A nanomaterial with high-contrast reversible two-color fluorescence and LFP detection

Through the combination of rhodamine-modified aminated mesoporous silica and Mn2+-doped NaYF4:Yb, Er nanomaterials, a high-contrast reversible two-color fluorescent nanomaterial RB@MSN-UC is formed, which solves the problem of fluorescence in latent fingerprint detection in the existing technology. The problem of insufficient imaging contrast and stability has been achieved, and efficient latent fingerprint imaging and support for forensic investigations and medical diagnosis have been achieved.

CN116445152BActive Publication Date: 2024-10-18ANHUI UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310248705.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2024-10-18
Estimated Expiration
2043-03-10

Smart Images

  • Figure CN116445152B_ABST
    Figure CN116445152B_ABST
Patent Text Reader

Abstract

The invention discloses a nanomaterial with high-contrast reversible two-color fluorescence characteristics and LFP detection, which relates to the technical field of fluorescent materials. The nanomaterial is RB@MSN-UC, which includes rhodamine-modified amino mesoporous silica nanoparticles RB@MSN-NH2 and an upconversion nanomaterial UC loaded on RB@MSN-NH2; the UC is Mn 2+ The doped NaYF4:Yb,Er; the RB@MSN-UC nanomaterial emits yellow light under 980nm excitation and green light under 365nm excitation. The RB@MSN-UC of the present invention has good water dispersibility, and its reversible yellow-green switching fluorescence mode can effectively improve the optical contrast. Compared with other stimuli (such as pH, chemical stimuli), RB@MSN-UC has the advantages of cleanliness, non-invasiveness, no waste, high spatiotemporal accuracy, etc., so it is more convenient and can be used for the detection of LFP in forensic investigations, criminal cases and medical diagnosis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fluorescent materials, and in particular to a nano material with high-contrast reversible two-color fluorescent characteristics and LFP detection. Background Art

[0002] Fingerprints, as one of the important marks of an individual, play an important role in the fields of criminal science, medical diagnosis, etc. Those fingerprints that are difficult to identify with the naked eye are usually called latent fingerprints (LFP). At present, the rational development of an intelligent tool for high-contrast fluorescence imaging of LFP has attracted increasing attention in many applications such as medical diagnosis and forensic investigation.

[0003] Stimuli-responsive fluorescent materials can produce corresponding reversible / irreversible changes in photophysical or photochemical properties under the induction of external stimuli, which are mainly manifested as changes in color and fluorescence emission intensity / peak position, and thus have a wide range of applications in the fields of intelligent optoelectronic devices, optical information storage, and chemical / biosensors. The reversible on / off of fluorescence can stimulate the signal of responsive fluorescent materials to effectively increase the optical contrast and be cut off to identify the cations of candidate LFPs. Wang et al. (Angew. Chem. Int. Ed. 2018, 57, 6786–6790) first demonstrated the ClO / SCN-reversibly responsive lanthanide TbIII-CMC complex for high-contrast imaging of LFP; and subsequently developed a water-dispersible aptamer-functionalized covalent organic framework hydrogel whose fluorescence can be turned on and off when exposed to Cu 2+ / H2O. Despite their progress in increasing optical contrast, fingerprint details are often lost when exposed to chemical stimuli (ClO - 、SCN - , Cu 2+ ).

[0004] To effectively solve the above problems, fluorescent materials (such as spiropyran, azobenzene and diarylethenes) combined with optical switch materials and photochromic materials are one of the most attractive examples. Photoluminescence has many advantages, such as clean, non-large, no waste, high spatiotemporal precision, etc. In particular, reversible two-color light-switchable fluorescent polymer nanoparticles have good brightness and high-contrast fluorescence, which has been used in fluorescent imaging, anti-counterfeiting and inkjet printing. If polymer nanoparticles with high-contrast fluorescent properties can be selectively combined with fingerprint ridges, the goal of efficient LFP imaging can be achieved. Summary of the invention

[0005] Based on the technical problems existing in the background technology, the present invention proposes a nanomaterial RB@MSN-UC with high-contrast reversible two-color fluorescence characteristics, which has good water dispersibility. Its reversible yellow-green switching fluorescence mode can effectively improve the optical contrast and can be used for the detection of LFP in forensic investigations, criminal cases and medical diagnosis.

[0006] The present invention proposes a nanomaterial with high-contrast reversible dual-color fluorescence characteristics, the nanomaterial is RB@MSN-UC, which includes rhodamine-modified amino mesoporous silica nanoparticles RB@MSN-NH2 and an upconversion nanomaterial UC loaded on RB@MSN-NH2; the UC is Mn 2+ Doped NaYF4:Yb,Er; the RB@MSN-UC nanomaterial emits yellow light under 980nm excitation and green light under 365nm excitation.

[0007] The present invention also proposes a method for preparing the above-mentioned nanomaterial with high-contrast reversible dual-color fluorescence characteristics, comprising the following steps:

[0008] S1、Mn 2+ Preparation of doped NaYF4:Yb,Er(UC):

[0009] Aqueous solutions of manganese chloride, yttrium chloride, ytterbium chloride and erbium chloride are prepared respectively, added to a mixed solution containing an aqueous sodium hydroxide solution, oleic acid and anhydrous ethanol, and an aqueous sodium fluoride solution is added dropwise. The solution is stirred to react to form a colloidal solution, which is then transferred to an autoclave for heating and reaction. After the reaction is completed, the solution is washed and dried to obtain Mn 2+ Doped NaYF4:Yb,Er nanomaterials;

[0010] S2, Mn with negative charge 2+ Doped NaYF4:Yb,Er(UC - ) Preparation:

[0011] Mn 2+ The doped NaYF4:Yb,Er and sodium 4-styrenesulfonate were added to the sodium chloride solution, mixed evenly, left to react in the dark, centrifuged, washed, and dried to obtain a white powder, which is Mn with a negative charge. 2+ Doped NaYF4:Yb,Er;

[0012] S3. Preparation of rhodamine-composite amino-modified mesoporous silica RB@MSN-NH2:

[0013] Take rhodamine, CaCO3, CTAB and TEA, add them into water, stir, and heat in an oil bath for reaction; then add TEOS and continue stirring for reaction, cool, centrifuge, wash, and dry to obtain a pink powder, which is calcium carbonate / rhodamine composite silica nanospheres CaCO3@RB@SiO2; ultrasonically disperse CaCO3@RB@SiO2 in ethanol, add acid for acid etching, centrifuge, wash, and dry to obtain rhodamine composite mesoporous silica RB@MSN; then ultrasonically disperse RB@MSN in ethanol, add 3-aminopropyltriethoxysilane thereto, reflux reaction, centrifuge, and wash to obtain rhodamine composite amino mesoporous silica RB@MSN-NH2;

[0014] Preparation of S4. RB@MSN-UC

[0015] UC - and RB@MSN-NH2 were added to water, stirred for reaction, centrifuged, washed, and dried to obtain the nanomaterial RB@MSN-UC powder with high-contrast reversible dual-color fluorescence characteristics.

[0016] Preferably, in S1, in the aqueous solution, the molar ratio of manganese ions, yttrium ions, ytterbium ions and erbium ions is 30:50:18:2.

[0017] Preferably, in S1, the mixture is transferred to a reaction vessel and reacted at 180-220° C. for 8-12 h.

[0018] Preferably, in S1, a mixed solution of ethanol and cyclohexane is used for centrifugal washing; preferably, the volume ratio of ethanol to cyclohexane is 1:1.

[0019] Preferably, in S2, Mn 2+ The mass ratio of doped NaYF4:Yb,Er to sodium 4-styrenesulfonate is 1:1; preferably, the reaction is allowed to stand in the dark for 3-5 hours.

[0020] Preferably, in S3, the mass ratio of rhodamine, calcium carbonate, CTAB and TEA is 0.7-1.2:0.8-1.2:100:7-9; the mass volume ratio of rhodamine and TEOS g / L is 10:2.8-3.2.

[0021] Preferably, in S3, the mass ratio of RB@MSN to APTES is 30-40:1.

[0022] Preferably, in S3, rhodamine, CaCO3, CTAB and TEA are taken, added to water, stirred, and heated in an oil bath to 85-95°C for reaction for 6-8h; TEOS is then added and stirred for reaction for 2-3h, cooled, centrifuged, washed, and dried to obtain a pink powder, which is calcium carbonate / rhodamine composite silica nanospheres CaCO3@RB@SiO2; CaCO3@RB@SiO2 is ultrasonically dispersed in ethanol, acid is added to adjust the pH to 3.5-4.5, refluxed and stirred for reaction for 5-7h for acid etching, centrifuged, washed, and dried to obtain rhodamine composite mesoporous silica RB@MSN; RB@MSN is ultrasonically dispersed in ethanol, APTES is added thereto, refluxed for reaction for 5-7h, centrifuged, and washed to obtain rhodamine composite amino mesoporous silica RB@MSN-NH2;

[0023] Preferably, UC - The mass ratio of RB@MSN-NH2 is 1-2:1-2.

[0024] The present invention firstly prepares rhodamine-modified amino-modified mesoporous silica nanoparticles RB@MSN-NH2 by a self-template method, and then electrostatically adsorbs Mn 2+ The doped NaYF4:Yb,Er material is adsorbed on the surface of RB@MSN-NH2 mesoporous nanospheres to prepare a high-contrast reversible two-color fluorescent light switch material RB@MSN-UC. The present invention introduces two fluorescent nanomaterials, RB and UC, by electrostatic adsorption, effectively overcoming the problem of dye leakage; at the same time, the fluorescence of RB@MSN-UC can be reversibly switched between yellow and green under ultraviolet / laser irradiation, thereby significantly improving the optical contrast, thereby achieving efficient LFPs imaging.

[0025] Compared with some fluorescent materials for LFPs imaging disclosed in the prior art, the RB@MSN-UC nanomaterial of the present invention has the following advantages:

[0026] 1. RB@MSN-UC has good water dispersibility, while most organic small molecule fluorescent materials can only be dissolved in organic solvents;

[0027] 2. Encapsulating RB into porous silica nanoparticles can effectively overcome the dye leakage problem;

[0028] 3. The reversible yellow-green switching fluorescence mode can effectively improve the optical contrast, while the fluorescence mode can well avoid background interference;

[0029] 4. Compared with other stimuli (e.g., pH, chemical stimuli), RB@MSN-UC is more convenient due to its advantages of being clean, non-invasive, waste-free, and having high spatiotemporal precision.

[0030] 5. The RB@MSN-UC prepared in the present invention can be used for the detection of LFP in forensic investigations, criminal cases and medical diagnosis. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 TEM images of UC (a and b), RB@MSN-NH2 (c and d), and RB@MSN-UC (e and f) in Example 1 of the present invention;

[0032] Figure 2 X-ray diffraction patterns of MSNs (a), UCNPs (b), and RB@MSN-UC (c) in Example 1 of the present invention;

[0033] Figure 3 Fourier transform infrared spectra of MSNs (a), UCNPs (b), and RB@MSN-UC (line c) in Example 1 of the present invention;

[0034] Figure 4 (A) PL spectrum of UCNPs excited by 980 nm laser (a) and absorption spectrum of RB@MSN-NH2 (b); (B) PL spectrum of RB@MSN-UC excited by 508 nm laser (a) and absorption spectrum of UCNPs (b);

[0035] Figure 5 (A) is the effect of different excitation wavelengths on the fluorescence intensity of UC@RB@MNS-NH2 (from a to e, 428, 448, 468, 488, 508); (B) is the trend of the fluorescence intensity of UC@RB@MNS-NH2 under different excitation wavelengths.

[0036] Figure 6 Fluorescence images of RB@MSN-UC for LFPs detection under normal conditions (a, a', and a") and after water washing (b, b', and b");

[0037] Figure 7 Fluorescence images of fresh and differently aged fingerprints, (a and a') aged for 1 day, (b and b') aged for 7 days, (c and c') aged for 10 days, (d and d') aged for 21 days, and (e and e') aged for 30 days.

[0038] Figure 8 Fluorescence images of the imaged fingerprints, (a and a') 1 day, (b and b') 7 days, (c and c') 10 days, (d and d') 21 days, (e and e') 30 days;

[0039] Fig. 9Fluorescence images on different substrates under fluorescent lamp (ae), UV-365nm (a'-e') and laser-980nm; glass (a, a' and a"), platinum sheet (b, b' and b"), tile (c, c' and c") and A4 paper (d, d' and d"). DETAILED DESCRIPTION

[0040] The experimental instruments used in the present invention are shown in Table 1.

[0041] Table 1 Experimental instruments

[0042] Instrument Name model Manufacturer Electronic balance FA-1104N Shanghai Leton Industrial Co., Ltd. Magnetic stirrer 85-1 Shanghai Silo Instrument Co., Ltd. Vacuum drying oven DZF-6050 Shanghai Jinghong Experimental Equipment Co., Ltd. Electric constant temperature blast drying oven DHG-9036A Shanghai Jinghong Experimental Equipment Co., Ltd. Automatic Triple Pure Water Distiller VE-20LH-D Walchi Environmental Protection (Shenzhen) Co., Ltd. Fourier Transform Infrared Spectrometer NicoletNexus470 Thermo Instruments Ltd. Fluorescence spectrophotometer F-4600 HITACHI Ultraviolet-visible (UV-vis) spectrophotometer UV-2700 Japan Shimadzu Corporation High-resolution transmission electron microscopy JEM-2100F Hitachi Corporation Scanning electron microscopy TESCANVEGA3-SBH Hitachi Corporation

[0043] The technical solution of the present invention is described in detail below through specific embodiments.

[0044] Example 1

[0045] The preparation of RB@MSN-UC is as follows:

[0046] (1) Preparation of Ytterbium Chloride Hexahydrate

[0047] Put 0.289g of ytterbium oxide, 0.8ml of concentrated hydrochloric acid and 8mL of water into a round-bottom flask and stir in a 100°C oil bath until completely dissolved. After dissolution, heat the oil bath to 120°C to evaporate the solvent. When the product is about to evaporate to dryness, take out the round-bottom flask and use the residual heat to evaporate the product to dryness to obtain ytterbium chloride hexahydrate. Take it out and set aside.

[0048] (2) Mn 2+ Preparation of doped NaYF4:Yb,Er (molar ratio n Mn :n Y :n Yb :n Er =30:50:18:2)

[0049] 0.065 g of manganese chloride, 0.4552 g of yttrium chloride hexahydrate, 0.1494 g of ytterbium chloride hexahydrate, 0.076 g of erbium chloride hexahydrate, 1 g of sodium hydroxide and 0.4175 of sodium fluoride are added to 1 ml, 3 ml, 2 ml, 1 ml, 5 ml and 5 ml of deionized water respectively to prepare manganese chloride solution, yttrium chloride solution, ytterbium chloride solution, erbium chloride solution, sodium hydroxide solution and sodium fluoride solution for standby use;

[0050] 0.6 ml of manganese chloride solution, 1 ml of yttrium chloride solution, 0.9 ml of ytterbium chloride solution and 0.1 ml of erbium chloride solution were added to a mixed solution of 0.3 ml of sodium hydroxide solution, 5.0 ml of oleic acid and 10.0 ml of anhydrous ethanol, respectively. Then 4 ml of sodium fluoride solution was added dropwise to the mixed solution and stirred for 30 minutes to form a colloidal solution. The colloidal solution was then transferred to a 40.0 mL polytetrafluoroethylene-lined autoclave and heated at 200 ° C for 10 h. The solution was then cooled naturally and washed several times by centrifugation with a 1:1 mixed solution of ethanol and cyclohexane. Finally, the product was dried in a vacuum at 60 ° C to obtain Mn 2+ Doped NaYF4:Yb,Er powders (UCNPs).

[0051] (3) Mn with negative charge 2+ Doped NaYF4:Yb,Er nanoparticles (UC - )

[0052] The powder obtained in step (2) and 20 mg of sodium 4-phenylenesulfonate (PSS) were added to 5 ml of 0.1 mol / L sodium chloride solution. The mixed solution was rotated with a vortexer for 5 minutes and then placed in a dark place for 4 hours. The precipitate was collected by centrifugation at 10000 rpm for 5 minutes, washed with deionized water and ethanol three times, and then vacuum dried for 24 hours to obtain a white powder, which was Mn with a negative charge. 2+ Doped NaYF4:Yb,Er nanoparticles (UC - ),spare.

[0053] (4) Preparation of RB@MSN-NH2

[0054] Dissolve 10 mg of rhodamine, 10 mg of CaCO3, 1.0 g of CTAB and 80 mg of TEA in 20 mL of deionized water, stir at room temperature for 30 min to form a clear solution, then pour into a 50.0 mL three-necked round-bottom flask, reflux, heat and stir in an oil bath. After heating at 95 ° C for 6 h, slowly add 3 ml of TEOS and continue stirring for 3 h. After the solution is cooled, centrifuge at 10000 rpm for 5 minutes to collect the CaCO3@RB@SiO2 nanospheres, wash several times with ethanol until the supernatant is a transparent liquid, and then vacuum dry the precipitate for 24 h to obtain a pink powder, which is calcium carbonate / rhodamine composite silica nanospheres CaCO3@RB@SiO2;

[0055] 40 mg of CaCO3@RB@SiO2 was ultrasonically dispersed in 20 mL of ethanol for 10 min, and hydrochloric acid was added to adjust the pH to 4. The mixture was refluxed and stirred for 6 h for acid etching. After the reaction, the MSNs nanospheres were collected by centrifugation at 10,000 rpm for 5 min, washed three times with deionized water and ethanol, and vacuum dried for 24 h to obtain rhodamine composite mesoporous silica RB@MSN.

[0056] Then, 40 mg of RB@MSN was ultrasonically dispersed in 20 mL of ethanol and ultrasonically dispersed for 10 min. 1 mL of APTES was added thereto, and the mixture was heated and stirred at 78 °C under reflux conditions for 6 h. After the reaction, the MSN-NH2 nanospheres were collected by centrifugation at 10,000 rpm for 5 min, and washed three times with deionized water and ethanol to obtain rhodamine-complexed amino-modified mesoporous silica RB@MSN-NH2.

[0057] (5) Preparation of RB@MSN-UC

[0058] Take 10 mg of UC - 10 mg of RB@MSN-NH2 and 10 mg of RB@MSN-NH2 were added to 20 ml of deionized water and stirred for 4 h. The precipitate was collected by centrifugation at 10000 rpm for 5 min, washed with deionized water and ethanol for 3 times, and finally vacuum dried for 24 h to obtain RB@MSN-UC powder.

[0059] Mesoporous silica (MSNs) was prepared as follows: 0.04 g of SiO2 was dissolved in 20 ml of ethanol and ultrasonicated for 10 min, and then hydrochloric acid was added to the mixed solution to adjust the pH to 4. The mixed solution was heated and stirred at 78 ° C under reflux conditions for 6 hours. After the reaction was completed, the MSNs nanospheres were collected by centrifugation at 10000 rpm for 5 min, washed with deionized water and ethanol three times, and vacuum dried for 24 hours.

[0060] The preparation of aminated mesoporous silica (MSN-NH2) was as follows: 0.04 g of MSNs was dissolved in 20 ml of ethanol and ultrasonicated for 10 min, 1 mL of APTES was added thereto, and the mixture was heated and stirred at 78 °C under reflux conditions for 6 h. After the reaction, the MSN-NH2 nanospheres were collected by centrifugation at 10,000 rpm for 5 min and washed three times with deionized water and ethanol.

[0061] 1. Characterization of the prepared RB@MSN-UC

[0062] Figure 1The TEM images show that UC (a and b) is roughly circular in shape and about 20 nm in size. RB@MSN-NH2 (c and d) is approximately 20 nm in size and is a porous circular shape, indicating that RB@MSN-NH2 has a large specific area and a strong adsorption capacity for materials. RB@MSN-UC (e and f) shows that more nanoparticles are adsorbed together with UC, which indicates that the material was successfully prepared.

[0063] Figure 2 The X-ray diffraction diagram shows that line (a) in the figure shows that only a relatively broad dispersion peak appears near 25°, which indicates the mesoporous structure and amorphous crystallinity of MSNs. The diffraction peaks of line (b) at 29.86°, 30.73°, 34.63°, 38.80°, 43.40°, 46.40°, 52.05°, 53.07°, 53.62°, 55.22°, 61.21°, 64.96° and 70.30° correspond to Mn 2+ Doped NaYF4: Yb, Er (110), (101), (102), (111), (201), (210), (002), (300), (211), (102), (112), (200) and (311). The basic diffraction peaks of line (c) are roughly the same as those of line (b), but some small protrusions appear at 22.57° in line (c), indicating the presence of MSNs.

[0064] Figure 3 This is the FT-IR spectrum. From the line (a) in the figure, we can see that 3458cm -1 The strong absorption peaks at 800 and 468 cm-1 are attributed to the stretching vibration of Si-OH. -1 The absorption peak at 1638cm is attributed to the stretching vibration of the symmetrical Si-O-Si skeleton; -1 The peaks at 1100 cm -1 The broad peak at 1090 cm is attributed to the asymmetric bending vibration of Si-O-Si. -1 There is an absorption peak at 463 cm, which is attributed to the stretching vibration of CO in UC. -1 The absorption peak at has changed and is much narrower than that in line (a), which may be caused by the doping of UCNPs particles. The other absorption peaks have not changed significantly.

[0065] 2. Optical properties test of RB@MSN-UC nanoparticles

[0066] Figure 4(A) shows the fluorescence spectra of UCNPs and RB@MSN-NH2 excited at 980nm. It can be seen that UCNPs (a) has two peaks at 525nm and 542nm, with fluorescence intensities of 80 and 131, respectively, that is, the nanomaterial exhibits the strongest yellow fluorescence at 542nm. RB@MSN-NH2 (b) has almost no peak, indicating that there is no fluorescence at this excitation wavelength. Figure 4 (B) shows the fluorescence spectra of UCNPs and RB@MSN-UC excited at 508 nm. It can be seen that the peak of UCNPs is slightly more to the left than that of RB@MSN-UC, which are 525 nm and 552 nm respectively, and the fluorescence intensity in this band is obviously 2-3 times different.

[0067] Figure 5 (A) shows the fluorescence intensity of RB@MSN-UC under different excitations. It can be seen that the fluorescence intensity increases with the increase of the excitation wavelength. When ex=508, the fluorescence intensity reaches the maximum. If the excitation wavelength is increased further, the fluorescence spectrum curve cannot be displayed well, so 508nm is the most suitable excitation light. Figure 5 (B) shows the trend of fluorescence intensity under different excitations.

[0068] The fluorescence intensity of RB@MSN-NH2 will also change with the change of UC content. The change of fluorescence curve when 10mg of RB@MSN-NH2 was doped with different contents of UC (1mg, 2mg, 3mg, 4mg, 5mg) was studied. It was found that when the UC content reached 2mg, the fluorescence intensity reached the maximum. When it was greater than 2mg, the fluorescence intensity would weaken with the increase of UC content.

[0069] The pH value greatly affects the fluorescence properties of fluorescent materials. Different pH values ​​have different quenching degrees for fluorescent materials. The pH value is an important factor that cannot be ignored for fluorescent materials. The fluorescence intensity change curves of RB@MSN-UC at different pH values ​​(5.7, 6.5, 7.0, 7.5, 8.0) were studied, and it was found that the fluorescence intensity of RB@MSN-UC changes with the change of pH. When pH = 7.0, the fluorescence intensity of the material reaches the maximum value; when pH > 7, the fluorescence intensity decreases with the increase of pH, which is because the material undergoes quenching.

[0070] The illumination time also has a certain impact on the fluorescence intensity of the material. RB@MSN-UC still has strong fluorescence after 5 minutes of excitation at 508nm. As time goes by, the fluorescence intensity of the material continues to weaken, and it has weak fluorescence at 25 minutes. This is because different illumination times cause different degrees of quenching of the material.

[0071] RB@MSN-UC nanomaterials reveal latent fingerprints

[0072] The composition of fingerprints is complex. Generally speaking, fingers are always full of fat due to the secretion of sebaceous glands, and they are constantly touching oily parts of the body such as the face or forehead. Many fingerprint development methods are based on the affinity between the oily components in fingerprints and the hydrophobic compounds in the developer. Figure 6 The fingerprint images of RB@MSN-UC under normal conditions (a, a' and a") and after water washing (b, b' and b") are shown. Since fingerprints washed with water will cause some oil to be lost, it is difficult for the material to adsorb on them. The silica material in RB@MSN-UC enhances the adsorption capacity of the composite material, so that there is no big difference in the fingerprint images under the above two conditions, and the fingerprint pattern can be clearly seen. This shows that the RB@MSN-UC composite material has good adsorption performance and excellent fluorescence stability.

[0073] The fingerprint developed under ultraviolet light and laser has similar readability. There is a certain contrast between ultraviolet light and laser, such as Figure 7 (ae, a'-e'), the fluorescence photos under UV light clearly show enhanced readability. For aged fingerprints stored for 1 day and 30 days, the advantage of fluorescence development is more obvious, because the resolution / clarity of the developed fluorescence images of the fingerprint pattern is stronger than the fingerprint under infrared. For fingerprints stored for 30 days, darker fluorescence is shown under UV and laser, most likely because some components on the ridges are lost over time. However, the fluorescence image shows higher resolution, probably because the adsorption of RB@MSN-UC nanoparticles is reduced, thereby weakening the fluorescence halo effect, but the general outline of the fingerprint can still be seen, which shows that the composite material has good adsorption properties and excellent fluorescence stability.

[0074] Figure 8 (ae) and (a'-e') show the images of the fluorescent fingerprint after application at different time periods. Most fluorescent materials have the phenomenon of quenching, which makes it difficult to preserve the image for a long time. However, the RB@MSN-UC composite material was applied for 30 days (e.g. Figure 8 (e and e')) fingerprints, the fluorescence image of the fingerprint can still be seen under ultraviolet and laser, although it is smaller than that on the first day (such as Figure 8 This shows that the material has certain chemical stability and pit quenching performance.

[0075] Glass, platinum sheets and tiles and A4 paper are common monochrome substrates, and the fingerprint photos obtained under different conditions have similar contrast and clarity. Fig. 9The following figure shows the photos of latent fingerprints detected on glass, platinum sheet, ceramic tile and A4 paper substrate. As can be seen from the figure, fingerprints on glass and platinum sheet can show clear fingerprints under fluorescent light, ultraviolet light and laser (such as Fig. 9 a, a', a", b, b' and b"). Under fluorescent light on the tile, the pattern of fingerprints cannot be seen clearly (such as Fig. 9 c), while under UV and laser conditions, a clear outline of the fingerprint was shown (e.g. Fig. 9 c'and c”). The fingerprint on A4 paper has strong background interference, such as Fig. 9 (d) and (d') show that it is difficult to see the fingerprint under fluorescent light and ultraviolet light, but the outline of the fingerprint is displayed under laser light, eliminating the influence of background interference on fingerprint imaging. The above data show that RB@MSN-UC has high contrast, high selectivity and no background interference on all tested substrates.

[0076] In summary, the present invention has successfully designed and synthesized the nanoparticle RB@MSN-UC high-contrast reversible dual-color fluorescent light switch to achieve efficient LFPs imaging. The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field within the technical scope disclosed by the present invention, according to the technical solution and its inventive concept of the present invention, shall be covered within the protection scope of the present invention.

Claims

1. A nanomaterial with high-contrast reversible two-color fluorescence characteristics, characterized in that: The nanomaterial is RB@MSN-UC, which includes rhodamine-modified amino-modified mesoporous silica nanoparticles RB@MSN-NH2 and upconversion nanomaterials UC loaded on RB@MSN-NH2; the UC is Mn 2+ Doped NaYF4:Yb,Er; the RB@MSN-UC nanomaterial emits yellow light under 980nm excitation and green light under 365nm excitation.

2. The method for preparing the nanomaterial having high-contrast reversible dual-color fluorescence characteristics as claimed in claim 1, characterized in that: The following steps are involved: S1、Mn 2+ Preparation of doped NaYF4:Yb,Er (UC): Aqueous solutions of manganese chloride, yttrium chloride, ytterbium chloride and erbium chloride are prepared respectively, added to a mixed solution containing an aqueous sodium hydroxide solution, oleic acid and anhydrous ethanol, and an aqueous sodium fluoride solution is added dropwise. The solution is stirred to react to form a colloidal solution, which is then transferred to an autoclave for heating and reaction. After the reaction is completed, the solution is washed and dried to obtain Mn 2+ Doped NaYF4:Yb,Er nanomaterials; S2, Mn with negative charge 2+ Doped NaYF4:Yb,Er (UC - ) Preparation: Mn 2+ The doped NaYF4:Yb,Er and sodium 4-styrenesulfonate were added to the sodium chloride solution, mixed evenly, left to react in the dark, centrifuged, washed, and dried to obtain a white powder, which is Mn with a negative charge. 2+ Doped NaYF4:Yb,Er; S3. Preparation of rhodamine-composite amino-modified mesoporous silica RB@MSN-NH2: Take rhodamine, CaCO3, CTAB and TEA, add them into water, stir, and heat in an oil bath for reaction; then add TEOS and continue stirring for reaction, cool, centrifuge, wash, and dry to obtain a pink powder, which is calcium carbonate / rhodamine composite silica nanospheres CaCO3@RB@SiO2; ultrasonically disperse CaCO3@RB@SiO2 in ethanol, add acid for acid etching, centrifuge, wash, and dry to obtain rhodamine composite mesoporous silica RB@MSN; then ultrasonically disperse RB@MSN in ethanol, add 3-aminopropyltriethoxysilane thereto, reflux reaction, centrifuge, and wash to obtain rhodamine composite amino mesoporous silica RB@MSN-NH2; Preparation of S4. RB@MSN-UC UC - and RB@MSN-NH2 were added to water, stirred for reaction, centrifuged, washed, and dried to obtain the nanomaterial RB@MSN-UC powder with high-contrast reversible dual-color fluorescence characteristics.

3. The method according to claim 2, characterized in that In S1, the molar ratio of manganese ions, yttrium ions, ytterbium ions and erbium ions in the aqueous solution is 30:50:18:

2.

4. The method according to claim 2 or 3, characterized in that: In S1, the mixture is transferred to an autoclave and reacted at 180-220°C for 8-12 hours.

5. The method according to claim 4, characterized in that In S1, a mixed solution of ethanol and cyclohexane is used for centrifugal washing; the volume ratio of ethanol to cyclohexane is 1:

1.

6. The method according to claim 5, characterized in that In S2, Mn 2+ The mass ratio of doped NaYF4:Yb,Er to sodium 4-styrenesulfonate is 1:1; the reaction is allowed to stand in the dark for 3-5 hours.

7. The method according to claim 6, characterized in that In S3, the mass ratio of rhodamine, calcium carbonate, CTAB and TEA is 0.7-1.2:0.8-1.2:100:7-9; the mass volume ratio of rhodamine and TEOS is 10:2.8-3.2 g / L.

8. The method according to claim 7, characterized in that In S3, the mass volume ratio of RB@MSN and APTES was 30-40:1 in mg / mL.

9. The method according to claim 8, characterized in that In S3, rhodamine, CaCO3, CTAB and TEA are added to water, stirred, and heated in an oil bath to 85-95°C for reaction for 6-8h; TEOS is then added and stirred for reaction for 2-3h, cooled, centrifuged, washed, and dried to obtain a pink powder, which is calcium carbonate / rhodamine composite silica nanospheres CaCO3@RB@SiO2; CaCO3@RB@SiO2 is ultrasonically dispersed in ethanol, acid is added to adjust the pH to 3.5-4.5, refluxed and stirred for reaction for 5-7h, acid-etched, centrifuged, washed, and dried to obtain rhodamine composite mesoporous silica RB@MSN; RB@MSN is ultrasonically dispersed in ethanol, APTES is added thereto, refluxed for reaction for 5-7h, centrifuged, and washed to obtain rhodamine composite amino mesoporous silica RB@MSN-NH 2。 10. The method according to claim 9, characterized in that UC - The mass ratio of RB@MSN-NH2 is 1-2:1-2.

Citation Information

Patent Citations

  • Preparation method of fluorescent mesoporous silica-based core-shell nanoscale capsule

    CN102350281A

  • Cl-PFR-coated MSN-NH2 nano composite material as well as preparation method and application thereof

    CN115651355A