A supported copper-iron bimetallic ammonia synthesis catalyst and its preparation method and application

Through the supported copper-iron bimetallic catalyst, TiO2 carrier and Cu/Fe active components are used to solve the problems of high energy consumption and poor NOx conversion of the existing ammonia synthesis technology, and achieve low-energy consumption and high-efficiency ammonia synthesis, especially at 400 High efficiency in converting NO to NH3 at ℃.

CN116408079BActive Publication Date: 2024-10-22SHIHEZI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211473330.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-21
Publication Date
2024-10-22
Estimated Expiration
2042-11-21

AI Technical Summary

Technical Problem

Existing ammonia synthesis technology consumes high energy and cannot effectively convert NOx into NH3, resulting in high energy consumption and serious environmental pollution. In particular, the use of catalysts under high temperature and high pressure conditions leads to excessive energy consumption.

Method used

A supported copper-iron bimetallic catalyst is used, with Cu and Fe as active components, and the carrier is TiO2. Through the preparation process of double titration method, the use temperature of the catalyst is reduced and the ammonia selectivity and conversion rate are improved.

Benefits of technology

Efficient ammonia synthesis is achieved at lower temperatures, energy consumption is reduced, the efficiency of converting NO into NH3 is increased to 85%, and catalyst preparation costs are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116408079B_ABST
    Figure CN116408079B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of catalysts and discloses a supported copper-iron bimetallic ammonia synthesis catalyst and its preparation method and application. The catalyst uses Cu and Fe as active components and TiO 2 as a carrier; the molar ratio of Cu to Fe is 1:1-3, and the mass ratio of active component to carrier is 1:4-6. The preparation method is: 2 The carrier powder was dissolved in a mixed solution of copper salt and iron salt to obtain solution A; 3 mol / L NaOH solution and 1 mol / L Na 2 CO 3 The solution is titrated to pH 10-12 by double titration, stirred for 10-12 hours, aged by standing, filtered until the pH value is neutral, dried, ground once, calcined, and ground twice to obtain the catalyst. 2 On the carrier, the catalytic effect of the active components is exerted, and at the same time, the surface oxygen vacancies of the catalyst are increased through the carrier. The preparation process is simple and highly operable, and it has a higher conversion rate and ammonia selectivity at a lower operating temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and more particularly to a supported copper-iron bimetallic ammonia synthesis catalyst and a preparation method and application thereof. Background Art

[0002] Ammonia is an important basic chemical raw material in the field of fertilizer production and fiber manufacturing, and its output ranks first among all chemical products. At present, the Haber-Bosch process is widely used in the industry to synthesize ammonia, that is, nitrogen N2 and hydrogen H2 are combined under high temperature (500℃) and high pressure (20-50MPa) catalyst (iron) to produce ammonia NH3. Since nitrogen molecule is a very stable single substance, its triple bond energy is 94l KJ·mol -1 It is highly inert and difficult to activate, so it is costly and consumes a lot of energy. Its annual energy consumption is as high as 1-2% of the world's total energy consumption. Therefore, it is necessary to develop a new method for synthesizing ammonia with low energy consumption to save energy and reduce costs.

[0003] With the advancement of industrialization, environmental pollution has become an inevitable development problem that needs to be faced. Nitrogen oxides contained in industrial waste gas and automobile exhaust are one of the main sources of air pollution. The emission of nitrogen oxides into the air will lead to acid rain, photochemical smog pollution, ozone layer destruction and other adverse consequences. The most widely used nitrogen oxide control technology is the reduction denitrification technology, which uses NH3 or CO as a reducing agent. Although this method can convert nitrogen oxides into nitrogen gas, it consumes ammonia instead of generating ammonia. It can be seen that for the catalytic reduction reaction of NO, previous research has mainly focused on how to reduce NO to N2, and has not studied its direct reduction to NH3. Therefore, the development of a catalyst that can reduce NO x Catalysts for conversion to NH3 are a new direction in the field of catalysis.

[0004] Chinese patent CN114210372A discloses an Fe-based denitration ammonia synthesis catalyst and its preparation method and application, which uses MIL-125 (Ti) as a carrier and transition metal Fe as an active component, and has high denitration efficiency and high NH3 selectivity. However, in order to achieve excellent conversion rate and selectivity, the reaction temperature of this catalyst needs to reach about 500°C, resulting in excessive energy consumption.

[0005] Therefore, how to provide a synthetic ammonia catalyst with a low operating temperature is an important problem that needs to be solved urgently in this field. Summary of the invention

[0006] In view of this, the present invention provides a supported copper-iron bimetallic ammonia synthesis catalyst and a preparation method thereof. By loading a copper-iron metal salt having an active component onto a TiO2 carrier, the catalytic effect of the active component is exerted, and at the same time, the surface oxygen vacancies of the catalyst are increased through the carrier. The preparation process is simple and highly operable, thereby having a higher conversion rate and a higher ammonia selectivity at a lower operating temperature.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A supported copper-iron bimetallic ammonia synthesis catalyst has Cu and Fe as active components and TiO2 as a carrier; the molar ratio of Cu to Fe is 1:1-3, and the mass ratio of the active component to the carrier is 1:4.

[0009] The present invention also provides a method for preparing the above-mentioned supported copper-iron bimetallic ammonia synthesis catalyst, comprising the following steps:

[0010] (1) dissolving TiO2 carrier powder in a mixed solution of copper salt and iron salt to obtain solution A;

[0011] (2) Prepare 3 mol / L NaOH solution and 1 mol / L Na2CO3 solution respectively, and titrate the obtained solution A to a pH value of 10 by double titration method. After titration, stir the obtained solution for 10-12 hours, and then stand for aging. Finally, filter with water until the pH value is neutral, dry, grind once, calcine, and grind twice to obtain the catalyst.

[0012] Preferably, the copper salt in step (1) is copper nitrate hexahydrate, and the iron salt is iron nitrate nonahydrate.

[0013] Preferably, the NaOH solution and the Na2CO3 solution in step (1) are used in the same volume during double titration.

[0014] Preferably, the stirring rate in step (2) is 400-600 r / min.

[0015] Preferably, the static aging time in step (2) is 12-24 hours.

[0016] Preferably, the drying temperature in step (2) is 80-100°C.

[0017] Preferably, the calcination temperature in step (2) is 400-550° C. and the calcination time is 2-4 hours.

[0018] Preferably, the particle size after the first grinding and the second grinding in step (2) is 150-200 um.

[0019] Another object of the present invention is to provide the use of the above-mentioned supported copper-iron bimetallic ammonia synthesis catalyst in the synthesis of ammonia by the reaction of NO and H2.

[0020] It can be seen from the above technical solution that, compared with the prior art, the present invention uses double transition metal copper and iron as active components, which reduces the preparation cost of the catalyst. The combination of copper and iron has a synergistic effect, and the efficiency of synthetic ammonia is improved by adjusting the ratio of the double metals. At the same time, the use of TiO2 as a carrier can also produce a synergistic effect with the active component, and the effect is better than using other existing carriers.

[0021] The catalyst prepared by the present invention can be used for preparing ammonia synthesis reaction under normal pressure with NO and H2 as reactants, and can realize the conversion of 85% NO into NH3 at 400°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0023] Figure 1 The NO conversion rate of the catalysts prepared in Examples 1-3 and Comparative Example 1;

[0024] Figure 2 NH3 selectivity of the catalysts prepared in Examples 1-3 and Comparative Example 1.

[0025] Figure 3 is the NO conversion rate of the catalyst prepared in Comparative Example 2-3;

[0026] Figure 4 NH3 selectivity of the catalyst prepared in Comparative Example 2-3. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] Preparation of CuFe(1:1) / TiO2 catalyst, the specific steps are as follows:

[0030] (1) At room temperature and pressure, add copper nitrate trihydrate (0.251 g), iron nitrate nonahydrate (0.424 g) and TiO2 powder (1 g Macklin P25) into a beaker, add 100 ml of deionized water to dissolve, and stir continuously in a magnetic stirrer at a speed of 500 r / min to make the solution evenly mixed, and continue stirring for 1 hour;

[0031] (2) Weigh sodium hydroxide (12 g) and sodium carbonate (10.6 g) to prepare 3 mol / L NaOH solution (100 ml) and 1 mol / L Na2CO3 solution (100 ml);

[0032] (3) Then double titration is performed to titrate the solution obtained in step (1) to a pH value of 10, followed by continued stirring and aging for 12 h;

[0033] (4) Filter the obtained precipitate with water until it becomes neutral;

[0034] (5) The precipitate obtained in step (4) is dried in a forced air drying oven at 80° C. to obtain a catalyst precursor, which is ground to an average particle size of 178 μm after grinding, and then calcined in a muffle furnace at 500° C. for 3 hours, taken out and ground to an average particle size of 150 μm after grinding to obtain the supported copper-iron bimetallic ammonia synthesis catalyst.

[0035] Example 2

[0036] Preparation of CuFe(1:2) / TiO2 catalyst, the specific steps are as follows:

[0037] (1) At room temperature and pressure, add copper nitrate trihydrate (0.151 g), iron nitrate nonahydrate (0.505 g) and TiO2 powder (1 g) into a beaker, add 100 ml of deionized water to dissolve, and continue stirring in a magnetic stirrer at a magnetic speed of 400 r / min to make the solution evenly mixed, and continue stirring for 1 hour;

[0038] (2) Weigh sodium hydroxide (12 g) and sodium carbonate (10.6 g) to prepare 3 mol / L NaOH solution (100 ml) and 1 mol / L Na2CO3 solution (100 ml);

[0039] (3) Then double titration was performed to titrate the solution obtained in step (1) to a pH value of 12, followed by continued stirring and aging for 18 h;

[0040] (4) Filter the obtained precipitate with water until it becomes neutral;

[0041] (5) The precipitate obtained in step (4) is dried in a 100° C. forced air drying oven to obtain a catalyst precursor, which is ground to an average particle size of 170 μm after grinding, and then calcined in a muffle furnace at 550° C. for 2 hours, taken out and ground to an average particle size of 160 μm after grinding, thereby obtaining the supported copper-iron bimetallic ammonia synthesis catalyst.

[0042] Example 3

[0043] Preparation of CuFe(1:3) / TiO2 catalyst, the specific steps are as follows:

[0044] (1) At room temperature and pressure, add copper nitrate trihydrate (0.151 g), iron nitrate nonahydrate (0.505 g) and TiO2 powder (1 g) into a beaker, add 100 ml of deionized water to dissolve, and continue stirring in a magnetic stirrer at a speed of 600 r / min to make the solution evenly mixed. Continue stirring for 1 hour;

[0045] (2) Weigh sodium hydroxide (12 g) and sodium carbonate (10.6 g) to prepare 3 mol / L NaOH solution (100 ml) and 1 mol / L Na2CO3 solution (100 ml);

[0046] (3) Then double titration is performed to titrate the solution obtained in step (1) to a pH value of 11, followed by continued stirring and aging for 24 hours;

[0047] (4) Filter the obtained precipitate with water until it becomes neutral;

[0048] (5) The precipitate obtained in step (4) is dried in a 90° C. forced air drying oven to obtain a catalyst precursor, which is ground to an average particle size of 180 μm after grinding, and then calcined in a muffle furnace at 400° C. for 4 hours, taken out and ground to an average particle size of 150 μm after grinding, thereby obtaining the supported copper-iron bimetallic ammonia synthesis catalyst.

[0049] Comparative Example 1

[0050] Preparation of CuFe(2:1) / TiO2 catalyst

[0051] The difference between this comparative example and Example 1 is that the amount of copper nitrate trihydrate is 0.376 g and the amount of ferric nitrate nonahydrate is 0.315 g.

[0052] Comparative Example 2

[0053] Preparation of CuCe(1:3) / TiO2 catalyst

[0054] The difference between this comparative example and Example 1 is that the amount of copper nitrate trihydrate is 0.101 g and the amount of cerium nitrate hexahydrate is 0.546 g.

[0055] Comparative Example 3

[0056] Preparation of FeCe(1:3) / TiO2 catalyst

[0057] The difference between this comparative example and Example 1 is that the amount of ferric nitrate trihydrate is 0.149 g and the amount of cerium nitrate hexahydrate is 0.481 g.

[0058] Application Examples

[0059] Evaluation of ammonia synthesis performance of catalysts of Examples 1-3 and Comparative Examples 1-3

[0060] The catalysts prepared in Examples 1-3 and Comparative Examples 1-3 were used for NO synthesis ammonia reaction. The performance test of synthetic ammonia was carried out in a fixed bed reactor at atmospheric pressure. The reactor was a stainless steel tube with an inner diameter of 10.0 mm. Before the experiment, quartz sand and quartz wool were placed in the reaction tube to ensure the contact between the powder catalyst and the thermocouple. The simulated flue gas consisted of 350 ppm NO, 2000 ppm H2, and N2 as the balance gas. The air velocity was 20000 mL·g -1 ·h -1 The temperature of the reaction device was raised from room temperature to 500°C by program heating, and each temperature point was 50°C. Each temperature point was kept warm for 40 minutes before testing. The detection device was Fourier infrared, and the synthetic ammonia performance at different temperatures was detected at each temperature point. The results of Examples 1-3 and Comparative Example 1 are as follows: Figure 1 , Figure 2 As shown; Comparative Examples 2-3 results are as follows Figure 3 , Figure 4 shown.

[0061] NO conversion and NH3 selectivity were calculated by the following formula:

[0062] NO conversion (%) = ([NO]in-[NO]out) / [NO]in×100%

[0063] NH3 selectivity (%)=[NH3]out / ([NO]in-[NO]out)×100%

[0064] from Figure 1-2 It can be seen that the catalysts with a copper-iron bimetallic ratio of 1:1-1:3 show higher NH3 selectivity. However, the selectivity of ammonia for the copper-iron 2:1 catalyst at 400°C reaches up to 65%, which is much lower than the catalysts with other ratios.

[0065] from Figure 3-4 It can be seen that after replacing the active components, the conversion rate of NO and the selectivity of NH3 decreased significantly. Figure 1-2 This shows that there is a better synergistic effect between copper and iron bimetallics.

[0066] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0067] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. Application of a supported copper-iron bimetallic ammonia synthesis catalyst in the reaction of NO and H2 to synthesize ammonia, characterized in that: The catalyst uses Cu and Fe as active components and TiO2 as a carrier; the molar ratio of Cu to Fe is 1:1-3, and the mass ratio of the active component to the carrier is 1:4-6.

2. The use according to claim 1, characterized in that: The preparation method of the supported copper-iron bimetallic ammonia synthesis catalyst comprises the following steps: (1) dissolving nano-sized TiO2 carrier powder in a mixed solution of copper salt and iron salt to obtain solution A; (2) Prepare 3 mol / L NaOH solution and 1 mol / L Na2CO3 solution respectively, and titrate the obtained solution A to a pH value of 10-12 by double titration method, stir the obtained solution for 10-12 hours after titration, and then stand for aging, and finally filter with water to a neutral pH value, dry, grind once, calcine, and grind twice to obtain the catalyst.

3. The use according to claim 2, characterized in that: The copper salt in step (1) is copper nitrate hexahydrate, and the iron salt is iron nitrate nonahydrate.

4. The use according to claim 2, characterized in that: The NaOH solution and the Na2CO3 solution in step (1) are used in the same volume during double titration.

5. The use according to claim 2, characterized in that: The stirring rate in step (2) is 400-600 r / min.

6. The use according to claim 2, characterized in that: The static aging time in step (2) is 12-24 hours.

7. The use according to claim 2, characterized in that: The drying temperature in step (2) is 80-100°C.

8. The use according to claim 2, characterized in that: The calcination temperature in step (2) is 400-550° C. and the calcination time is 2-4 hours.

9. The use according to claim 2, characterized in that: The particle sizes after the first grinding and the second grinding in step (2) are both 150-200 μm.