A metal oxide doped hard carbon composite material and preparation method thereof
By doping hard carbon materials with metal oxides and coating them with porous silver, the first problem of low efficiency and power performance of hard carbon materials is solved, significantly improving its application performance in the field of pure electric vehicles.
Patent Information
- Application Number
- CN202310415659.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-18
AI Technical Summary
The application of hard carbon materials in the field of pure electric vehicles is limited by their low initial efficiency, low specific capacity and low compaction density, and the power performance of existing sulfur-doped biomass hard carbon materials deviates significantly.
By doping metal oxide in the hard carbon precursor, and coating the outer shell with porous silver, the metal oxide doped hard carbon composite material is prepared using hydrothermal reaction and evaporation methods to improve the power performance and first-time efficiency of the material. .
The power performance and first-time efficiency of hard carbon materials are improved, the specific surface area and energy density of the material are significantly enhanced, and the cycle performance and rate performance are improved.
Smart Images

Figure CN116443847B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to a metal oxide-doped hard carbon composite material and a preparation method thereof. Background Art
[0002] Hard carbon materials are used in fields such as hybrid batteries due to their advantages such as low expansion, excellent low-temperature performance, and good high-rate cycle performance. However, their own disadvantages such as low first efficiency, low specific capacity, and low compaction density limit their application in fields such as pure electric vehicles. There are many measures to improve the specific capacity and first efficiency of hard carbon, such as doping and pore making to reduce the impedance of the material and improve the first efficiency. The patent application for a sulfur-doped biomass hard carbon material and its preparation method and application (application number 202111105546.X) has the following preparation process: pretreating and crushing the biomass raw material to obtain a precursor powder, which is then mixed with an inorganic salt and a sulfur source and ball-milled, carbonized and sintered, and pickled to obtain a hard carbon composite material. However, it has problems such as power performance deviation and low first efficiency. Summary of the invention
[0003] The present invention proposes a metal oxide doped hard carbon composite material and a preparation method thereof, which improves the power performance and first efficiency by doping metal in the core of a hard carbon precursor and coating its outer shell with porous silver, thereby solving the problems of room temperature power performance deviation and low first efficiency of hard carbon materials in related technologies.
[0004] The technical solution of the present invention is as follows:
[0005] A method for preparing a metal oxide-doped hard carbon composite material comprises the following steps:
[0006] S1, mixing hydrocarbon, pore former and metal salt in a solvent uniformly and performing hydrothermal reaction to obtain a metal-doped hard carbon precursor material;
[0007] S2, using the metal-doped hard carbon precursor material as a matrix, depositing silver fluoride on the surface of the matrix by evaporation to obtain a silver-coated metal-doped hard carbon composite material;
[0008] S3, adding the silver-coated metal-doped hard carbon composite material into acidic steam for surface etching, washing and drying to obtain the metal oxide-doped hard carbon composite material.
[0009] As a further technical solution, in step S1, the reaction temperature of the hydrothermal reaction is 100-200° C., and the reaction time is 1-6 hours.
[0010] As a further technical solution, the step S2 is specifically as follows: the evaporation furnace cavity A is the metal-doped hard carbon precursor material, the evaporation furnace cavity B is the silver fluoride powder, and the cavity B is evacuated to 1 to 5*10 -5 Torr, and heated at 200-400A, 300°C-500°C for 10-60min, then opening the valve between cavity A and cavity B to allow silver fluoride to be deposited on the surface of the substrate, and then cooling in an inert atmosphere to obtain a silver-coated metal-doped hard carbon composite material.
[0011] As a further technical solution, in step S2, the cavity A is evacuated to 0.1-0.5 Torr.
[0012] As a further technical solution, the step S3 is specifically as follows: transferring the silver-coated metal-doped hard carbon composite material to a reactor, evacuating to -0.09 to -0.9 MPa, and heating concentrated nitric acid or concentrated sulfuric acid in the reactor to vaporize for etching, cooling to room temperature, washing, and vacuum drying to obtain the metal oxide-doped hard carbon composite material.
[0013] As a further technical solution, etching is performed for 30-300 minutes.
[0014] As a further technical solution, at least one of the following technical features is also included:
[0015] The hydrocarbons include one or more of glucose, sucrose, lignin, and cellulose;
[0016] The solvent includes one or more of benzyl alcohol, ferrocenyl methanol, cyclohexanol, 1,4-butanediol, and cinnamyl alcohol;
[0017] The pore-forming agent includes one or more of nickel acetate, copper acetate, manganese acetate, bismuth acetate, and cobalt acetate.
[0018] As a further technical solution, the metal salt includes one or more of silver diethyldithiocarbamate, silver iodide of trimethylphosphine, silver trifluoromethanesulfonate, and silver diethylaminodithiocarbamate.
[0019] As a further technical solution, the mass ratio of the hydrocarbon, the pore-forming agent, the metal salt and the solvent is 100:1-10:1-10:500-1000.
[0020] The present invention also provides a metal oxide doped hard carbon composite material, which is obtained according to the preparation method. The composite material presents a core-shell structure, wherein the core is metal oxide doped hard carbon and the shell is porous silver.
[0021] The working principle and beneficial effects of the present invention are:
[0022] 1. Metal salt compounds are doped into the hard carbon precursor by the hydrothermal method, which has the advantages of uniform doping, molecular-level mixing, and reduced impedance; at the same time, the energy density is improved by relying on the high specific capacity of the metal oxide itself.
[0023] 2. Silver fluoride deposited on the hard carbon surface by evaporation has the characteristics of high density, adjustable deposition thickness, and high deposition integrity. At the same time, after surface etching with concentrated acid, the porous silver obtained has a high specific surface area to improve the material's ability to absorb and retain liquid, and relies on the dual effects of the high electronic conductivity of the outer shell silver fluoride and the electronic conductivity of the inner core metal oxide to improve the power performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0025] Figure 1 This is a SEM image of the hard carbon composite material obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] Preparation method of porous silver oxide-coated metal-doped hard carbon composite material:
[0029] S1. Add 100 g of glucose, 5 g of nickel acetate and 5 g of silver diethyldithiocarbamate to 800 g of benzyl alcohol and mix well. Then transfer to a high-pressure reactor and perform hydrothermal reaction at 150° C. for 3 h. Filter and vacuum dry at 80° C. for 24 h to obtain a metal-doped hard carbon precursor material.
[0030] S2, the metal-doped hard carbon precursor material is transferred into the evaporation furnace chamber A as a substrate, and the vacuum is pumped to 0.3 Torr; the silver fluoride powder is placed in the evaporation furnace chamber B, and the vacuum is pumped to 3*10 -5 Torr, heated at 400A, 400°C for 30 min, then opened the valve between chamber A and chamber B to deposit silver on the substrate surface, and then cooled in an argon atmosphere to obtain a silver-coated metal-doped hard carbon composite material;
[0031] S3. Transfer the silver-coated metal-doped hard carbon composite material to a glass reactor, evacuate to -0.2MPa, and heat the concentrated nitric acid in the reactor to 200°C to vaporize it and etch the composite material for 60 minutes. Then cool it to room temperature, wash it with deionized water, and vacuum dry it at 80°C for 24 hours to obtain a porous silver oxide-coated metal-doped hard carbon composite material.
[0032] Example 2
[0033] S1. Add 100 g of lignin, 1 g of copper acetate, and 1 g of silver iodide of trimethylphosphine to 500 g of ferrocene methanol and mix them evenly. Then transfer them to a high-pressure reactor and perform a hydrothermal reaction at a temperature of 100 ° C for 6 h. Filter and vacuum dry at 80 ° C for 24 h to obtain a metal-doped hard carbon precursor material.
[0034] S2, the metal-doped hard carbon precursor material is transferred into the evaporation furnace chamber A as a substrate, and the vacuum is pumped to 0.1 Torr; the silver fluoride powder is placed in the evaporation furnace chamber B, and the vacuum is pumped to 1*10 -5 Torr, heated at 200A, 300°C for 60 min, then opened the valve between chamber A and chamber B to deposit silver on the substrate surface, and then cooled in an argon atmosphere to obtain a silver-coated metal-doped hard carbon composite material;
[0035] S3. Transfer the silver-coated metal-doped hard carbon composite material to a glass reactor, evacuate to -0.09MPa, and heat the concentrated sulfuric acid in the reactor to 100°C to vaporize it and etch the composite material for 300 minutes. Then cool it to room temperature, wash it with deionized water, and vacuum dry it at 80°C for 24 hours to obtain a porous silver oxide-coated metal-doped hard carbon composite material.
[0036] Example 3
[0037] S1. Add 100 g of cellulose, 10 g of bismuth acetate and 10 g of silver trifluoromethanesulfonate to 1000 g of cyclohexanol and mix well, then transfer to a high-pressure reactor, and perform a hydrothermal reaction at a temperature of 200° C. for 1 h, filter, and vacuum dry at 80° C. for 24 h to obtain a metal-doped hard carbon precursor material;
[0038] S2, the metal-doped hard carbon precursor material is transferred into the evaporation furnace chamber A as a substrate, and the vacuum is pumped to 0.5 Torr; the silver fluoride powder is placed in the evaporation furnace chamber B, and the vacuum is pumped to 5*10 -5 Torr, heated at 400A, 500°C for 10 min, then opened the valve between chamber A and chamber B to deposit silver on the substrate surface, and then cooled in an argon atmosphere to obtain a silver-coated metal-doped hard carbon composite material;
[0039] S3. Transfer the silver-coated metal-doped hard carbon composite material to a glass reactor, evacuate to -0.9 MPa, and heat the concentrated nitric acid in the reactor to 300°C to vaporize it and etch the composite material for 30 minutes. Then cool it to room temperature, wash it with deionized water, and vacuum dry it at 80°C for 24 hours to obtain a porous silver oxide-coated metal-doped hard carbon composite material.
[0040] Comparative Example 1
[0041] Compared with Example 1, step S1 is different: 100 g of glucose is added to 800 g of benzyl alcohol and mixed evenly, then transferred to a high-pressure reactor, and subjected to hydrothermal reaction at a temperature of 150° C. for 3 h, filtered, and vacuum dried at 80° C. for 24 h to obtain a hard carbon precursor material;
[0042] The rest is the same as step S2 and step S3 in Example 1, to obtain a porous silver oxide-coated metal-doped hard carbon composite material.
[0043] Comparative Example 2
[0044] Compared with Example 1, in step S2, a metal silver sheet is placed in the cavity B of the evaporation furnace, and the rest is the same as Example 1.
[0045] Experiment 1
[0046] Figure 1 is a SEM image of the hard carbon composite material obtained in Example 1, Figure 1 It can be seen that the hard carbon composite material obtained in Example 1 has a granular structure with uniform size distribution and a particle size between 5 and 8 μm.
[0047] Experiment 2
[0048] According to the national standard GB / T-24533-2019 "Graphite Negative Electrode Materials for Lithium-ion Batteries", the specific surface area, tap density, particle size, powder conductivity, first discharge specific capacity and first charge and discharge efficiency of the hard carbon composite materials of the embodiments and comparative examples were tested; the test results are shown in Table 1.
[0049] Table 1 Physical and chemical properties of hard carbon composites
[0050]
[0051] It can be seen from Table 1 that the hard carbon composite materials obtained in Examples 1-3 are significantly better than those in the comparative example in terms of specific surface area and tap density. The reason is that the hydrothermal method is used to dope metal salt compounds in the hard carbon precursor to reduce impedance and improve the initial efficiency; at the same time, the energy density is improved by relying on the high specific capacity of the metal oxide itself.
[0052] Experiment 3
[0053] The hard carbon composite materials obtained in Examples 1-3 and Comparative Examples 1-2 are respectively used as negative electrodes (the mass ratio of the substances in the formula is hard carbon composite material: CMC: SBR: SP: H2O = 95:2.5:1.5:1:150), and lithium sheets are used as positive electrodes. The electrolyte adopts LiPF6 / EC+DEC (the volume ratio of the electrolyte solvent EC:DEC = 1:1). The diaphragm adopts a composite film of polyethylene PE, polypropylene PP and polyethylene propylene PEP. The button cells are assembled in an argon-filled glove box to form button cells A1, A2, A3 and B1, B2. The electrochemical properties were tested on a Wuhan Blue Electric CT2001A battery tester. The charge and discharge voltage range was controlled at 0.0-2V, and the charge and discharge rate was 0.1C / 0.1C. At the same time, the 2C and 0.1C lithium removal capacities of the button cells, the DCR of the button cells, and the cycle performance of the button cells (0.2C / 0.2C, 100 weeks) were tested. The test results are shown in Table 2.
[0054] Table 2 Cycle performance of button cell
[0055]
[0056] It can be seen from Table 2 that the cycle performance and rate performance of the button cells made of the hard carbon composite materials of Examples 1-3 are significantly higher than those of the control examples. The reason is that the materials of the present invention have high powder conductivity, which reduces DCR and improves rate performance. At the same time, the larger specific surface area of the example materials improves the liquid retention performance of the materials and improves the cycle performance.
[0057] Experiment 4
[0058] The hard carbon composite materials prepared in Examples 1-3 and Comparative Examples 1-2 were mixed and coated to prepare negative electrode sheets, the ternary material NCM811 was used as the positive electrode, the solvent was EC / DEC / PC (volume ratio, EC:DEC:PC=1:1:1) as the electrolyte, the solute was LiPF6 (concentration of 1.3 mol / L), and the Celgard 2400 membrane was used as the separator. 2Ah soft-pack batteries C1, C2, C3 and D1, D2 were prepared respectively, and the results are shown in Tables 3 and 4 respectively.
[0059] (1) Liquid absorption capacity:
[0060] Use a 1mL burette and absorb VmL of electrolyte, add a drop on the surface of the electrode, and count until the electrolyte is completely absorbed, record the time t, and calculate the electrode's liquid absorption rate V / t. The test results are shown in Table 3.
[0061] (2) Liquid retention rate test:
[0062] According to the electrode parameters, the theoretical liquid absorption m1 of the electrode is calculated, and the weight m2 of the electrode is weighed. Then, the electrode is placed in the electrolyte and soaked for 24 hours. The weight of the electrode is weighed as m3, and the liquid absorption m3-m2 of the electrode is calculated. It is calculated according to the following formula: Liquid retention rate = (m3-m2)*100% / m1. The test results are shown in Table 3.
[0063] Table 3 Liquid absorption speed and liquid retention rate of soft pack batteries
[0064] Serial number Liquid absorption speed (S) Fluid retention rate Example 1 60 91.1% Example 2 65 90.3% Example 3 56 92.2% Comparative Example 1 120 85.6% Comparative Example 2 89 87.3%
[0065] It can be seen from Table 3 that the liquid absorption and retention capabilities of the negative electrodes prepared using the hard carbon composite materials obtained in Examples 1-3 are significantly better than those of the comparative examples. The reason for this is that the hard carbon materials in the examples have a high specific surface area, which improves the liquid absorption and retention performance of the electrode.
[0066] (3) Rate performance test:
[0067] The rate performance of the soft-pack battery was tested with a charge and discharge voltage range of 2.75 to 4.2 V and a temperature of 25 ± 3.0 °C. The batteries were charged at 1.0 C, 3.0 C, 5.0 C, and 10.0 C and discharged at 1.0 C. The test results are shown in Table 4.
[0068] Table 4 Rate performance of soft pack batteries
[0069]
[0070] It can be seen from Table 4 that the rate charging performance of the soft-pack batteries in Examples 1 to 3 is significantly better than that of the comparative example, that is, the charging time is shorter. The reason for this is that the power performance of the material is improved by relying on the dual effects of the silver fluoride with high electronic conductivity of the outer shell and the electronic conductivity of the metal oxide in the inner core.
[0071] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a metal oxide-doped hard carbon composite material, It is characterized in that The following steps are involved: S1, mixing hydrocarbon, pore former and metal salt in a solvent uniformly and performing hydrothermal reaction to obtain a metal-doped hard carbon precursor material; S2, using the metal-doped hard carbon precursor material as a matrix, depositing silver fluoride on the surface of the matrix by evaporation to obtain a silver-coated metal-doped hard carbon composite material; S3, adding the silver-coated metal-doped hard carbon composite material to acidic steam for surface etching, washing and drying to obtain the metal oxide-doped hard carbon composite material; The metal salt includes one or more of silver diethyldithiocarbamate, silver iodide of trimethylphosphine, silver trifluoromethanesulfonate, and silver diethylaminodithiocarbamate; The step S2 is specifically as follows: the evaporation furnace cavity A is the metal-doped hard carbon precursor material, the evaporation furnace cavity B is the silver fluoride powder, and the cavity B is evacuated to 1~5*10 -5 Torr, and heated at 200-400A, 300-500°C for 10-60min, then opened the valve between cavity A and cavity B to deposit silver fluoride on the surface of the substrate, and then cooled in an inert atmosphere to obtain a silver-coated metal-doped hard carbon composite material; The pore-forming agent includes one or more of nickel acetate, copper acetate, manganese acetate, bismuth acetate, and cobalt acetate.
2. The method for preparing the metal oxide-doped hard carbon composite material according to claim 1, It is characterized in that In step S1, the reaction temperature of the hydrothermal reaction is 100-200° C., and the reaction time is 1-6 hours.
3. The method for preparing the metal oxide-doped hard carbon composite material according to claim 1, It is characterized in that In step S2, the chamber A is evacuated to a pressure of 0.1-0.5 Torr.
4. The method for preparing the metal oxide-doped hard carbon composite material according to claim 1, It is characterized in that The step S3 is specifically as follows: transferring the silver-coated metal-doped hard carbon composite material to a reactor, evacuating to -0.09~-0.9MPa, and heating concentrated nitric acid or concentrated sulfuric acid in the reactor until it vaporizes for etching, cooling to room temperature, washing, and vacuum drying to obtain the metal oxide-doped hard carbon composite material.
5. The method for preparing the metal oxide-doped hard carbon composite material according to claim 4, It is characterized in that Etching for 30-300 minutes.
6. The method for preparing the metal oxide-doped hard carbon composite material according to claim 1, It is characterized in that Also includes at least one of the following technical features: The hydrocarbons include one or more of glucose, sucrose, lignin, and cellulose; The solvent includes one or more of benzyl alcohol, ferrocenyl methanol, cyclohexanol, 1,4-butanediol, and cinnamyl alcohol.
7. The method for preparing the metal oxide-doped hard carbon composite material according to claim 1, It is characterized in that The mass ratio of hydrocarbon, pore former, metal salt and solvent is 100:1~10:1~10:500~1000.
8. A metal oxide doped hard carbon composite material, It is characterized in that The composite material is obtained by the preparation method according to any one of claims 1 to 7, wherein the composite material has a core-shell structure, wherein the core is metal oxide-doped hard carbon and the shell is porous silver.
Citation Information
Patent Citations
Sulfur-doped biomass hard carbon material as well as preparation method and application thereof
CN113912039A
Cathode active material coated with fluorine compound for lithium secondary batteries and method for preparing the same
CN101156260A
Silver-doped lignin porous carbon nanosheet, preparation method thereof and application of silver-doped lignin porous carbon nanosheet in supercapacitor electrode material
CN110015660A
Metal oxide amorphous carbon coated hard carbon composite material as well as preparation method and application thereof
CN114420938A
Composite negative electrode material and preparation method and application thereof
CN115072703A