A high entropy hydrogen storage alloy and preparation method thereof

By optimizing the composition and preparation method of high-entropy hydrogen storage alloys, the shortcomings of existing hydrogen storage materials in terms of capacity, activation performance and cycle life have been solved, an efficient hydrogen absorption and release process and stable cycle performance have been achieved, meeting the needs of high-capacity and low cost requirements.

CN116397150BActive Publication Date: 2024-10-25JIANGXI INST OF RARE EARTHS CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310501531.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-10-25
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

Existing hydrogen storage materials are difficult to meet the requirements for high capacity, activation performance and cycle life, which hinders the further development of hydrogen storage materials.

Method used

The general formula of the high-entropy hydrogen storage alloy is TiaCrbVcMndMoeCef. By optimizing the proportion of each component and the preparation method, including smelting, packaging, annealing and other steps, the lattice structure and element ratio of the alloy are controlled to improve the stability of the alloy. Activation performance and cycle performance.

Benefits of technology

It achieves excellent stability, activation performance and cycle performance of high-entropy hydrogen storage alloy. The maximum hydrogen absorption capacity is higher than 3.5wt%, the effective hydrogen release capacity is higher than 2.4wt%, and hydrogen absorption and release can be achieved at normal temperature, reducing the Difficulty and cost of alloy activation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116397150B_ABST
    Figure CN116397150B_ABST
Patent Text Reader

Abstract

The present invention provides a high entropy hydrogen storage alloy and a preparation method thereof. The high entropy hydrogen storage alloy has a general composition formula of Ti a Cr b V c Mn d Mo e Ce f ; Wherein 0.3≤a≤0.5, 0.05≤b≤0.2, 0.2≤c≤0.3, 0.25≤d≤0.4, 0.05≤e≤0.1, 0.01≤f≤0.03. It has excellent hydrogen absorption and desorption performance, with a maximum hydrogen absorption capacity of ≥3.5wt%, an effective hydrogen desorption capacity of ≥2.4wt%, a room temperature hydrogen desorption platform pressure of ≥0.2MPa, and a maximum hydrogen absorption capacity of ≥3.2wt% after 100 cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogen storage alloys, and in particular relates to a high entropy hydrogen storage alloy and a preparation method thereof. Background Art

[0002] At present, human beings mainly rely on non-renewable energy such as mineral fuels (such as oil, natural gas and coal) to meet the energy needs of modern life. According to estimates, by the middle of this century, oil resources will be exhausted. Faced with the severe challenge of the shortage of traditional energy, various countries are actively developing renewable energy such as solar energy, wind energy and ocean energy (including tidal energy and wave energy). At the same time, fuels such as hydrogen and methanol have also received widespread attention as substitutes for gasoline and diesel.

[0003] Hydrogen energy, wind energy, solar energy, ocean energy, etc. are considered to be the most promising green energy. At present, hydrogen storage alloys are divided into five categories according to the main types of constituent elements: rare earth alloys, titanium iron alloys, zirconium alloys, magnesium alloys, and vanadium alloys. The biggest disadvantage of rare earth alloys is that their capacity is too small to meet the demand for high capacity, and the unit cell volume expands greatly during the hydrogen absorption and desorption cycle; titanium zirconium hydrogen storage alloys are actually a Laves phase that can absorb hydrogen, with advantages such as high hydrogen storage capacity and long cycle life, but there are also some difficult to overcome disadvantages such as difficulty in activation and high price; titanium iron alloys can reversibly absorb and desorb hydrogen in large quantities, and the two elements are abundant in nature, but their activation is more difficult; magnesium hydrogen storage alloys have abundant resources and high hydrogen storage capacity, but the hydrogen absorption / desorption kinetics of this type of alloy are poor.

[0004] Vanadium-based BCC alloys have a high hydrogen storage capacity. Currently developed BCC (Body-Centered Cubic (lattice)) solid solution hydrogen storage alloys are mainly concentrated in V-Ti, V-Ti-Cr, V-Ti-Fe and V-Ti-Cr-Fe, among which the alloys containing Fe are particularly popular. Although V-Fe alloys improve hydrogen absorption and desorption kinetics and cycle life, they are difficult to activate.

[0005] Existing hydrogen storage materials are difficult to meet current application requirements, which hinders the further development of hydrogen storage materials. Therefore, developing a new type of hydrogen storage material is a technical problem that those skilled in the art need to solve urgently. Summary of the invention

[0006] The purpose of the present invention is to provide a high entropy hydrogen storage alloy and a preparation method thereof. By optimizing the design of each component, the high entropy hydrogen storage alloy provided has excellent stability, activation performance and cycle performance, and also has the excellent mechanical properties of high entropy alloys. The preparation method provided is simple in process and low in cost.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a high entropy hydrogen storage alloy, wherein the general composition formula of the high entropy hydrogen storage alloy is Ti a Cr b V c Mn d Mo e Ce f ; Among them, 0.3≤a≤0.5, 0.05≤b≤0.2, 0.2≤c≤0.3, 0.25≤d≤0.4, 0.05≤e≤0.1, 0.01≤f≤0.03.

[0009] The high entropy hydrogen storage alloy provided by the present invention has excellent stability, activation performance and cycle performance through the optimization design of each component, and also has excellent mechanical properties of the high entropy alloy. The present invention dopes the rare earth element Ce into the hydrogen storage material high entropy alloy to obtain the rare earth high entropy alloy, which can further reduce the temperature used during activation and improve the stability performance.

[0010] The platform pressure of the high entropy hydrogen storage alloy in the process of dehydrogenation can reach above 0.2 MPa, and the temperature in the process of hydrogen absorption and dehydrogenation is as low as below 30° C., so that the process of hydrogen absorption and dehydrogenation of the high entropy hydrogen storage alloy is simple and easy to operate, and the alloy is easier to activate.

[0011] In the present invention, the ratio of Ti element in the high entropy hydrogen storage alloy is 0.3≤a≤0.5, for example, it can be 0.32, 0.34, 0.36, 0.38, 0.4, 0.42, 0.44, 0.46 or 0.48, etc.; the ratio of Cr element in the high entropy hydrogen storage alloy is 0.05≤b≤0.2, for example, it can be 0.07, 0.09, 0.1, 0.12, 0.14, 0.16, 0.18 or 0.19, etc.; the ratio of V element in the high entropy hydrogen storage alloy is 0.2≤c≤0.3, for example, it can be 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28 or 0.29, etc.; The proportion of Mn elements in the high entropy hydrogen storage alloy is 0.25≤d≤0.4, for example, it can be 0.27, 0.29, 0.3, 0.32, 0.34, 0.36, 0.38 or 0.39; the proportion of Mo elements in the high entropy hydrogen storage alloy is 0.05≤e≤0.1, for example, it can be 0.06, 0.07, 0.08 or 0.09; the proportion of Ce elements in the high entropy hydrogen storage alloy is 0.01≤f≤0.03, for example, it can be 0.012, 0.014, 0.016, 0.018, 0.02, 0.024, 0.026 or 0.028, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0012] As a preferred technical solution of the present invention, the high entropy hydrogen storage alloy has the following molar ratios: 0.3≤a≤0.4, 0.07≤b≤0.12, 0.2≤c≤0.3, 0.27≤d≤0.32, 0.05≤e≤0.1, and 0.01≤f≤0.03.

[0013] Preferably, in the high entropy hydrogen storage alloy, the molar ratio is: 0.75≤(a+b+e) / (c+d+f)≤0.85, for example, it can be 0.76, 0.77, 0.78, 0.79, 0.8, 0.81, 0.82, 0.83 or 0.84, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0014] It is worth noting that the present invention further controls the ratio of (Ti+Cr+Mo) / (V+Mn+Ce) within the range of 0.75 to 0.85. By adjusting the ratio of each element in the alloy, the alloy can have a single BCC phase structure, and the appropriate lattice constant of the alloy makes the hydrogen absorption capacity of the alloy higher than 3.5wt% and the hydrogen desorption platform pressure within the range of 0.1-1MPa, thereby making the high entropy alloy have an effective hydrogen desorption capacity higher than 2.4wt%.

[0015] As a preferred technical solution of the present invention, the temperature of the high entropy hydrogen storage alloy during the hydrogen absorption and desorption process is 20-30°C, for example, it can be 22°C, 24°C, 25°C, 27°C, 28°C or 29°C, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0016] Preferably, the maximum hydrogen absorption capacity of the high entropy hydrogen storage alloy is ≥3.5wt%, for example, it can be 3.55wt%, 3.6wt%, 3.65wt%, 3.7wt%, 3.75wt% or 3.8wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0017] Preferably, the effective hydrogen release amount of the high entropy hydrogen storage alloy is ≥2.4wt%, for example, it can be 2.42wt%, 2.44wt%, 2.46wt%, 2.48wt%, 2.5wt%, 2.52wt%, 2.64wt%, 2.68wt% or 2.7wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0018] In the present invention, the platform pressure of the high entropy hydrogen storage alloy during the process of absorbing and releasing hydrogen is ≥0.1 MPa, which can ensure the effective amount of hydrogen released in practical applications.

[0019] Preferably, after 100 cycles of use, the maximum hydrogen absorption capacity of the high entropy hydrogen storage alloy is ≥3.2wt%, for example, it can be 3.25wt%, 3.3wt%, 3.35wt%, 3.4wt%, 3.45wt%, 3.5wt% or 3.6wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0020] Preferably, the crystal structure of the high entropy hydrogen storage alloy includes a main phase of a body-centered cubic structure (BCC type) and a small amount of distributed Ce-rich phase.

[0021] In a second aspect, the present invention provides a method for preparing the high entropy hydrogen storage alloy according to the first aspect, the preparation method comprising the following steps:

[0022] (1) preparing ingredients according to the element ratio of the general composition formula of the high entropy hydrogen storage alloy, and then smelting to obtain a cast alloy;

[0023] (2) The cast alloy described in step (1) is packaged and annealed in sequence to obtain a high entropy hydrogen storage alloy.

[0024] The preparation method provided by the present invention adopts a specific raw material ratio and redesigns the preparation method, thereby improving the hydrogen storage performance of the high entropy hydrogen storage alloy, and also significantly improving the hydrogen absorption and desorption kinetics, activation performance, hydrogen absorption rate and cycle stability of the alloy; the preparation method is simple to operate, low in cost, and reduces the difficulty of activating the alloy hydrogen storage material.

[0025] As a preferred technical solution of the present invention, the smelting current in step (1) is 100-150A, for example, it can be 105A, 110A, 115A, 120A, 125A, 130A, 135A, 140A or 145A, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0026] In the present invention, the raw materials used in the batching in step (1) are all metal powders with a purity of ≥99.9%.

[0027] In the present invention, the smelting in step (1) is carried out under an inert gas, the smelting equipment includes an electric arc furnace, and the inert gas includes argon.

[0028] Preferably, the smelting time in step (1) is 10 to 20 seconds per time, for example, 12 seconds per time, 14 seconds per time, 16 seconds per time, 18 seconds per time or 20 seconds per time, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0029] Preferably, the smelting in step (1) is performed 3 to 5 times, for example, 3 times, 4 times or 5 times.

[0030] In the present invention, the smelting is repeated 3 to 5 times. After one smelting, the metal is cooled to room temperature along with the equipment, and then turned over for the next smelting. Multiple smelting can make multiple metal components mixed more evenly.

[0031] As a preferred technical solution of the present invention, the crystal structure of the cast alloy in step (1) includes a body-centered cubic structure.

[0032] Preferably, the lattice constant of the cast alloy in step (1) is 0.303-0.306 nm, for example, 0.3035 nm, 0.304 nm, 0.3045 nm, 0.305 nm or 0.3055 nm, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0033] As a preferred technical solution of the present invention, the packaging in step (2) is as follows: the cast alloy is wrapped with a tantalum sheet and placed in a quartz tube, and then the quartz tube is evacuated and an inert gas is introduced, and then the quartz tube is sealed;

[0034] Preferably, the vacuuming is performed 2 to 4 times, for example, 2 times, 3 times or 4 times.

[0035] Preferably, the pressure of the inert gas in the sealed tube is 0.4-0.6atm, for example, it can be 0.42atm, 0.44atm, 0.46atm, 0.48atm, 0.5atm, 0.52atm, 0.54atm, 0.56atm or 0.58atm, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0036] As a preferred technical solution of the present invention, the heating rate of the annealing treatment in step (2) is 5 to 10°C / min, for example, it can be 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0037] Preferably, the holding temperature of the annealing treatment is 1350-1450°C, for example, it can be 1360°C, 1370°C, 1380°C, 1390°C, 1400°C, 1410°C, 1420°C, 1430°C or 1440°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0038] Preferably, the holding time of the annealing treatment is 1 to 10 minutes, for example, it can be 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes or 9 minutes, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0039] As a preferred technical solution of the present invention, the annealing treatment in step (2) further includes water quenching, grinding and crushing in sequence.

[0040] Preferably, the particle size of the crushed alloy powder is 80-200 mesh, for example, it can be 90 mesh, 100 mesh, 110 mesh, 120 mesh, 130 mesh, 140 mesh, 150 mesh, 160 mesh, 170 mesh, 180 mesh or 190 mesh, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0041] Preferably, the crystal structure of the high entropy hydrogen storage alloy includes a main phase of a body-centered cubic structure and a small amount of distributed Ce-rich phase.

[0042] Preferably, the crystal constant of the high entropy hydrogen storage alloy is 0.302-0.305 nm, for example, it can be 0.3025 nm, 0.303 nm, 0.3035 nm, 0.304 nm or 0.3045 nm, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0043] The crystal constant of the high entropy hydrogen storage alloy of the present invention is slightly smaller than the crystal constant of the cast alloy obtained in step (1). Since the BCC alloy usually contains a small amount of Ti-rich region, the alloy lattice constant is relatively large. After annealing, the atoms are rearranged, which improves the uniformity of the alloy and avoids the generation of Ti-rich. Therefore, the lattice constant of the high entropy hydrogen storage alloy is reduced.

[0044] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0045] (1) preparing ingredients according to the element ratio of the general formula of high entropy hydrogen storage alloy, and then smelting to obtain a cast alloy with a lattice constant of 0.303 to 0.306 nm;

[0046] The smelting current is 100-150A, the time is 10-20s / time, and the number of times is 3-5 times;

[0047] (2) After encapsulating the cast alloy described in step (1), heating the alloy to 1350-1450° C. at a rate of 5-10° C. / min for annealing for 1-10 min, and then sequentially water quenching, grinding and crushing to obtain a high entropy hydrogen storage alloy with a crystal constant of 0.302-0.305 nm;

[0048] The packaging is as follows: the cast alloy is wrapped with a tantalum sheet and then placed in a quartz tube, the quartz tube is then evacuated, an inert gas is introduced, and then the quartz tube is sealed.

[0049] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] (1) The high entropy hydrogen storage alloy provided by the present invention has an elemental molar composition of Ti a Cr b V c Mn d Mo e Ce f ; Its hydrogen absorption and desorption performance is relatively excellent, with a maximum hydrogen absorption capacity of ≥3.5wt%, an effective hydrogen desorption capacity of ≥2.4wt%, and a room temperature hydrogen desorption platform pressure of ≥0.2MPa. After 100 cycles of use, the maximum hydrogen absorption capacity is still ≥3.2wt%;

[0052] (2) The present invention utilizes specific components and preparation processes to regulate the crystal form of high entropy hydrogen storage alloys, and then combines annealing and water quenching to improve the alloy's hydrogen absorption and desorption capacity, hydrogen desorption platform pressure, activation performance and cycle performance, and the high entropy hydrogen storage alloy can be activated at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 The hydrogen absorption process diagram of the high entropy hydrogen storage alloy in Examples 1-2 and Comparative Example 1 (25°C);

[0054] Figure 2 It is a hydrogen desorption PCT curve diagram (25°C) of the high entropy hydrogen storage alloys in Examples 1-2, Example 8 and Comparative Example 3. DETAILED DESCRIPTION

[0055] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0056] Example 1

[0057] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. The high entropy hydrogen storage alloy has a general composition formula of Ti 0.35 Cr 0.10 V 0.25 Mn 0.3 Mo 0.07 Ce 0.01 ;

[0058] The preparation method comprises the following steps:

[0059] (1) 10 g of metal powder was mixed according to the molar ratio of the target high entropy hydrogen storage alloy, and then pressed into a metal ingot with a diameter of 1 cm under a 10 t press, and then melted in an arc furnace under a vacuum of 0.5 atm. After the crucible was cooled to room temperature, it was turned over and the melting was repeated 4 times to obtain a cast alloy with a lattice constant of 0.306 nm;

[0060] The smelting current is 120A and the smelting time is 20s / time;

[0061] (2) Wrapping the cast alloy described in step (1) with a tantalum sheet and placing it in a quartz tube, evacuating the quartz tube three times, introducing an inert gas, sealing the quartz tube, and then heating to 1400° C. at a rate of 6° C. / min for annealing for 2 min, then water quenching, and finally mechanically grinding to remove the oxide scale, and mechanically crushing and sieving to 100 mesh to obtain a high entropy hydrogen storage alloy with a crystal constant of 0.304 nm;

[0062] The pressure of the inert gas in the sealed tube is 0.4 atm.

[0063] After 100 cycles of hydrogen absorption and desorption, the high entropy hydrogen storage alloy prepared in this embodiment has a maximum hydrogen absorption capacity of 3.3 wt%.

[0064] Example 2

[0065] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. In addition to the general composition formula of the high entropy hydrogen storage alloy being Ti 0.3 Cr 0.10 V 0.3 Mn 0.3 Mo 0.07 Ce 0.01 Except for this, other conditions are the same as those in Example 1.

[0066] Example 3

[0067] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. The general composition formula of the high entropy hydrogen storage alloy is Ti 0.35 Cr 0.10 V 0.25 Mn 0.3 Mo 0.07 Ce 0.01 ;

[0068] The preparation method comprises the following steps:

[0069] (1) 10 g of metal powder was mixed according to the molar ratio of the target high entropy hydrogen storage alloy, and then pressed into a metal ingot with a diameter of 1 cm under a 10 t press, and then melted in an arc furnace under a vacuum of 0.5 atm. After the crucible was cooled to room temperature, it was turned over and the melting was repeated 5 times to obtain a cast alloy with a lattice constant of 0.306 nm;

[0070] The smelting current is 150A and the smelting time is 10s / time;

[0071] (2) Wrapping the cast alloy described in step (1) with a tantalum sheet and placing it in a quartz tube, evacuating the quartz tube three times, introducing an inert gas, sealing the quartz tube, and then heating to 1450° C. at a rate of 10° C. / min for annealing for 1 min, then water quenching, and finally mechanically grinding to remove the oxide scale, and mechanically crushing and sieving to 100 mesh to obtain a high entropy hydrogen storage alloy with a crystal constant of 0.304 nm;

[0072] The pressure of the inert gas in the sealed tube is 0.4 atm.

[0073] Example 4

[0074] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. In addition to the general composition formula of the high entropy hydrogen storage alloy being Ti 0.40 Cr 0.10 V 0.25 Mn 0.2 Mo 0.07 Ce 0.01 Except for this, other conditions are the same as those in Example 1.

[0075] Example 5

[0076] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. In addition to the general composition formula of the high entropy hydrogen storage alloy being Ti 0.30 Cr 0.10 V 0.30 Mn 0.5 Mo 0.07 Ce 0.01 Except for this, other conditions are the same as those in Example 1.

[0077] Example 6

[0078] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the number of smelting times in step (1) is 2 times, other conditions are the same as those in Example 1.

[0079] Example 7

[0080] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the pressure of the inert gas in the sealed tube in step (2) is 1 atm, other conditions are the same as those in Example 1.

[0081] Example 8

[0082] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the holding temperature of the annealing treatment in step (2) is 1000° C., other conditions are the same as those in Example 1.

[0083] Example 9

[0084] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the holding temperature of the annealing treatment in step (2) is 1500° C., other conditions are the same as those in Example 1.

[0085] Example 10

[0086] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the heating rate of the annealing treatment in step (2) is 2°C / min, other conditions are the same as those in Example 1.

[0087] Embodiment 11

[0088] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the heating rate of the annealing treatment in step (2) is 15°C / min, other conditions are the same as those in Example 1.

[0089] Example 12

[0090] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the holding time of the annealing treatment in step (2) is 60 minutes, other conditions are the same as those in Example 1.

[0091] Embodiment 13

[0092] This embodiment provides a high entropy hydrogen storage alloy and a preparation method thereof. Except for the annealing treatment in step (2) followed by furnace cooling, other conditions are the same as those in embodiment 1.

[0093] Comparative Example 1

[0094] This comparative example provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the rare earth element Ce is not doped in the alloy and the content of the Cr element is increased by an equal amount, other conditions are the same as those in Example 1.

[0095] Comparative Example 2

[0096] This comparative example provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the molar ratio of the Mo element in the high entropy hydrogen storage alloy is 0.12 at%, and the content of the Cr element is reduced by an equal amount, other conditions are the same as those in Example 1.

[0097] Comparative Example 3

[0098] This comparative example provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the Mo element is not doped in the high entropy hydrogen storage alloy and the content of the Cr element is increased in an equal amount, other conditions are the same as those in Example 1.

[0099] Comparative Example 4

[0100] This comparative example provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the molar ratio of the Mn element in the high entropy hydrogen storage alloy is 0.47 at %, and the content of the Ti element is reduced by an equal amount, other conditions are the same as those in Example 1.

[0101] Comparative Example 5

[0102] This comparative example provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the high entropy hydrogen storage alloy is not doped with Mn element and the content of Ti element is increased in an equal amount, other conditions are the same as those in Example 1.

[0103] Comparative Example 6

[0104] This comparative example provides a high entropy hydrogen storage alloy and a preparation method thereof. Except that the molar ratio of the Cr element in the high entropy hydrogen storage alloy is 0.30at%, and the content of the Ti element is reduced by an equal amount, other conditions are the same as those in Example 1.

[0105] The high entropy hydrogen storage alloys prepared in the above examples and comparative examples were tested for hydrogen storage performance at 25° C. and 8 MPa hydrogen pressure.

[0106] Figure 1 This is a diagram of the hydrogen absorption process of the high entropy hydrogen storage alloy in Examples 1-2 of the present invention and Comparative Example 1 (25°C). It can be found that the alloy cannot absorb hydrogen directly without adding the Ce element and needs high-temperature activation to absorb hydrogen.

[0107] Figure 2 It is the hydrogen desorption PCT curve (25°C) of the high entropy hydrogen storage alloys in Examples 1-2, Example 8 and Comparative Example 3 of the present invention. It can be found that when the Mo element content is reduced, the hydrogen desorption platform of the high entropy hydrogen storage alloy is too low.

[0108] The test results of the above embodiments and comparative examples are shown in Table 1.

[0109] Table 1

[0110]

[0111]

[0112] From Table 1, we can draw the following conclusions:

[0113] (1) The high entropy hydrogen storage alloy and the preparation method thereof provided in Examples 1-3 of the present invention have excellent hydrogen absorption and desorption capacity at room temperature, with a maximum hydrogen absorption amount of ≥3.5wt%, an effective hydrogen desorption amount of ≥2.4wt%, a hydrogen desorption platform pressure of ≥0.2MPa at room temperature, and can directly absorb hydrogen at room temperature without high temperature activation energy;

[0114] (2) Combining Example 1 and Examples 4-5, it can be seen that when the ratio of (Ti+Cr+Mo) / (V+Mn+Ce) is not within the preferred range of 0.75 to 0.85, when (Ti+Cr+Mo) / (V+Mn+Ce) is greater than 0.85, the alloy has a low hydrogen desorption platform pressure (<0.1MPa), making it difficult for the alloy to dehydrogenate, and the amount of hydrogen desorption is less than 2wt%; when (Ti+Cr+Mo) / (V+Mn+Ce) is less than 0.75, the alloy has a high hydrogen desorption platform pressure, making the amount of hydrogen absorption only 3.1wt%, which leads to poor hydrogen storage performance of the high entropy alloy, and the amount of hydrogen desorption is only 1.8wt%;

[0115] (3) Combining Example 1 and Example 6, it can be seen that the melting point of metal Mo in the alloy component is relatively high, and multiple smelting is required to achieve the alloying process of the multi-element alloy. When the number of smelting times is small, it will lead to smelting non-uniformity and poor hydrogen storage performance; Combining Example 1 and Example 7, it can be seen that due to the high annealing temperature, the pressure in the quartz tube increases too high, the quartz tube breaks, and the sample is oxidized during the heat treatment process, and does not have hydrogen storage performance;

[0116] (4) Comprehensively from Example 1 and Examples 8-9, it can be seen that due to the low annealing temperature, the stress reduction of the alloy is small, so that the hydrogen absorption and desorption platform of the alloy is still relatively inclined, resulting in a small amount of hydrogen absorption and effective hydrogen desorption; due to the high annealing temperature, the quartz tube softens and breaks, and the sample is oxidized during the heat treatment process, and does not have hydrogen storage performance; Comprehensively from Example 1 and Examples 10-11, when the heating rate of the annealing treatment is too low, the low melting point metal Mn is easy to volatilize due to the long holding time, and the hydrogen desorption performance deteriorates; when the heating rate of the annealing treatment is too high, due to the short heat treatment time, the alloy components have no time to be evenly distributed, and the hydrogen desorption performance deteriorates; Comprehensively from Example 1 and Example 12, it can be seen that due to the long annealing time, new thermal stress will be caused, and recrystallization and grain growth will also occur, so that the hydrogen desorption platform of the alloy is not significantly improved, thereby affecting the effective hydrogen desorption;

[0117] (5) Based on Example 1 and Example 13, it can be seen that due to the cooling of the furnace at high temperature, the difference in melting point caused the alloy to undergo component segregation, and failed to maintain a uniform molten state at high temperature, resulting in poor hydrogen release performance;

[0118] (6) Based on Example 1 and Comparative Example 1, it can be seen that since Ce is a metal that is easily hydrogenated, it can significantly improve the activation performance of the alloy, thereby effectively solving the problem of difficult activation of BCC alloys;

[0119] (7) Based on Example 1 and Comparative Examples 2-3, it can be seen that since Mo atoms are B-side elements, the increase of B-side elements makes the hydrogen absorption and desorption platform of the alloy too high, thereby affecting the reduction of hydrogen absorption and effective hydrogen desorption; since Mo atoms are B-side elements, the reduction of B-side elements makes the hydrogen absorption and desorption platform of the alloy too low, thereby affecting the reduction of effective hydrogen desorption and platform pressure;

[0120] (8) Based on Example 1 and Comparative Examples 4-5, it can be seen that when the Mn atomic content in the high entropy hydrogen storage alloy is too high, the alloy dehydrogenation platform pressure is too high, resulting in a decrease in the amount of hydrogen absorbed by the high entropy alloy, and the amount of hydrogen released also decreases accordingly; when the high entropy hydrogen storage alloy is not doped with Mn elements, the alloy dehydrogenation is too low and the platform hysteresis is large, resulting in difficulty in dehydrogenation of the high entropy alloy;

[0121] (9) Based on Example 1 and Comparative Example 6, it can be seen that when the Cr atom content in the high entropy hydrogen storage alloy is too high, the hydrogen desorption platform pressure of the alloy is too high, resulting in a decrease in the hydrogen absorption amount of the high entropy alloy, and the hydrogen desorption amount also decreases accordingly, resulting in a deterioration of the hydrogen storage performance.

[0122] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A high entropy hydrogen storage alloy, characterized in that: The general composition formula of the high entropy hydrogen storage alloy is Ti a Cr b V c Mn d Mo e Ce f ; wherein, by molar ratio, 0.3≤a≤0.5, 0.05≤b≤0.2, 0.2≤c≤0.3, 0.25≤d≤0.4, 0.05≤e≤0.1, 0.01≤f≤0.

03.

2. The high entropy hydrogen storage alloy according to claim 1, characterized in that: The high entropy hydrogen storage alloy has the following molar ratios: 0.3≤a≤0.4, 0.07≤b≤0.12, 0.2≤c≤0.3, 0.27≤d≤0.32, 0.05≤e≤0.1, and 0.01≤f≤0.

03.

3. The high entropy hydrogen storage alloy according to claim 1, characterized in that: In the high entropy hydrogen storage alloy, the molar ratio is: 0.75≤(a+b+e) / (c+d+f)≤0.

85.

4. The high entropy hydrogen storage alloy according to claim 1, characterized in that: The temperature of the high entropy hydrogen storage alloy during the process of absorbing and releasing hydrogen is 20-30°C.

5. The high entropy hydrogen storage alloy according to claim 1, characterized in that: The maximum hydrogen absorption capacity of the high entropy hydrogen storage alloy is ≥3.5wt%.

6. The high entropy hydrogen storage alloy according to claim 1, characterized in that: The effective hydrogen release amount of the high entropy hydrogen storage alloy is ≥2.4wt%.

7. The high entropy hydrogen storage alloy according to claim 1, characterized in that: After the high entropy hydrogen storage alloy is used for 100 cycles, the maximum hydrogen absorption capacity is ≥3.2wt%.

8. The high entropy hydrogen storage alloy according to claim 1, characterized in that: The crystal structure of the high entropy hydrogen storage alloy includes a main phase of a body-centered cubic structure and a small amount of distributed Ce-rich phase.

9. A method for preparing the high entropy hydrogen storage alloy according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: (1) preparing ingredients according to the element ratio of the general composition formula of the high entropy hydrogen storage alloy, and then smelting to obtain a cast alloy; (2) The cast alloy described in step (1) is packaged and annealed in sequence to obtain a high entropy hydrogen storage alloy.

10. The preparation method according to claim 9, characterized in that: The smelting current in step (1) is 100-150A.

11. The preparation method according to claim 9, characterized in that: The smelting time in step (1) is 10 to 20 seconds per time.

12. The preparation method according to claim 9, characterized in that: The smelting is performed 3 to 5 times in step (1).

13. The preparation method according to claim 9, characterized in that: The crystal structure of the cast alloy in step (1) includes a body-centered cubic structure.

14. The preparation method according to claim 9, characterized in that: The lattice constant of the cast alloy in step (1) is 0.303-0.306 nm.

15. The preparation method according to claim 9, characterized in that: The packaging in step (2) is as follows: the cast alloy is wrapped with a tantalum sheet and then placed in a quartz tube, the quartz tube is then evacuated, an inert gas is introduced, and the quartz tube is sealed.

16. The preparation method according to claim 15, characterized in that: The vacuuming is performed 2 to 4 times.

17. The preparation method according to claim 15, characterized in that: The pressure of the inert gas in the sealed tube is 0.4-0.6 atm.

18. The preparation method according to claim 9, characterized in that: The heating rate of the annealing treatment in step (2) is 5 to 10°C / min.

19. The preparation method according to claim 9, characterized in that: The holding temperature of the annealing treatment is 1350-1450°C.

20. The preparation method according to claim 9, characterized in that: The holding time of the annealing treatment is 1 to 10 minutes.

21. The preparation method according to claim 9, characterized in that: The annealing treatment in step (2) further includes water quenching, grinding and crushing in sequence.

22. The preparation method according to claim 21, characterized in that: The particle size of the crushed alloy powder is 80-200 meshes.

23. The preparation method according to claim 9, characterized in that: The crystal structure of the high entropy hydrogen storage alloy includes a main phase of a body-centered cubic structure and a small amount of distributed Ce-rich phase.

24. The preparation method according to claim 9, characterized in that: The lattice constant of the high entropy hydrogen storage alloy is 0.302-0.305 nm.

25. The preparation method according to claim 9, characterized in that: The preparation method comprises the following steps: (1) preparing ingredients according to the element ratio of the general formula of high entropy hydrogen storage alloy, and then smelting to obtain a cast alloy with a lattice constant of 0.303 to 0.306 nm; The smelting current is 100-150A, the time is 10-20s / time, and the number of times is 3-5 times; (2) After encapsulating the cast alloy described in step (1), heating the alloy to 1350-1450° C. at a rate of 5-10° C. / min for annealing for 1-10 min, and then sequentially water quenching, grinding and crushing to obtain a high entropy hydrogen storage alloy with a crystal constant of 0.302-0.305 nm; The packaging is as follows: the cast alloy is wrapped with a tantalum sheet and then placed in a quartz tube, the quartz tube is then evacuated, an inert gas is introduced, and then the quartz tube is sealed.