-imparting agent contains a sulfur atom.
[0040] According to this configuration, electrical stability can be imparted to the insulating layer.
[0041] [6] In the electric power cable according to any one of [2] to [5] above, the resistance imparting agent has a melting point at which it becomes a liquid at 27°C.
[0042] According to this configuration, the surface of the metal impurities can be more reliably covered with the resistance-imparting agent, and the decrease in insulation properties due to the metal impurities can be further suppressed.
[0043] [7] In the electric power cable according to any one of [2] to [6] above, the resistance-imparting agent is a phenolic antioxidant.
[0044] According to this configuration, the effect of the antioxidant can be imparted to the insulating layer.
[0045] [8] In the power cable described in any one of [2] to [7] above, the resin composition comprises: a propylene homopolymer having a melting point of 160°C to 175°C and a heat of fusion of 100 J / g to 120 J / g as a propylene-based resin, and the resin composition has a melting point of 158°C to 168°C and a heat of fusion of 55 J / g to 110 J / g.
[0046] According to this configuration, excessive crystal growth of the acrylic resin can be suppressed in the insulating layer, thereby achieving high insulation properties.
[0047] [9] In the power cable described in any one of [2] to [7] above, the resin composition comprises: a propylene random copolymer having a melting point of 140°C to 155°C and a heat of fusion of 90 J / g to 105 J / g as a propylene-based resin, wherein the melting point of the resin composition is 140°C to 150°C and the heat of fusion is 55 J / g to 100 J / g.
[0048] According to this configuration, excessive crystal growth of the acrylic resin can be suppressed in the insulating layer, thereby achieving high insulation properties.
[0049] [Details of the embodiments of the present disclosure]
[0050] Next, an embodiment of the present disclosure will be described below with reference to the drawings. It should be noted that the present disclosure is not limited to these examples, but is shown by the claims, and is intended to include all changes within the meaning and scope equivalent to the claims.
[0051] <One embodiment of the present disclosure>
[0052] (1) Resin composition
[0053] The resin composition of this embodiment is a material constituting the insulating layer 130 of the power cable 10 described later, and includes, for example, a resin component containing propylene units, a resistance imparting agent, and other additives as required. In addition, the resin composition contains metal impurities that are inevitably mixed in during its production process.
[0054] Metal impurities are substances mixed in during the polymerization stage of the material, the mixing / extrusion stage of the material, and are metal powders containing copper, iron, their alloys, or other metals used at the manufacturing site. The size of the metal powder is not particularly limited, and is, for example, 50 μm or more and 500 μm or less. The content of the metal impurities, i.e., the amount mixed, is less than 0.02% by volume. The content of the metal impurities can be obtained, for example, by collecting 100 mm of the resin composition and 3 The volume of the sample piece is calculated by considering the metal impurities contained in the sample piece as spherical, and the volume ratio is obtained.
[0055] The resin composition of the present embodiment contains at least propylene resin as a resin component. Therefore, when the resin composition is analyzed by a nuclear magnetic resonance (NMR) device, at least propylene units are detected. For example, when the propylene resin is random polypropylene, propylene units and ethylene units are detected, and when the propylene resin is a propylene homopolymer, propylene units are detected.
[0056] The resin component preferably includes at least one of a low-crystalline resin and a styrene resin as a soft component that reduces the crystallinity of the propylene resin to improve the softness of the insulating layer. When the resin component includes a low-crystalline resin and a styrene resin, when the resin composition is analyzed by NMR, monomer units derived from these resins are detected. For example, when an ethylene-propylene rubber (EPR) described later is included as a low-crystalline resin, propylene units and ethylene units derived from the ethylene-propylene rubber are detected. In addition, for example, when a styrene resin is included, styrene units derived from the styrene resin are detected.
[0057] Hereinafter, each component will be described.
[0058] (Acrylic resin)
[0059] Propylene resin is the base polymer of the resin composition and is the component with the highest content in the resin component. As the propylene resin, for example, a propylene homopolymer (hereinafter, also referred to as homo-PP) or a propylene random copolymer (hereinafter, also referred to as random PP) can be used. From the viewpoint of obtaining higher insulation in the insulating layer, it is preferred to use random PP. Although homo-PP has a larger amount of crystallization than random PP and can obtain high insulation, cracks are caused in the crystals and between the crystals in the insulating layer, so sometimes the insulation originally possessed cannot be obtained. In contrast, although random PP has a lower amount of crystallization due to the inclusion of ethylene units, cracks caused by coarse crystallization are not easily generated in the insulating layer, and high insulation can be obtained compared to homo-PP.
[0060] In addition, the stereoregularity of the propylene resin is not particularly limited, but is preferably isotactic. When mixed with a low-crystalline resin, the isotactic propylene resin can be further low-crystalline compared to the syndiotactic and atactic resins, thereby improving the brittleness of the insulating layer at low temperatures and improving the insulation.
[0061] The melting point and heat of fusion of the propylene resin are not particularly limited. For example, in the case of homopolymer PP, the melting point is preferably 160°C to 175°C, and the heat of fusion is preferably 100 J / g to 120 J / g. In addition, for example, in the case of random PP, the melting point is preferably 140°C to 155°C, and the heat of fusion is preferably 90 J / g to 105 J / g.
[0062] (Low crystalline resin)
[0063] The low-crystalline resin is a component that controls the crystal growth (crystallization amount) of the propylene resin to impart flexibility to the insulating layer. Here, the low-crystalline resin refers to a component that has low crystallinity or is amorphous and has no melting point or has a melting point of 100°C or less. The heat of fusion of the low-crystalline resin is, for example, 50 J / g or less, preferably 30 J / g or less.
[0064] As the low crystalline resin, from the viewpoint of improving the controllability of crystal growth and the flexibility of the insulating layer, a copolymer obtained by copolymerizing at least two of ethylene, propylene, butene, hexene and octene is preferred. It should be noted that the carbon-carbon double bond in the monomer unit constituting the low crystalline resin is preferably located at the α position, for example.
[0065] Examples of low-crystalline resins include ethylene propylene rubber (EPR), very low-density polyethylene (VLDPE), and the like. For example, very low-density polyethylene has a density of 0.91 g / cm 3 Below, preferably 0.855 g / cm 3 ~0.890g / cm 3 of polyethylene.
[0066] For example, from the viewpoint of compatibility with the propylene-based resin, the low crystalline resin is preferably a copolymer containing propylene. Examples of the copolymer containing propylene include EPR among those mentioned above.
[0067] Preferably, the ethylene content of EPR is, for example, 20% by mass or more, preferably 40% by mass or more, and more preferably 55% by mass or more. When the ethylene content is less than 20% by mass, the compatibility of EPR with respect to the propylene resin becomes too high. Therefore, even if the content of EPR in the insulating layer is reduced, the insulating layer can be softened. However, the crystallization of the propylene resin cannot be fully controlled, and the insulation may decrease. In contrast, by setting the ethylene content to 20% by mass or more, the compatibility of EPR with respect to the propylene resin can be suppressed from becoming too high. Thus, the softening effect produced by EPR can be obtained, and the crystallization of the propylene resin caused by EPR can be fully controlled. As a result, the decrease in insulation can be suppressed. Moreover, by preferably setting the ethylene content to 40% by mass or more, and more preferably to 55% by mass or more, the crystallization can be more stably controlled, and the decrease in insulation can be stably suppressed. It should be noted that the ethylene content represents the mass ratio of ethylene units in the ethylene units and propylene units constituting the EPR.
[0068] On the other hand, the low crystalline resin may be, for example, a copolymer not containing propylene. As a copolymer not containing propylene, VLDPE is preferred from the viewpoint of easy availability. As VLDPE, for example, PE composed of ethylene and 1-butene, PE composed of ethylene and 1-octene, etc. can be cited.
[0069] As a low crystalline resin, according to the copolymer without propylene, a predetermined amount of low crystalline resin can be mixed with the propylene resin while suppressing complete compatibility. Therefore, by setting the content of such a copolymer to a predetermined amount or more, the crystallization of the propylene resin can be stably controlled.
[0070] (Styrene resin)
[0071] Styrene resin is a styrene thermoplastic elastomer containing styrene as a hard segment and containing at least one of ethylene, propylene, butylene and isoprene as a soft segment. Styrene resin can be dispersed in a resin composition in the same manner as a low-crystalline resin to control the crystal growth of propylene resin. Specifically, it can be considered that when styrene resin is mixed with a low-crystalline resin in a propylene resin, a specific phase structure is formed by finely dispersing the low-crystalline resin as a starting point in the propylene resin, and the excessive crystal growth of the propylene resin can be suppressed by the phase structure. In addition, styrene resin can form a stable resonance structure by capturing electrons through an aromatic ring, and thus the insulation of the insulating layer can be further improved. It should be noted that styrene resin does not have a melting point and heat of fusion.
[0072] Examples of styrene-based resins include styrene butadiene styrene block copolymers (SBS), hydrogenated styrene butadiene styrene block copolymers, styrene isoprene styrene copolymers (SIS), hydrogenated styrene isoprene styrene copolymers, hydrogenated styrene butadiene rubber, hydrogenated styrene isoprene rubber, styrene ethylene butene olefin crystalline block copolymers, etc. Two or more of these may be used in combination.
[0073] It should be noted that the "hydrogenation" mentioned here refers to hydrogenation of double bonds. For example, "hydrogenated styrene butadiene styrene block copolymer" refers to a polymer obtained by hydrogenating the double bonds of styrene butadiene styrene block copolymer. It should be noted that the double bonds of the aromatic rings possessed by styrene are not hydrogenated. "Hydrogenated styrene butadiene styrene block copolymer" can also be called styrene ethylene butylene styrene block copolymer (SEBS).
[0074] As the styrene resin, a substance that does not contain a double bond in the chemical structure other than the benzene ring is preferred. When a substance having a double bond is used, the resin component may be thermally degraded during the molding of the resin composition, and the properties of the obtained molded product may be reduced. In this regard, since the substance that does not contain a double bond has high resistance to thermal degradation, the properties of the molded product can be maintained at a high level.
[0075] The styrene content of the styrene resin is not particularly limited, but is preferably 5% by mass or more and 35% by mass or less from the viewpoint of controlling the crystal growth of the propylene resin and softening the molded body. It should be noted that the styrene content represents the mass ratio of the styrene unit in the component units constituting the styrene resin.
[0076] (Resistance-imparting agent)
[0077] The resistance-imparting agent is a component that covers the metal impurities present in the insulating layer to mitigate the rapid resistance change at the interface between the metal impurities and the insulating layer. Specifically, the resistance-imparting agent is a monomer having a phenolic skeleton and having hydrogen or an alkyl group having 1 to 3 carbon atoms bonded to at least one of the ortho positions of the hydroxyl group in the phenolic skeleton, a melting point of 215° C. or less, and a molecular weight of 200 to 500. Preferably, the resistance-imparting agent is a phenolic antioxidant having the above-mentioned melting point, molecular weight, and chemical structure.
[0078] The mechanism by which the resistance-imparting agent covers the metal impurities and alleviates the resistance change at the interface is presumed to be as follows.
[0079] Generally, since the melting point of propylene resin is about 140°C to 160°C, the resistance-imparting agent and the resin component containing the propylene resin are mixed while being heated at, for example, 200°C to 220°C. Therefore, the resistance-imparting agent having a melting point of 215°C or less tends to melt and become a liquid state during heating and mixing. The resistance-imparting agent has polarity due to the phenol skeleton and has a high affinity for metal impurities. Therefore, it is presumed that when heated and mixed with the resin component, it gathers around the metal impurities mixed in the resin component and covers the metal impurities.
[0080] Furthermore, the resistance-imparting agent has hydrogen or an alkyl group having 1 to 3 carbon atoms at at least one of the ortho positions of the hydroxyl group constituting the phenol skeleton, and no bulky substituent is arranged at least on one side of the ortho position of the hydroxyl group. That is, in the resistance-imparting agent, the steric hindrance around the hydroxyl group is small. Therefore, there is a tendency for the reactivity of the hydroxyl group in the resistance-imparting agent to become higher. In contrast, for example, in a monomer (so-called hindered phenol antioxidant) in which a bulky substituent (tert-butyl group, etc.) is arranged at two ortho positions of the hydroxyl group, the steric hindrance is large. In such a monomer, due to the steric hindrance, the reactivity of the hydroxyl group is hindered, and the affinity with the metal impurities becomes low. In this regard, according to the resistance-imparting agent of this embodiment, the steric hindrance is small and the reactivity of the hydroxyl group is high, so that the metal impurities can be more reliably coated compared with components with large steric hindrance such as hindered phenol antioxidants.
[0081] In addition, by setting the molecular weight of the tolerance-imparting agent to 200 or more, the volatilization of the tolerance-imparting agent can be suppressed when the mixed resin composition is heated. In addition, by setting the molecular weight to 500 or less, the tolerance-imparting agent can be appropriately moved in the resin component. As a result, the agglomeration of the tolerance-imparting agent in the resin composition can be suppressed and the tolerance-imparting agent can be uniformly dispersed, and the surface of the metal impurities present in the resin composition can be coated with the tolerance-imparting agent.
[0082] In addition, the tolerance imparting agent has polarity due to the phenol skeleton, so it can alleviate the rapid resistance change at the interface between the metal impurity and the insulating layer in a gradient manner. In addition, since it has an aromatic ring derived from the phenol skeleton, it can impart electrical stability to the vicinity of the metal impurity through the electron capture effect.
[0083] In this way, the resistance imparting agent can cover the metal impurities in the insulating layer, and acts to alleviate the resistance change at the interface between the metal impurities and the insulating layer and to concentrate the electric field on the metal impurities.
[0084] The molecular weight of the resistance-imparting agent is 200 to 500. The molecular weight of the resistance-imparting agent is preferably 300 to 450 from the viewpoint of suppressing volatilization of the resistance-imparting agent and suppressing aggregation of the resistance-imparting agent to disperse it in the resin composition.
[0085] The melting point of the resistance-imparting agent is not particularly limited as long as it is below 215°C, but is preferably below 130°C. By having a melting point below 130°C, the metal impurities can be more reliably coated with the resistance-imparting agent during the heating and mixing of the resin composition. Furthermore, it is better that the melting point is a temperature at which the resistance-imparting agent becomes a liquid at room temperature (27°C), and specifically, it is more preferably below 27°C. By having a melting point below 27°C, the resistance-imparting agent can flow even in the insulating layer, so that it remains around the metal impurities. As a result, the surface of the metal impurities can be more reliably coated, thereby further suppressing the decrease in insulation caused by the metal impurities. It should be noted that the lower limit is not particularly limited, but is preferably above -30°C.
[0086] In the tolerance-imparting agent, the number of phenol skeletons is not particularly limited as long as the molecular weight of the tolerance-imparting agent is within the range of 200 or more and 500 or less, and for example, 1 or 2 is preferable.
[0087] In addition, from the viewpoint of improving compatibility with the resin component, the tolerance imparting agent preferably has a linear carbon chain structure with a carbon number of 5 or more and 10 or less in the phenolic skeleton. By improving the compatibility of the tolerance imparting agent, the tolerance imparting agent can be uniformly present in the resin composition, so that the metal impurities can be more reliably coated. As long as the molecular weight of the tolerance imparting agent is within the above range, the number of linear carbon chain structures is not particularly limited, for example, one or two is better. From the viewpoint of satisfying the molecular weight range and improving compatibility, the number of linear carbon chain structures is preferably two. In addition, the linear carbon chain structure can be located on the other side of the ortho position of the hydroxyl group. This is because, in the ortho position of the hydroxyl group, if hydrogen or an alkyl group with a carbon number of 1 to 3 is present on at least one side, the decrease in reactivity caused by steric hindrance can be suppressed. In addition, the linear carbon chain structure can be directly bonded to the aromatic ring, or it can be bonded to the aromatic ring via other atoms such as sulfur atoms and nitrogen atoms.
[0088] The tolerance imparting agent is a monomer containing carbon atoms, hydrogen atoms, and oxygen atoms, and may contain sulfur atoms and nitrogen atoms in addition to these atoms, preferably sulfur atoms.
[0089] As a resistance imparting agent, it is not particularly limited as long as it satisfies the above-mentioned chemical structure, molecular weight and melting point. For example, 2-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2-hydroxy-4-n-octyloxybenzophenone, 2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,4-bis(octylthiomethyl)-6-methylphenol, nonylphenol, dinonylphenol, etc. can be used. Among them, 2,4-bis(octylthiomethyl)-6-methylphenol is preferred because of its high compatibility with the resin component due to the presence of sulfur atoms and a linear carbon chain structure with a carbon number of 5 or more and 10 or less in the chemical structure.
[0090] The content of the resistance imparting agent is 0.4 mass parts or more and 10 mass parts or less relative to 100 mass parts of the resin component. Preferably, it is 0.5 mass parts or more and 8 mass parts or less. By setting it to more than 0.4 mass parts, it is easy to coat the metal impurities with the resistance imparting agent, so the decline of the insulation caused by the metal impurities can be alleviated. In addition, when the addition amount of the resistance imparting agent is too much, it is difficult to shape the resin composition into an insulating layer, but by setting it to less than 10 mass parts, the moldability of the resin composition can be ensured.
[0091] (Other additives)
[0092] The resin composition may further contain other additives as necessary. Other additives may include an antioxidant, a copper damage inhibitor, a lubricant, and a colorant in addition to the above-mentioned resistance-imparting agent.
[0093] However, the resin composition preferably has a small content of an additive that functions as a nucleating agent for generating propylene crystals, and more preferably substantially contains no such additive. Specifically, for example, when the total content of the resin component is set to 100 parts by mass, the content of the additive that functions as a nucleating agent is preferably less than 1 part by mass, and more preferably 0 parts by mass. Thus, the occurrence of unexpected abnormal crystallization caused by the nucleating agent can be suppressed, and the amount of crystallization can be easily controlled.
[0094] In addition, from the viewpoint of recycling, the resin composition is preferably non-crosslinked without crosslinking, but may also contain a crosslinking agent in order to make it crosslinked. However, even if it is crosslinked, it is preferably crosslinked in a manner with a low gel fraction (crosslinking degree). Specifically, it is preferred to crosslink the crosslinking degree such that the residue of the crosslinking agent in the resin composition is less than 300ppm by mass ratio. It should be noted that, when dicumyl peroxide is used as a crosslinking agent, the residue is, for example, cumyl alcohol, α-methylstyrene, etc.
[0095] (Melting Point and Heat of Fusion of Resin Composition)
[0096] The melting point and heat of fusion of the resin composition vary according to the contents of the propylene resin and the low crystalline resin used as the resin component, and become an index of the resin composition. The melting point and heat of fusion of the resin composition are not particularly limited, but in the case of containing random PP as the propylene resin, it is preferred that the melting point is 140°C or more and 150°C or less, and the heat of fusion is 55J / g or more and 100J / g or less. More preferably, the melting point is 140°C or more and 148°C or less, and the heat of fusion is 55J / g or more and 95J / g or less. On the other hand, in the case of containing homopolymer PP as the propylene resin, it is preferred that the melting point is 158°C or more and 168°C or less, and the heat of fusion is 55J / g or more and 110J / g or less. More preferably, the melting point is 158°C or more and 165°C or less, and the heat of fusion is 55J / g or more and 100J / g or less. By blending at least one of the low-crystalline resin and the styrene-based resin and the propylene-based resin so as to achieve such a melting point and heat of fusion, it is possible to suppress excessive crystal growth of the propylene-based resin and obtain the characteristics of each resin.
[0097] It should be noted that the "melting point" and "heat of fusion" mentioned here are measured by differential scanning calorimetry (DSC). "Differential scanning calorimetry" is performed, for example, in accordance with JIS-K-7121 (1987). Specifically, in a DSC device, the measurement sample is heated from room temperature (normal temperature, such as 27°C) to 220°C at 10°C / min. Thus, the DSC curve is obtained by plotting the amount of heat absorbed (heat flow) per unit time relative to the temperature.
[0098] At this time, the temperature at which the heat absorption per unit time in the sample becomes maximum (highest peak) is defined as the "melting point (melting peak temperature)". In addition, at this time, it is assumed that the heat absorption of the sample is entirely carried out by the resin component, and the value (J / g) obtained by dividing the heat absorption (J) of the sample from room temperature to 220°C by the mass (g) of the entire resin component in the sample is defined as the "melting heat". It should be noted that the crystallinity (%) of the sample can be calculated based on the theoretical value of the melting heat of the sample and the melting heat of a completely crystalline body.
[0099] (Resin composition)
[0100] The content of each component contained in the resin composition is preferably appropriately changed in a manner that the melting point and heat of fusion of the resin composition become the above-mentioned range. For example, when the total of the propylene resin and the soft component comprising at least one of the low crystalline resin and the styrene resin is set to 100 parts by mass, the resin composition preferably comprises propylene resins of more than 55 parts by mass and less than 95 parts by mass, and soft components of more than 5 parts by mass and less than 45 parts by mass. More preferably, propylene resins of more than 60 parts by mass and less than 95 parts by mass, and soft components of more than 5 parts by mass and less than 40 parts by mass are included. By setting such an addition amount, the amount of crystallization can be adjusted to an appropriate range in the resin composition. As a result, when the insulating layer is formed with the resin composition, the formation of voids can be suppressed in the insulating layer. It should be noted that the addition ratio of the low crystalline resin and the styrene resin is not particularly limited, and the addition amount obtained by summing them up satisfies the above-mentioned range.
[0101] (2) Power cables
[0102] Next, use Figure 1 The power cable according to this embodiment will be described. Figure 1 This is a cross-sectional view perpendicular to the axial direction of the power cable according to the present embodiment.
[0103] The power cable 10 of this embodiment is configured as a so-called solid insulation power cable. The power cable 10 of this embodiment is configured to be laid on land (in a pipeline), in water or on the bottom of the water, for example. It should be noted that the power cable 10 is used for alternating current, for example.
[0104] Specifically, the power cable 10 includes, for example, a conductor 110 , an inner semiconductive layer 120 , an insulating layer 130 , an outer semiconductive layer 140 , a shielding layer 150 , and a jacket 160 .
[0105] (Conductor (conductive part))
[0106] The conductor 110 is formed by twisting a plurality of conductor core wires (conductive core wires) made of, for example, pure copper, copper alloy, aluminum, or aluminum alloy.
[0107] (Inner semi-conductive layer)
[0108] The inner semiconductive layer 120 is provided to cover the outer periphery of the conductor 110. The inner semiconductive layer 120 is configured to have semiconductivity and suppress electric field concentration on the surface side of the conductor 110. The inner semiconductive layer 120 includes, for example, ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-butyl acrylate copolymer, and ethylene-vinyl acetate copolymer, olefin-based elastomer, at least one of the above-mentioned low-crystalline resins, and conductive carbon black.
[0109] (Insulation layer)
[0110] Insulating layer 130 is provided to cover the outer periphery of inner semiconductive layer 120 and is constituted as the above-mentioned resin composition molded body. Insulating layer 130 is extrusion-molded from the resin composition as described above, for example.
[0111] (Outer semiconductive layer)
[0112] The outer semiconductive layer 140 is provided to cover the outer periphery of the insulating layer 130. The outer semiconductive layer 140 is configured to have semiconductivity and suppress electric field concentration between the insulating layer 130 and the shielding layer 150. The outer semiconductive layer 140 is formed of the same material as the inner semiconductive layer 120, for example.
[0113] (Shielding layer)
[0114] The shielding layer 150 is provided to cover the outer periphery of the outer semiconductive layer 140. The shielding layer 150 is formed, for example, by winding a copper tape, or is formed as a wire shield formed by winding a plurality of soft copper wires, etc. It should be noted that a tape made of a tape or the like may be wound inside and outside the shielding layer 150.
[0115] (jacket)
[0116] The sheath 160 is provided to cover the outer periphery of the shield layer 150. The sheath 160 is made of, for example, polyvinyl chloride or polyethylene.
[0117] It should be noted that if the power cable 10 of the present embodiment is an underwater cable or an underwater cable, it may have a so-called waterproof layer made of a metal such as aluminum or a wire armor outside the shield layer 150 .
[0118] On the other hand, the power cable 10 of the present embodiment may not have a waterproof layer outside the shield layer 150. That is, the power cable 10 of the present embodiment may be configured with a non-complete waterproof structure.
[0119] (Specific dimensions, etc.)
[0120] The specific dimensions of the power cable 10 are not particularly limited, for example, the diameter of the conductor 110 is 5 mm or more and 60 mm or less, the thickness of the inner semiconductive layer 120 is 0.5 mm or more and 3 mm or less, the thickness of the insulating layer 130 is 3 mm or more and 35 mm or less, the thickness of the outer semiconductive layer 140 is 0.5 mm or more and 3 mm or less, the thickness of the shielding layer 150 is 0.1 mm or more and 5 mm or less, and the thickness of the sheath 160 is 1 mm or more. The AC voltage applicable to the power cable 10 of this embodiment is, for example, 20 kV or more.
[0121] (3) Cable characteristics
[0122] In the present embodiment, by configuring the insulating layer 130 (resin composition molded body) to include the above-mentioned resistance imparting agent, the following insulation properties can be obtained.
[0123] The insulating layer 130 of the present embodiment shows high insulation when the proportion of metal impurities is less than 0.02% by volume. Specifically, for the sample, at room temperature, an AC voltage of a commercial frequency (e.g., 60 Hz) is applied under the conditions of applying a voltage of 10 kV for 10 minutes and then repeatedly increasing the voltage by 1 kV each time and applying the voltage for 10 minutes. At this time, the AC breakdown electric field strength is more than 45 kV / mm, wherein the sample is a 0.4 mm thick sheet formed by the above-mentioned resin composition and a copper sheet with a diameter of less than 200 μm is buried as a metal impurity. That is, if the proportion of metal impurities is less than 0.02% by volume, the desired AC breakdown electric field strength can be obtained in the insulating layer, and high insulation can be ensured.
[0124] (4) Manufacturing method of power cable
[0125] Next, a method for manufacturing a power cable according to the present embodiment will be described. Hereinafter, the step will be simply referred to as "S".
[0126] (S100: Resin composition preparation step)
[0127] First, a resin composition for forming the insulating layer 130 is prepared.
[0128] In this embodiment, a mixer is used to mix (knead) a propylene resin as a resin component, a soft component including at least one of a low-crystalline resin and a styrene resin, a resistance-imparting agent, and other additives as needed to form a mixed material. During kneading, the melted resistance-imparting agent gathers around the metal impurities contained in the resin component, thereby coating the metal impurities. As a mixer, for example, an open mill, a Banbury mixer, a pressure kneading machine, a single-screw mixer, a multi-screw mixer, etc. can be listed.
[0129] At this time, regarding the addition amount of each resin, for example, when the total content of the propylene resin and the soft component containing at least one of the low-crystalline resin and the styrene resin is 100 parts by mass, the propylene resin is preferably 55 parts by mass or more and 95 parts by mass or less, and the soft component is preferably 5 parts by mass or more and 45 parts by mass or less. In addition, when the total content of the propylene resin and the soft component is 100 parts by mass, the content of the tolerance imparting agent is preferably 0.4 parts by mass or more and 10 parts by mass or less.
[0130] After the mixed material is formed, the mixed material is granulated by an extruder, thereby forming a granular resin composition that will constitute the insulating layer 130. It should be noted that a twin-screw extruder with a high kneading effect can also be used to perform the steps from mixing to granulation at the same time.
[0131] In this embodiment, when the resin component and the resistance-imparting agent are heated and mixed, the resistance-imparting agent can be melted to cover the surface of the metal impurities mixed in the resin component. In the resin composition, the resistance-imparting agent is dispersed in the resin component and is sandwiched at the interface between the metal impurities and the resin component.
[0132] (S200: conductor preparation process)
[0133] On the other hand, a conductor 110 formed by twisting a plurality of conductor core wires is prepared.
[0134] (S300: Cable core forming process (extrusion process, insulation layer forming process))
[0135] After the resin composition preparation step S100 and the conductor preparation step S200 are completed, the insulating layer 130 is formed using the above-mentioned resin composition so as to cover the outer circumference of the conductor 110 with a thickness of 3 mm or more.
[0136] At this time, for example, a three-layer simultaneous extruder is used to simultaneously form the inner semiconductive layer 120 , the insulating layer 130 , and the outer semiconductive layer 140 .
[0137] Specifically, in a three-layer simultaneous extruder, for example, the composition for the internal semiconductive layer is fed into the extruder A for forming the internal semiconductive layer 120 .
[0138] The pelletized resin composition is introduced into the extruder B for forming the insulating layer 130. The set temperature of the extruder B is set to a temperature 10° C. or higher and 50° C. or lower than the desired melting point. The set temperature is preferably adjusted appropriately based on the line speed and extrusion pressure.
[0139] Into the extruder C for forming the outer semiconductive layer 140 , a composition for an outer semiconductive layer containing the same materials as the resin composition for an inner semiconductive layer fed into the extruder A is fed.
[0140] Next, the extrudates from the extruders A to C are directed to a common head, and the inner semiconductive layer 120, the insulating layer 130, and the outer semiconductive layer 140 are simultaneously extruded from the inside to the outside to the outer periphery of the conductor 110. Thus, an extruded material that becomes a cable core is formed.
[0141] Thereafter, the extruded material is cooled, for example using water.
[0142] Through the above cable core forming step S300 , a cable core including the conductor 110 , the inner semiconductive layer 120 , the insulating layer 130 , and the outer semiconductive layer 140 is formed.
[0143] (S400: Shielding Layer Forming Step)
[0144] After the cable core is formed, the shielding layer 150 is formed by winding, for example, a copper tape around the outside of the outer semiconductive layer 140 .
[0145] (S500: Sheath Forming Step)
[0146] After the shield layer 150 is formed, vinyl chloride is put into an extruder and extruded, thereby forming the sheath 160 on the outer periphery of the shield layer 150 .
[0147] In the above manner, the power cable 10 as a solid insulated power cable is manufactured.
[0148] (4) Effects of this embodiment
[0149] According to the present embodiment, one or more of the following effects are achieved.
[0150] (a) The insulating layer of the present embodiment is formed by a resin composition, which contains a resin component and a resistance-imparting agent in a manner that the content of the resistance-imparting agent is 0.4 to 10 parts by mass relative to 100 parts by mass of the resin component. The resin component contains at least one of a low-crystalline resin and a styrene-based resin and a propylene-based resin, and the resistance-imparting agent has a specified molecular weight, melting point, and chemical structure. According to the low-crystalline resin and the styrene-based resin, the excessive crystal growth of the propylene-based resin can be suppressed, and the insulation of the insulating layer can be improved. According to the resistance-imparting agent with a specified melting point and chemical structure, it can be melted when heated and mixed with the resin component to cover the surface of the metal impurities mixed into the resin component. That is, the resistance-imparting agent can be sandwiched at the interface between the metal impurities and the resin component. The resistance-imparting agent has an aromatic ring derived from a phenolic skeleton and polarity, and therefore, by alleviating the sharp resistance change between the resin component and the metal impurities, it also alleviates the electric field concentration to the metal impurities, and can suppress the decrease in insulation caused by the metal impurities. As described above, according to the insulating layer of this embodiment, when the content ratio of metal impurities is within the range of 0.02% by volume or less, the metal impurities are coated with the resistance imparting agent, thereby suppressing the decrease in insulation due to the metal impurities and stably achieving high insulation.
[0151] (b) The melting point of the resistance-imparting agent is preferably 130° C. or less, and more preferably a melting point at which the agent becomes liquid at 27° C. The resistance-imparting agent having such a melting point can more reliably cover the surface of the metal impurities during the heating and mixing of the resin composition, and can further improve the insulation properties of the insulating layer.
[0152] (c) The resistance-imparting agent preferably has a linear carbon chain structure having a carbon number of 5 or more and 10 or less. In addition, the resistance-imparting agent preferably contains a sulfur atom. Such a resistance-imparting agent has excellent compatibility with the resin component, and therefore, is easily coated with metal impurities during heating and mixing of the resin composition, and can impart electrical stability to the insulating layer.
[0153] (d) The resin composition preferably contains random PP as the propylene-based resin. Random PP can suppress cracks in the insulating layer compared to homo-PP, and can provide higher insulation properties.
[0154] (e) The resin composition preferably contains random PP and a styrene resin, or random PP, a low-crystalline resin and a styrene resin. By using at least random PP and a styrene resin, the growth of coarse crystals of the propylene resin can be easily suppressed, and high insulation can be obtained in the insulating layer.
[0155] (f) The resin composition preferably contains random PP as a propylene resin and a soft component (the soft component is a low-crystalline resin, a styrene resin) at a ratio such that the melting point of the resin composition is 140°C to 150°C and the heat of fusion is 55 J / g to 100 J / g. In addition, the resin composition preferably contains homopolymer PP as a propylene resin and a soft component (the soft component is a low-crystalline resin, a styrene resin) at a ratio such that the melting point of the resin composition is 158°C to 168°C and the heat of fusion is 55 J / g to 110 J / g. By including the components at a ratio such that the heat of fusion and the melting point of the resin composition are within the above range, excessive crystal growth of the propylene resin can be suppressed in the insulating layer, and higher insulation can be obtained in the insulating layer.
[0156] (g) The resin composition preferably contains acryl resin, low-crystalline resin and styrene resin as resin components. Thus, compared with the case where only low-crystalline resin or styrene resin is added, the crystal growth of the acryl resin can be further controlled, and higher insulation can be obtained in the insulating layer.
[0157] <Other embodiments of the present disclosure>
[0158] As mentioned above, although embodiment of this disclosure was specifically described, this disclosure is not limited to the said embodiment, Various changes are possible within the range which does not deviate from the summary.
[0159] In the above embodiment, the case where the resin composition molded product as the insulating layer is a resin composition molded product obtained by mechanical mixing and extrusion molding has been described, but the resin composition molded product may be a resin composition molded product obtained by polymerization and extrusion molding.
[0160] In the above-mentioned embodiment, the case where the power cable 10 may not have a waterproof layer is described, but the present disclosure is not limited to this case. Since the power cable 10 has the above-mentioned significant water tree suppression effect, it may also have a simple waterproof layer. Specifically, the simple waterproof layer is composed of, for example, a metal laminate tape. The metal laminate tape, for example, has a metal layer composed of aluminum or copper, and an adhesive layer provided on one or both sides of the metal layer. The metal laminate tape is, for example, longitudinally added and wound to surround the outer periphery of the cable core (closer to the outer periphery than the outer semiconductive layer). It should be noted that the waterproof layer can be provided on the outside of the shielding layer, and can also serve as a shielding layer. Through such a structure, the cost of the power cable 10 can be reduced.
[0161] In the above-mentioned embodiment, the case where the power cable 10 is configured to be laid on land, in water, or on the bottom of the water is described, but the present disclosure is not limited to this case. For example, the power cable 10 may be configured as a so-called overhead wire (overhead insulated wire).
[0162] In the above-mentioned embodiment, three layers are extruded simultaneously in the cable core forming step S300 , but they may be extruded layer by layer.
[0163] Example
[0164] Next, embodiments of the present disclosure will be described. These embodiments are examples of the present disclosure, and the present disclosure is not limited to these embodiments.
[0165] (1) Preparation of evaluation samples
[0166] In this example, an evaluation sample simulating an insulation layer of a power cable was prepared by the following steps: In this example, in order to evaluate the change in insulation due to the mixing of metal impurities, metal powder was added as metal impurities to the resin composition to prepare the evaluation sample.
[0167] (1-1) Materials
[0168] The following components were prepared as materials for forming the resin composition of the evaluation sample.
[0169] As the propylene resin (A), the following were used.
[0170] Isotactic propylene homopolymer (homo-PP): melt flow rate: 0.5 g / 10 min, density: 0.9 g / ml, melting point: 165°C, heat of fusion: 115 J / g.
[0171] Random polypropylene (random PP): melt flow rate: 1.3 g / 10 min, density: 0.9 g / ml, melting point: 145°C, heat of fusion: 100 J / g.
[0172] As the low-crystalline resin (B), the following were used.
[0173] Ethylene propylene rubber (EPR): ethylene content: 52% by mass, Mooney viscosity ML (1+4) 100°C: 40, melting point: none, heat of fusion: none.
[0174] As the styrene-based resin (C), the following were used.
[0175] Hydrogenated styrene-based thermoplastic elastomer (SEBS): Styrene content: 12% by mass, hardness: A42, melt flow rate: 4.5 g / 10 min (230° C., 2.16 kg), melting point: none, heat of fusion: none.
[0176] The following substances were used as the tolerance imparting agent (D) and the comparative component (D′) serving as a comparative form of the component (D).
[0177] In addition, as a metal powder, what was used was the copper powder obtained by cutting a copper material with a metal file, and the copper powder was sieved with a sieve with a mesh size of 200 μm.
[0178] [Table 1]
[0179]
[0180] In Table 1, the phenol number indicates the number of phenol skeletons in the compound, and 0 is indicated as "-". The hydroxyl surrounding indicates whether there is steric hindrance at the hydroxyl group, and the case of small steric hindrance is indicated as "-", the case where a bulky substituent is located on one side of the ortho position of the hydroxyl group is indicated as "single hindered", and the case where a bulky substituent is located on both sides of the ortho position is indicated as "hindered". In addition, regarding the tolerance imparting agent (d6) and the tolerance imparting agent (d'9), they are liquid at room temperature (27°C), so the boiling point (bp) is shown.
[0181] (1-2) Preparation of resin composition
[0182] The above materials were heated and mixed according to the formulations shown in Tables 2 to 7 below to prepare resin compositions.
[0183] [Table 2]
[0184]
[0185] [Table 3]
[0186]
[0187] [Table 4]
[0188]
[0189] [Table 5]
[0190]
[0191] [Table 6]
[0192]
[0193] [Table 7]
[0194]
[0195] (Samples 1 to 6)
[0196] In sample 1, as shown in Table 2, 75 parts by mass of isotactic propylene homopolymer (homo PP) as propylene resin (A), 25 parts by mass of ethylene propylene rubber (EPR) as low crystalline resin (B), and 6 parts by mass of component (d1) shown in Table 1 as resistance imparting agent (D) are mixed. Furthermore, copper powder is added to the mixture in such a manner that the content of copper powder becomes 0.02% by volume ratio of the resin composition. Then, the mixture is heated and mixed at 220°C using a kneader, thereby preparing a resin composition. In addition, in sample 2, the resistance imparting agent (D) is not added, and the resin composition is prepared in the same manner as sample 1. In samples 3 to 6, the addition amount of component (d1) is changed to 0.3 parts by mass, 0.5 parts by mass, 9 parts by mass, and 12 parts by mass, respectively, and the resin composition is prepared in the same manner as sample 1.
[0197] (Samples 7 to 15)
[0198] In Samples 7 to 15, resin compositions were prepared in the same manner as in Sample 1 except that the type of the resistance-imparting agent (D) was changed to (d2) to (d8) as shown in Tables 3 and 4, and the amount of each resistance-imparting agent added was appropriately changed.
[0199] (Samples 16 to 18)
[0200] In samples 16 and 17, as shown in Table 5, the type of propylene resin (A) was changed from homo-PP to random polypropylene (random PP), and the addition amount of each component was changed, and the resin composition was prepared in the same manner as sample 1. In sample 18, the resin composition was prepared in the same manner as samples 16 and 17, except that the resistance imparting agent (D) was not added.
[0201] (Samples 19-21)
[0202] In samples 19 and 20, as shown in Table 5, a styrene resin (C) was further added as a resin component, and the addition amount of each component was appropriately changed, and a resin composition was prepared in the same manner as sample 16. In sample 21, a resin composition was prepared in the same manner as samples 19 and 20, except that no resistance-imparting agent (D) was added.
[0203] (Samples 22 to 31)
[0204] In Samples 22 to 31, resin compositions were prepared in the same manner as in Sample 1 except that the components (d′1) to (d′10) as comparative components (D′) were used instead of the resistance imparting agent (D) and the amounts added were appropriately changed as shown in Tables 6 and 7.
[0205] (1-3) Preparation of evaluation samples
[0206] Next, the prepared resin compositions of samples 1 to 31 were pressure-molded at 220° C., and slowly cooled by water cooling under pressure, thereby producing sheet-shaped evaluation samples with a thickness of 0.4 mm. It should be noted that in the production of the evaluation samples, the resin composition was extruded in such a way that copper powder with a diameter of less than 200 μm was arranged in the center of the sheet. It should be noted that the evaluation samples were produced without copper powder in samples 18 and 21.
[0207] (2) Evaluation
[0208] The following items were evaluated for the prepared evaluation samples.
[0209] (Melting point and heat of fusion)
[0210] The melting point and heat of fusion of the produced evaluation samples were measured.
[0211] The melting point of each evaluation sample is obtained by DSC measurement. The DSC measurement is carried out in accordance with JIS-K-7121 (1987). Specifically, as a DSC device, DSC8500 (input compensation type) manufactured by Perkin Elmer was used. The reference sample is set to α-alumina, for example. The mass of the evaluation sample is set to 8 to 10 g. In the DSC device, the temperature is raised from room temperature (27°C) to 220°C at 10°C / min. Thus, the DSC curve is obtained by plotting the amount of heat absorbed (heat flow) per unit time relative to the temperature.
[0212] At this time, the temperature at which the endothermic amount per unit time in each evaluation sample becomes maximum (highest peak) is defined as the “melting point.” In addition, at this time, the “heat of fusion” is determined by determining the area of the region surrounded by the melting peak and the baseline in the DSC curve.
[0213] (AC breakdown electric field strength)
[0214] Regarding the insulation of the evaluation samples produced, the AC breakdown electric field strength was measured. The AC breakdown electric field strength was obtained by an AC breakdown test. Specifically, at room temperature (27°C), an AC voltage of a commercial frequency (e.g., 60 Hz) was applied to the evaluation samples under the condition of applying a voltage of 10 kV for 10 minutes and then repeatedly increasing the voltage by 1 kV each time and applying the voltage for 10 minutes. The electric field strength when the insulation breakdown occurred in the evaluation samples was measured. In this embodiment, if the AC breakdown electric field strength is 45 kV / mm or more, it is considered good.
[0215] (3) Evaluation results
[0216] Tables 2 to 7 show the results of the above-mentioned evaluations for each evaluation sample.
[0217] According to samples 1 to 6, it was confirmed that: compared with sample 2 without adding the resistance imparting agent (D) and sample 3 with an addition amount of 0.3 mass parts, samples 1, 4, and 5 in which the addition amount of the resistance imparting agent (D) was set to 0.4 mass parts to 10 mass parts, the AC breakdown electric field strength was high and the insulation was excellent. It can be considered that this is because in samples 1, 4, and 5, the metal impurities can be coated by the resistance imparting agent (D), which can suppress the decrease in insulation caused by the metal impurities. It should be noted that in sample 6, the addition amount of the resistance imparting agent (D) was excessive to 12 mass parts, so the evaluation sample could not be formed into a sheet, and the insulation could not be evaluated.
[0218] In addition, in samples 1, 7 to 10, and 13 to 15, the type of the resistance imparting agent (D) was appropriately changed, but it was confirmed that the AC breakdown electric field strength was high and high insulation properties could be obtained. In addition, according to sample 10, it was confirmed that a higher AC breakdown electric field strength could be obtained compared with other samples. Therefore, it was confirmed that as the resistance imparting agent (D), a resistance imparting agent having a sulfur atom and a linear carbon chain structure with 5 or more and 10 or less carbon atoms in the chemical structure is preferred.
[0219] Moreover, according to Samples 10 to 12, it was confirmed that, similarly to Samples 1 to 6, high insulation properties can be obtained by adjusting the amount of the resistance imparting agent (D) added to an appropriate amount.
[0220] According to samples 16 and 17, it was confirmed that by using random PP as the propylene resin, the AC breakdown electric field strength can be further improved compared with sample 1 using homopolymer PP. In addition, according to samples 19 and 20, it was confirmed that by adding a styrene resin together with a low crystalline resin to the propylene resin, the AC breakdown electric field strength can be improved in the same manner as samples 16 and 17. In contrast, in samples 18 and 21 to which a tolerance imparting agent (D) was not added, it was confirmed that due to the influence of metal impurities, the AC breakdown electric field strength was lower than 45 kV / mm, and the insulation was lowered compared with samples 16, 17, 19, and 20. It should be noted that when the same resin composition as samples 18 and 21 was used and copper powder was not added, it was confirmed that the AC breakdown electric field strength became 66 kV / mm and 68 kV / mm, and the desired insulation could be obtained in the absence of metal impurities.
[0221] In samples 22 to 31, it was confirmed that, as shown in Tables 6 and 7, the insulating properties were significantly reduced because the comparative component (D') having a molecular weight outside the range of 200 to 500, having no phenolic skeleton, generating steric hindrance around the hydroxyl group, or having a melting point higher than 215° C. was used. This is considered to be because the comparative component (D') could not sufficiently cover the surface of the metal impurities during heating and mixing, or even if it was covered, it could not sufficiently alleviate the resistance change between the metal impurities and the resin component.
[0222] As described above, it was confirmed that by adding a predetermined amount of a resistance-imparting agent having a predetermined chemical structure, molecular weight and melting point to a resin component containing propylene units, high insulation properties can be stably achieved in the insulating layer as long as the content of metal impurities is within a range of 0.02% by volume or less.
[0223] <Preferred embodiment of the present disclosure>
[0224] Preferred aspects of the present disclosure are described below.
[0225] (Note 1)
[0226] A resin composition comprising a resin component containing propylene units and a resistance-imparting agent, wherein the resistance-imparting agent is a monomer having a phenolic skeleton and having hydrogen or an alkyl group having 1 to 3 carbon atoms bonded to at least one of the ortho positions of a hydroxyl group in the phenolic skeleton, the melting point being 215° C. or lower and the molecular weight being 200 to 500, the content of the resistance-imparting agent being 0.4 to 10 parts by mass based on 100 parts by mass of the resin component, and the content ratio of metal impurities being 0.02% or less by volume.
[0227] (Note 2)
[0228] A power cable comprises: a conductor; and an insulating layer covering the outer periphery of the conductor, wherein the insulating layer is formed of a resin composition, the resin composition containing a resin component containing a propylene unit and a resistance-imparting agent, the resistance-imparting agent is a monomer having a phenolic skeleton and having a hydrogen or an alkyl group having 1 to 3 carbon atoms bonded to at least one of the ortho positions of a hydroxyl group in the phenolic skeleton, the melting point being 215° C. or less, and the molecular weight being 200 to 500, the content of the resistance-imparting agent being 0.4 to 10 parts by mass relative to 100 parts by mass of the resin component, and the content ratio of metal impurities being 0.02% or less by volume.
[0229] (Note 3)
[0230] The electric power cable according to Supplementary Note 2, wherein the resin component contains at least one of an ethylene unit and a styrene unit.
[0231] (Note 4)
[0232] The electric power cable according to Supplementary Note 2 or 3, wherein the resistance imparting agent has a melting point at which it becomes a liquid state at 27°C.
[0233] (Note 5)
[0234] The electric power cable according to any one of Appendix 2 to 4, wherein the resistance imparting agent has a linear carbon chain structure having 5 to 10 carbon atoms.
[0235] (Note 6)
[0236] The electric power cable according to any one of Supplementary Notes 2 to 5, wherein the resistance-imparting agent contains a sulfur atom.
[0237] (Note 7)
[0238] The electric power cable according to any one of Supplementary Notes 2 to 6, wherein the resistance imparting agent is a phenolic antioxidant.
[0239] (Note 8)
[0240] The power cable according to any one of Notes 2 to 7, wherein the resin composition comprises: a propylene homopolymer having a melting point of 160°C to 175°C and a heat of fusion of 100 J / g to 120 J / g as a propylene-based resin, and the resin composition has a melting point of 158°C to 168°C and a heat of fusion of 55 J / g to 110 J / g.
[0241] (Note 9)
[0242] The power cable according to any one of Notes 2 to 7, wherein the resin composition comprises: a propylene random copolymer as a propylene-based resin with a melting point of 140°C to 155°C and a heat of fusion of 90 J / g to 105 J / g, and the resin composition has a melting point of 140°C to 150°C and a heat of fusion of 55 J / g to 100 J / g.
[0243] (Note 10)
[0244] A method for manufacturing a power cable comprises the following steps: preparing a resin composition by mixing a propylene resin, a softening component including at least one of a low-crystalline resin and a styrene resin, and a resistance-imparting agent; and coating a conductor with an insulating layer using the resin composition, wherein the resistance-imparting agent is a monomer having a phenolic skeleton and having hydrogen or an alkyl group having 1 to 3 carbon atoms bonded to at least one of the ortho positions of a hydroxyl group in the phenolic skeleton, and having a melting point of 215° C. or less and a molecular weight of 200 to 500. In the step of preparing the resin composition, 0.4 to 10 parts by mass of the resistance-imparting agent is added to 100 parts by mass of the resin component including the propylene resin and the softening component.
[0245] (Note 11)
[0246] The method for manufacturing a power cable according to Appendix 10, wherein, in the step of preparing the resin composition, when the total of the propylene resin and the soft component is set to 100 parts by mass, 55 parts by mass or more and 95 parts by mass or less of the propylene resin and 5 parts by mass or more and 45 parts by mass or less of the soft component are mixed.
[0247] (Note 12)
[0248] A method for manufacturing a power cable according to Note 10 or 11, wherein the propylene resin is a propylene homopolymer having a melting point of 160°C to 175°C and a heat of fusion of 100 J / g to 120 J / g, and in the step of preparing the resin composition, the propylene resin and the soft component are mixed in such a manner that the melting point of the resin composition is 158°C to 168°C and the heat of fusion is 55 J / g to 110 J / g.
[0249] (Note 13)
[0250] A method for manufacturing a power cable according to Note 10 or 11, wherein the propylene-based resin is a propylene random copolymer having a melting point of 140°C to 155°C and a heat of fusion of 90 J / g to 105 J / g, and in the step of preparing the resin composition, the propylene-based resin and the soft component are mixed in such a manner that the melting point of the resin composition is 140°C to 150°C and the heat of fusion is 55 J / g to 100 J / g.
[0251] Description of Reference Numerals
[0252] 10: Power cable
[0253] 110: Conductor
[0254] 120: Inner semi-conductive layer
[0255] 130: Insulation layer
[0256] 140: Outer semi-conductive layer
[0257] 150: Shielding layer
[0258] 160: Sheath.
Claims
1. A resin composition comprising a resin component containing propylene units and a resistance-imparting agent, The resin component contains an acrylic resin and a soft component, wherein the soft component contains at least one of a low-crystalline resin and a styrene resin. The tolerance imparting agent is a monomer having a phenol skeleton and a hydrogen or carbon 1-3 alkyl group bonded to at least one of the ortho positions of the hydroxyl group in the phenol skeleton, having a melting point of 215° C. or less and a molecular weight of 200 or more and 500 or less. The content of the resistance-imparting agent is 0.4 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the resin component. The resin composition contains metal impurities, and the content of the metal impurities is 0.02% or less by volume.
2. A power cable having: Conductors; and An insulating layer, covering the outer periphery of the conductor, The insulating layer is formed from the resin composition according to claim 1.
3. The power cable according to claim 2, wherein: The resin component includes at least one of an ethylene unit and a styrene unit.
4. The power cable according to claim 2 or 3, wherein: The tolerance-imparting agent has a linear carbon chain structure having 5 to 10 carbon atoms.
5. The power cable according to any one of claims 2 to 4, wherein: The resistance-imparting agent contains a sulfur atom.
6. The power cable according to any one of claims 2 to 5, wherein: The tolerance-imparting agent has a melting point at 27° C. where it becomes a liquid state.
7. The power cable according to any one of claims 2 to 6, wherein: The tolerance-imparting agent is a phenolic antioxidant.
8. The power cable according to any one of claims 2 to 7, wherein: The resin composition comprises: a propylene homopolymer having a melting point of 160° C. to 175° C. and a heat of fusion of 100 J / g to 120 J / g as a propylene-based resin; The resin composition has a melting point of 158° C. to 168° C., and a heat of fusion of 55 J / g to 110 J / g.
9. The power cable according to any one of claims 2 to 7, wherein: The resin composition comprises: a propylene random copolymer having a melting point of 140° C. or higher and 155° C. or lower and a heat of fusion of 90 J / g or higher and 105 J / g or lower as a propylene-based resin; The resin composition has a melting point of 140° C. to 150° C., and a heat of fusion of 55 J / g to 100 J / g.