A Beta molecular sieve catalyst and its preparation method and application in the preparation of cyclohexylbenzene

By accurately controlling the distribution of acid sites in Beta molecular sieve catalysts, the problem of insufficient selectivity and conversion of catalysts under high-quality spacespeed conditions in the prior art is solved, and efficient alkylation reaction between benzene and cyclohexene is achieved. Extend the service life of the catalyst.

CN116459866BActive Publication Date: 2024-11-01GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310466324.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-01
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

When the existing molecular sieve catalyst catalyzes the alkylation reaction between benzene and cyclohexene, it is difficult to maintain high selectivity and conversion under conditions where the mass space velocity is higher than 2h-1, and the distribution of acidic sites is difficult to accurately regulate. , resulting in reduced reactivity and short service life.

Method used

By controlling the concentration and distribution of acidic sites in the Beta molecular sieve catalyst, it is ensured that the acidic sites in the a-axis and b-axis channel account for 49-99% of the total concentration, and the acidic sites are accurately regulated by specific synthesis methods and probe determination techniques. Point distribution to form an excellent catalyst.

Benefits of technology

The selectivity of the target reaction and the conversion of reactants were significantly improved under the condition that the mass space speed was higher than 2h-1, and the service life of the catalyst was extended, reaching a selectivity of 70% and a conversion of 21%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116459866B_ABST
    Figure CN116459866B_ABST
Patent Text Reader

Abstract

The present invention discloses a Beta molecular sieve catalyst, a preparation method thereof and an application thereof in the preparation of cyclohexylbenzene, and specifically relates to the technical field of catalyst preparation. The Beta molecular sieve catalyst provided by the present invention has pores in three directions of a, b and c, wherein the concentration of #imgabs0# acid sites in the pore skeleton in the a-axis and b-axis directions can be precisely controlled to a specific value, which accounts for 49-99% of the total concentration of acid sites in the molecular sieve skeleton, and the #imgabs1# acid sites in the a-axis and b-axis pores of the molecular sieve are the active sites of the Beta molecular sieve catalyst provided by the present invention when catalyzing the alkylation reaction between benzene and cyclohexene. Therefore, when the #imgabs2# acid sites can be precisely distributed in the a-axis and b-axis pores of the Beta molecular sieve and account for more than 49% of the total concentration, the mass space velocity of the reactant flow into the system of the Beta molecular sieve catalyst in the reaction system is higher than 2h ‑1 In the case of the above reaction, the target reaction has excellent selectivity and reactant conversion rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to a Beta molecular sieve catalyst and a preparation method thereof and application thereof in the preparation of cyclohexylbenzene. Background Art

[0002] As environmental issues become increasingly prominent, the use of environmentally friendly solid acid catalysts to catalyze the alkylation of cyclohexene and benzene to produce cyclohexylbenzene has received increasing attention in the current production of cyclohexylbenzene. Among solid acid catalysts, molecular sieve catalysts have received great attention due to their high thermal stability, shape selectivity, and precisely adjustable acidity.

[0003] From the perspective of the mechanism of molecular sieve catalytic reaction, the acidic sites in the molecular sieve are the active sites for the catalytic reaction, which are usually divided into There are two types of acid sites: Lewis acid sites and Lewis acid sites. In the alkylation reaction of benzene with cyclohexene, the key role is played by Acid sites are acid sites that can donate protons during catalytic reactions. However, existing processes such as dealumination and surface passivation are limited in regulating It is difficult to achieve accurate distribution of acid sites, and in molecular sieves, not all pores Acid sites can all catalyze the target reaction, so it is difficult to improve the target reaction selectivity and reactant conversion rate of the alkylation reaction between benzene and cyclohexene using existing processes.

[0004] The prior art discloses an application of a molecular sieve-supported heteropoly acid catalyst in the synthesis of cyclohexylbenzene. A catalyst for the alkylation reaction between benzene and cyclohexene is prepared by supporting a heteropoly acid in a Y-type molecular sieve. The heteropoly acid in the molecular sieve is the acid site for the catalytic reaction. Based on the distribution of acid sites, the catalyst can only have high selectivity and reactant conversion rate for the target reaction in a closed and high-pressure system. When benzene and cyclohexene in the reaction system are constantly flowing, the contact area between the catalyst and benzene and cyclohexene decreases, which inevitably leads to a decrease in the selectivity of the target reaction and the reactant conversion rate in the reaction system. Other existing catalysts for catalyzing the alkylation reaction between benzene and cyclohexene can generally only be used when the mass space velocity of the reactant flow is 2h / min when the reactant is constantly flowing in the reaction system. -1 The catalytic reaction is carried out under the conditions of , when the mass space velocity is further increased, the catalyst is easily deactivated, so the selectivity of the target reaction and the conversion rate of the reactants are both reduced. Summary of the invention

[0005] In order to solve the problem that the existing catalysts used for catalyzing the alkylation reaction between benzene and cyclohexene have a mass space velocity higher than 2h-1 In order to solve the problem of insufficient selectivity of target products and insufficient conversion rate of reactants under the condition of The concentration of acid sites and their distribution in different three-dimensional pores improve the catalyst's thermal conductivity at mass space velocity above 2h -1 The selectivity of the target product and the conversion rate of the reactants in the alkylation reaction between benzene and cyclohexene catalyzed under the conditions of.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned Beta molecular sieve catalyst.

[0007] Another object of the present invention is to provide a method for catalyzing the alkylation reaction between benzene and cyclohexene.

[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0009] A Beta molecular sieve catalyst, the pore framework of which The total concentration of acid sites is 0.077-0.101 mmol / g, among which the molecular sieve a-axis and b-axis pore skeleton The total concentration of acid sites accounts for the molecular sieve pore framework of Beta molecular sieve catalyst. 49-99% of the total acidic site concentration.

[0010] In the pore framework of the Beta molecular sieve catalyst provided by the present invention, the bridged hydroxyl group (Si-OH-Al) plays a key role in catalyzing the alkylation reaction between benzene and cyclohexene. Acidic sites. The total concentration of acid sites is controlled because the reaction system is complex during the synthesis of Beta molecular sieve catalysts. When the total concentration of acid sites can be controlled to 0.077-0.101 mmol / g, it is beneficial to The concentration of acid sites is controlled to account for all 49-99% of the total concentration of acidic sites.

[0011] When the Beta molecular sieve pore framework When the total concentration of acid sites is 0.077 to 0.101 mmol / g, the Beta molecular sieve catalyst provided by the present invention has excellent target reaction selectivity and reactant conversion rate when catalyzing the alkylation reaction between benzene and cyclohexene. However, in terms of the contribution to the selectivity and conversion rate, more importantly, in the catalyst provided by the present invention The concentration of acid sites in the pore skeleton in the a-axis and b-axis directions of the molecular sieve can be controlled to a value within the range of 49 to 99%, which shows that the Beta molecular sieve catalyst provided by the present invention can accurately control The distribution concentration of acid sites in the pore framework of the molecular sieve a-axis and b-axis directions, and when the distribution concentration of acid sites in the pore framework of the molecular sieve a-axis and b-axis directions is The concentration of acid sites accounts for the total pore size of the molecular sieve. When the total concentration of acid sites can reach 49-99%, the mass space velocity of the Beta molecular sieve catalyst prepared by the present invention in the reactant flow system can be higher than 2h -1 The alkylation reaction between benzene and cyclohexene has excellent target reaction selectivity and reactant conversion rate under the conditions of

[0012] Specifically, Beta molecular sieve is a porous aluminosilicate crystal, whose basic skeleton structure is composed of silicon oxygen and aluminum oxygen tetrahedron, with a three-dimensional twelve-membered ring staggered channel structure, and the a-axis and b-axis directions are the diameters. (these two values ​​are the lengths of the shortest and longest diagonals in the channel section) of a straight channel, and the c-axis direction is a curved channel that intersects the a-axis and the b-axis. Its channel diameter is In the alkylation reaction of benzene and cyclohexene to form cyclohexylbenzene, the kinetic diameters of benzene and cyclohexene are and Therefore, benzene molecules can diffuse in the channels of the a, b, and c axes of the Beta molecular sieve, while cyclohexene can only diffuse in the channels of the a and b axes. Under the action of the acidic site, it is protonated to generate an active cyclohexane carbon cation, which can form a conjugated system with benzene and then release hydrogen ions to generate cyclohexylbenzene. However, cyclohexene cannot enter the c-axis channel of the Beta molecular sieve, so the c-axis channel skeleton The acid sites do not catalyze the reaction between benzene and cyclohexene. The acidic sites will adsorb smaller benzene molecules, which will lead to a reduction in the distribution of benzene in the a-axis and b-axis pores, making the self-polymerization reaction of cyclohexene easier to proceed. This is a side reaction in the system and will cause carbon deposits to form in the a- and b-axis pores, which not only reduces the catalytic activity of the Beta molecular sieve catalyst for the reaction between benzene and cyclohexene, but also reduces its service life.

[0013] In the existing Beta molecular sieve Acidic sites are often randomly distributed, although in the a-axis and b-axis pore framework of the molecular sieve Acid site concentration in the molecular sieve The proportion of acid sites in the total concentration has a certain value, but this value cannot be precisely controlled by changing the preparation conditions. The distribution of acid sites can be precisely controlled and the a-axis and b-axis pores in the skeleton The acid site concentration accounts for When the total concentration of acid sites is 49-99%, the mass space velocity of the Beta molecular sieve catalyst in the reactant flow system is higher than 2h -1 The alkylation reaction between benzene and cyclohexene has excellent target reaction selectivity and conversion rate under the conditions of

[0014] In a specific embodiment of the present invention, the Beta molecular sieve pore framework The acid site concentration was obtained by using pyridine and 2,4,6-trimethylpyridine with different molecular sizes as probes and combining them with infrared spectroscopy. Pyridine can adsorb to the pores in three directions. On the acidic site, 2,4,6-trimethylpyridine can only adsorb to the a and b axes. After successful adsorption, characteristic absorption peaks will appear in the infrared spectrum. The Lambert-Beer law can be used to measure the peak intensity to obtain the peak intensity in the pores in different directions. The concentration of acidic sites.

[0015] Preferably, the pores in the molecular sieve a-axis and b-axis directions of the Beta molecular sieve catalyst are The concentration of acid sites in the molecular sieve framework 59-99% of the total concentration of acidic sites.

[0016] When the pores in the a-axis and b-axis directions of the Beta molecular sieve catalyst are The concentration of acid sites in the molecular sieve framework When the total concentration of acid sites reaches 59-99%, the alkylation reaction between benzene and cyclohexene can be catalyzed. Acidic sites account for all The proportion of acidic sites is also higher, so the catalyst has higher selectivity for the target reaction and higher conversion rate of the reactants.

[0017] The present invention also protects a method for preparing the above-mentioned Beta molecular sieve catalyst, which specifically comprises the following steps:

[0018] S1. dissolving tetraethylammonium hydroxide in a solvent to obtain a solution A;

[0019] S2. Adding an aluminum source and a silicon source to the solution A obtained in step S1 in sequence, and aging to obtain a gel B;

[0020] S3. Crystallizing the gel B obtained in step S2 to obtain a Beta molecular sieve catalyst;

[0021] In step S2, the molar ratio of the silicon source, the aluminum source and tetraethylammonium hydroxide is 100:(3-7):(40-70).

[0022] The purpose of steps S2 and S3 is to make silicon atoms and aluminum atoms build a Beta molecular sieve framework around the structure directing agent molecules, wherein the purpose of aging is to form a uniform gel B in the system of solution A, and crystallization can convert gel B into Beta molecular sieve.

[0023] In the synthesis of Beta molecular sieves, tetraethylammonium hydroxide (TEAOH) as a structure-directing agent plays the role of a "template" and can induce The formation of acidic sites. Specifically, in the process of preparing Beta molecular sieve, due to the + Positively charged, [AlO4] in the molecular sieve synthesis system - The species interact electrostatically, so Al species are introduced into the molecular sieve framework, inducing partial silicon in the molecular sieve channel framework to be replaced by aluminum, and finally generating bridged hydroxyl groups (Si-OH-Al) in the molecular sieve. Because the silicon in the channel framework exists in the form of uncharged tetracoordinate SiO4, and when the silicon atoms in the framework are replaced by aluminum atoms, [AlO4] can be generated. - This negatively charged species neutralizes TEA + After subsequent calcination, it reacts with [AlO4] - Combined TEA + will be transformed into H + , which plays a key role in catalyzing the alkylation reaction between benzene and cyclohexene. The acidic sites are formed after calcination and can stably exist under the general temperature conditions of the reaction of benzene and cyclohexene during the catalytic reaction.

[0024] The ratio of the amount of silicon source, aluminum source and tetraethylammonium hydroxide in step S2 is limited to 100:(3-7):(40-70) because within this range, the pore framework of the obtained Beta molecular sieve catalyst is The total concentration of acid sites can be controlled to 0.077-0.101 mmol / g, and most of them Acid sites are composed of TEA + Induced generation, so the molecular sieve a-axis and b-axis direction The total concentration of acid sites in the molecular sieve About 99% of the total acidic site concentration.

[0025] Preferably, a sodium source is also added in step S1.

[0026] Adding sodium source will increase the c-axis pore size in Beta molecular sieve However, the preferred experimental scheme of adding a sodium source is not based on considerations of catalyst performance. In step S1, TEAOH and a sodium source with different cation sizes are added to the system in order to utilize TEA + While synthesizing Beta molecular sieves through the structure-directed effect of TEA + and Na + Differences in size and electropositive TEA + and Na + and electronegativity [AlO4] - The charge matching relationship between species is controlled by TEA in the Beta molecular sieve synthesis system. + and Na + ratio to achieve precise control [AlO4] - The distribution of species in different three-dimensional channels of Beta molecular sieve, thereby controlling The distribution of acid sites in different pores of Beta molecular sieve a-axis, b-axis and c-axis. + (Diameter is ) can enter the larger a-axis and b-axis channels in the Beta molecular sieve while acting as a template, while the smaller Na + (The ionic radius is ) can enter the channels of the three axes a, b, and c, and Na + It can also be induced by charge Therefore, adding a sodium source in step S1 can accurately control the formation of acidic sites in the Beta molecular sieve. The distribution concentration of acid sites in the three axes a, b, and c. Methods for the distribution of acidic sites include regulating the silicon-aluminum ratio in the molecular sieve synthesis raw materials, dealumination, surface passivation, etc., but it is difficult to achieve Precise regulation of the distribution of acidic sites. Specifically, by adjusting the silicon-aluminum ratio of the reactants to control When the distribution of acid sites is studied, the correlation between the Si / Al ratio and the distribution of acid sites is weak, so it is difficult to precisely control the a, b, and c axes of Beta molecular sieve. Acid site concentration; when the acid site distribution is regulated by dealumination, new channels are induced in the molecular sieve through a corrosion-like effect, and this "corrosion" means that part of the original channel Acidic sites will fall off; when the distribution of acidic sites is regulated by surface passivation, once the conditions of use of the catalyst change, the passivating material will easily fall off, and the Precise regulation of acidic site distribution.

[0027] More preferably, in step S1, the molar ratio of tetraethylammonium hydroxide to the sodium source is 5:(0-0.273).

[0028] When the molar ratio of TEAOH to sodium source is 5:(0-0.273), the pores in the a-axis and b-axis directions of the Beta molecular sieve are The concentration of acid sites can account for More than 49% of the total concentration of acid sites is achieved The precise distribution of acidic sites in the pore framework of the Beta molecular sieve ensures the catalytic activity of the Beta molecular sieve catalyst for the target reaction.

[0029] In a specific embodiment of the present invention, the molar ratio of water to TEAOH in step S1 can be (0.02-0.05):1, and the sodium source can be arbitrarily selected from one or more of sodium chloride, sodium bromide, sodium sulfate and sodium thiocyanate; the specific operation method of aging solution A in step S2 can be placing solution A at room temperature for 2-6 hours, the silicon source can be fumed silica, and the aluminum source can be aluminum isopropoxide; the specific operation method of crystallizing gel B in step S3 can be placing gel A at 140-160°C for 5-10 days, and after the crystallization is completed, the obtained Beta molecular sieve catalyst needs to be washed until the washing liquid is neutral, and the calcination can be calcined in an air atmosphere at 550-600°C for 4-8h.

[0030] More preferably, the sodium source in step S1 is sodium chloride.

[0031] Preferably, the molar ratio of the silicon source, the aluminum source and tetraethylammonium hydroxide in step S2 is 100:(4-6):(50-60).

[0032] Preferably, in step S2, a mesoporous template agent needs to be added to the solution A obtained in step S1.

[0033] By adding a mesoporous template to the system of synthesizing molecular sieves, the prepared Beta molecular sieve catalyst can have a multi-level pore structure in which mesopores and micropores coexist. This multi-level pore structure is accompanied by a larger specific surface area of ​​the catalyst. Therefore, in the same amount of time, the unit volume of catalyst can combine with more reactants, and the reaction will proceed faster.

[0034] In a specific embodiment of the present invention, the mesoporous template agent can be arbitrarily selected from one or more of dodecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide and hexadecyltrimethylammonium bromide.

[0035] Preferably, the mesoporous template agent is hexadecyltrimethylammonium bromide.

[0036] Preferably, the molar ratio of the mesoporous template added in step S2 to the silicon source is (1-3):50.

[0037] The present invention also protects a method for catalyzing the alkylation reaction between benzene and cyclohexene, which specifically comprises the following steps:

[0038] Benzene and cyclohexene are mixed to obtain a reaction solution, and the reaction solution is introduced into a reactor containing the above-mentioned Beta molecular sieve catalyst to carry out a reaction.

[0039] Preferably, the molar ratio of benzene to cyclohexene in the reaction solution is (10-30):1.

[0040] When the Beta molecular sieve catalyst provided by the present invention is used to catalyze the alkylation reaction between benzene and cyclohexene, when the molar ratio of benzene to cyclohexene is lower than 10:1, there is too little benzene in the reaction system, and the side reaction of olefin self-polymerization is likely to occur, which is not conducive to improving the selectivity of the target reaction of generating cyclohexylbenzene in the reaction system. However, when the molar ratio of benzene to cyclohexene in the system is higher than 30:1, there is too much unused benzene in the system, which is not conducive to energy saving.

[0041] More preferably, the molar ratio of benzene to cyclohexene in the reaction solution is (15-25):1.

[0042] Preferably, the mass space velocity of the reaction solution when it is passed into the reactor is 8 to 16 h -1 .

[0043] Space velocity refers to the amount of raw material passing through a unit catalyst per unit time, which reflects the processing capacity of the catalyst. In a specific embodiment of the present invention, the mass space velocity when the reaction solution is passed into the reactor is the raw material mass flow rate (in kgh -1 In industry, when catalyzing the alkylation reaction between benzene and cyclohexene, the mass space velocity of the reaction liquid entering the reactor is generally 0.5 to 2 h -1 The Beta molecular sieve catalyst provided by the present invention has the advantage of high catalytic activity and can rapidly carry out the alkylation reaction between benzene and cyclohexene. Therefore, the mass space velocity of the reaction liquid when it is introduced into the reactor is 8 to 16 h -1 catalyzes reactions under harsh conditions.

[0044] In a specific embodiment of the present invention, the temperature in the reactor is 70-90°C.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] The Beta molecular sieve catalyst provided by the present invention can accurately control The concentration and distribution of acid sites in the three-dimensional pores make it have excellent catalytic activity in the alkylation reaction between benzene and cyclohexene. -1 It can be used under harsh conditions and has a service life of up to 21 hours. At the same time, it can enable the reaction system to have a target reaction selectivity of up to 70%, and the conversion rate of the reactant cyclohexene can also be increased to 21%. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 The X-ray diffraction patterns of the Beta molecular sieve catalysts prepared in the examples and comparative examples of the present invention are shown in FIG.

[0048] Figure 2 The infrared spectra of the Beta molecular sieve catalysts prepared in the examples of the present invention and the comparative examples are shown when 2,4,6-trimethylpyridine is used as a probe molecule.

[0049] Figure 3 The infrared spectra of the Beta molecular sieve catalysts prepared in the examples of the present invention and the comparative examples are shown when pyridine is used as a probe molecule.

[0050] Figure 4 The target reaction selectivity and cyclohexene conversion rate change diagram when the Beta molecular sieve catalyst prepared by the present invention is used to catalyze the alkylation reaction between benzene and cyclohexene.

[0051] Figure 5 This is the nitrogen adsorption-desorption isotherm diagram of the Beta molecular sieve catalyst prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0052] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.

[0053] Example 1

[0054] A Beta molecular sieve catalyst, wherein the molecular sieve pore framework of the Beta molecular sieve catalyst The total concentration of acid sites is 0.077mmol / g, of which the molecular sieve a-axis and b-axis pore skeleton The total concentration of acid sites accounts for the molecular sieve pore framework of Beta molecular sieve catalyst. 49% of the total concentration of acidic sites.

[0055] The preparation method of the Beta molecular sieve catalyst in the above-mentioned embodiment 1 specifically comprises the following steps:

[0056] S1. dissolving tetraethylammonium hydroxide and sodium chloride in water to obtain solution A;

[0057] S2. To the solution A obtained in step S1, an aluminum source, a silicon source and a mesoporous template agent, namely, hexadecyltrimethylammonium bromide, are sequentially added, and the gel B is obtained after aging;

[0058] S3. The gel B obtained in step S2 is crystallized and calcined to obtain a Beta molecular sieve catalyst;

[0059] In step S1, the molar ratio of tetraethylammonium hydroxide to sodium chloride is 5:0.273;

[0060] In step S2, the molar ratio of the silicon source, the aluminum source and tetraethylammonium hydroxide is 100:5.2:55;

[0061] In step S2, the molar ratio of the mesoporous template agent to the silicon source is 1.95:50.

[0062] Example 2

[0063] A Beta molecular sieve catalyst, wherein the molecular sieve pore framework of the Beta molecular sieve catalyst The total concentration of acid sites is 0.082mmol / g, of which the molecular sieve a-axis and b-axis pore skeleton The total concentration of acid sites accounts for the molecular sieve pore framework of Beta molecular sieve catalyst. 59% of the total concentration of acidic sites.

[0064] The preparation method of the Beta molecular sieve catalyst in the above-mentioned Example 2 is different from that in Example 1 in that:

[0065] The molar ratio of tetraethylammonium hydroxide to sodium chloride in step S1 is 5:0.091.

[0066] Example 3

[0067] A Beta molecular sieve catalyst, wherein the molecular sieve pore framework of the Beta molecular sieve catalyst The total concentration of acid sites is 0.101mmol / g, among which the molecular sieve a-axis and b-axis pore skeleton The total concentration of acid sites accounts for the molecular sieve pore framework of Beta molecular sieve catalyst. 99% of the total concentration of acid sites.

[0068] The preparation method of the Beta molecular sieve catalyst in the above-mentioned embodiment 3 is different from that in embodiment 1 in that:

[0069] The molar ratio of tetraethylammonium hydroxide to sodium chloride in step S1 is 5:0, that is, no sodium source is added in step S1.

[0070] Comparative Example 1

[0071] A Beta molecular sieve catalyst, wherein the molecular sieve pore framework of the Beta molecular sieve catalyst The total concentration of acid sites is 0.088mmol / g, of which the molecular sieve a-axis and b-axis pore skeleton The total concentration of acid sites accounts for the molecular sieve pore framework of Beta molecular sieve catalyst. 41% of the total concentration of acidic sites.

[0072] The preparation method of the Beta molecular sieve catalyst in the above comparative example 1 is different from that in Example 1 in that:

[0073] The molar ratio of tetraethylammonium hydroxide to sodium chloride in step S1 is 5:0.545.

[0074] Performance Testing

[0075] X-ray diffraction test: The Beta molecular sieve catalyst prepared in the example was characterized using a D8 Advance X-ray diffractometer from Bruker, Germany.

[0076] The distribution of acid sites in the molecular sieve pore framework was tested by using pyridine and 2,4,6-trimethylpyridine as probe molecules. The distribution of acidic sites in different pore skeletons of molecular sieves. First, take about 20 mg of the Beta molecular sieve catalyst prepared in the embodiment and the comparative example and press it into a thin sheet, then place it in an adsorption cell and evacuate it, and then dry it at 400°C for 2.5 hours. After cooling to room temperature, turn on the adsorption switch to adsorb pyridine or 2,4,6-trimethylpyridine for 0.5 hours. After turning off the adsorption switch, remove the probe molecules adsorbed on the catalyst surface at a high temperature of 150°C to ensure that the remaining probe molecules are adsorbed inside the molecular sieve pores. After the adsorption cell is cooled to room temperature, data is collected by an infrared spectrometer. According to the results of infrared data collection, the catalyst is calculated by the Lambert-Beer law. Acid concentration, calculated as follows:

[0077]

[0078] In the infrared spectrum using pyridine as the probe molecule, the three axes a, b, and c of Beta molecular sieve can be determined. Acidic sites, with a characteristic peak at ~1545cm -1 The corresponding molar extinction coefficient is 2.22cm / μmol. In the infrared spectrum with 2,4,6-trimethylpyridine as the probe molecule, the a and b axes of Beta molecular sieve can be determined. Acidic sites, with a characteristic peak at ~1636cm -1 , the corresponding molar extinction coefficient is 10.1 cm / μmol.

[0079] Beta molecular sieve catalytic performance test: The catalysts obtained in the examples and comparative examples were granulated, passed through a 20-30 mesh sieve, and about 0.43 g of the sample was put into an oven and activated at 120°C for 12 hours in an air atmosphere. Benzene and cyclohexene were prepared into a reaction solution at a molar ratio of 20:1, and a certain amount of n-decane was added as an internal standard. The flow rate of the reaction solution was adjusted to a mass space velocity of 12 h. -1 , react at normal pressure, take a certain amount of reaction liquid as sample after a certain reaction time, determine the content of cyclohexylbenzene and cyclohexene therein, and calculate the selectivity of the catalyst for the target reaction and the conversion rate of the reactant cyclohexene.

[0080] Nitrogen adsorption-desorption isotherm test: The Beta molecular sieve catalyst provided in Example 3 was collected using the ASAP 2460 multi-station fully automatic specific surface area and pore size analyzer produced by McMurray, USA.

[0081] The specific performance test data are as follows Tables 1 to 3. Figures 1 to 4 As shown:

[0082] Table 1. Examples and Comparative Examples Concentration and proportion of acidic sites

[0083]

[0084] Table 2. Conversion rate of molecular sieve to cyclohexene in the examples and comparative examples

[0085]

[0086] Table 3. Selectivity of molecular sieves for target reactions in examples and comparative examples

[0087]

[0088]

[0089] It can be seen from Table 1 that from Example 1 to Example 3, as the sodium ion content decreases, the pores in the a-axis and b-axis directions of the Beta molecular sieve catalyst provided by the present invention are The concentration of acid sites is increasing. The proportion of acidic sites in the concentration is increasing, indicating that the TEA in the Beta molecular sieve synthesis system can be controlled + and Na + ratio to achieve precise control [AlO4] - The distribution of species in different three-dimensional channels of Beta molecular sieve, thereby controlling The distribution of acidic sites in three different pore channels of Beta molecular sieve a-axis, b-axis and c-axis.

[0090] It can be seen from Tables 2 and 3 that the mass space velocity of the reactant flowing into the system is higher than 2h -1 Under the conditions of , the Beta molecular sieve catalyst provided in Example 3 of the present invention exhibits a maximum cyclohexene conversion rate of 21%, a target reaction selectivity of 70% and a longest service life, which is mainly attributed to the The acidic sites are mainly distributed in the pores in the a-axis and b-axis directions, which increases the active centers in the pores in the a-axis and b-axis directions of the Beta molecular sieve ( On the other hand, it inhibits the adsorption of benzene in the c-axis pores of the Beta molecular sieve, increases the benzene-olefin ratio in the a-axis and b-axis pores of the Beta molecular sieve, inhibits the occurrence of olefin self-polymerization side reactions, improves the reaction selectivity, and prolongs the service life of the catalyst. At the same time, the cyclohexylbenzene selectivity of the Beta molecular sieve catalyst in the embodiment and the comparative example decreases with the extension of the reaction time. This is because the Beta molecular sieve The acid sites are gradually covered by carbon deposits caused by the self-polymerization of cyclohexene.

[0091] Figure 1 The X-ray diffraction patterns of the Beta molecular sieve catalysts prepared in the examples of the present invention and the comparative examples are shown in FIG. Figure 1 It can be seen that both the embodiments of the present invention and the comparative examples can effectively prepare Beta molecular sieve catalysts with good crystallinity.

[0092] Figure 2 The infrared spectra of the Beta molecular sieve catalysts prepared in the examples of the present invention and the comparative examples when 2,4,6-trimethylpyridine is used as the probe molecule are shown in FIG. Figure 3 The infrared spectra of the Beta molecular sieve catalyst prepared in the examples of the present invention and the comparative examples when pyridine is used as the probe molecule. Figure 2 and Figure 3 As can be seen from the figure, as the sodium ion content decreases, it can be adsorbed in the pores of the molecular sieve in the a-axis and b-axis directions. The characteristic absorption peak of 2,4,6-trimethylpyridine at the acidic site (~1636 cm -1 ) strength continues to rise, indicating that the molecular sieve a-axis and b-axis channels The total concentration of acid sites is increasing; at the same time, it can be adsorbed in the pores of the molecular sieve in the three axial directions of a, b, and c. The characteristic absorption peak intensity of pyridine at the acidic site (~1545cm -1 ) remains basically unchanged. According to the Lambert-Beer law, the pore size in the a-axis and b-axis directions of the molecular sieve can be calculated. The proportion of acidic sites to all sites is increasing.

[0093] Figure 4 The target reaction selectivity and cyclohexene conversion rate change diagram of the alkylation reaction between benzene and cyclohexene catalyzed by the Beta molecular sieve catalyst prepared by the present invention. Figure 4 It can be seen that the Beta molecular sieve catalyst provided in Example 3 has a mass space velocity of 12h -1 Under the conditions, it showed the highest cyclohexene conversion of 21%, 70% target reaction selectivity and the longest service life.

[0094] Figure 5 This is the nitrogen adsorption and desorption isotherm diagram of the Beta molecular sieve catalyst prepared in Example 3 of the present invention. Figure 5 It can be seen that the nitrogen adsorption amount of the Beta molecular sieve of Example 3 increases sharply when the relative pressure is 0.85-0.99, indicating that the Beta molecular sieve of Example 3 has a rich mesoporous structure. When the nitrogen adsorption-desorption isotherm diagram is tested by the instrument, the testing instrument can calculate the total volume of micropores and mesopores in the Beta molecular sieve of Example 3 according to the nitrogen adsorption-desorption isotherm diagram. 3 g -1 and 0.257cm 3 g -1 This means that in the preparation method provided by the present invention, the addition of a mesoporous template in step S2 will induce the formation of mesopores in the Beta molecular sieve, and the multi-level pore structure in which micro-mesopores coexist can increase the specific surface area of ​​the Beta molecular sieve catalyst, increase the contact area between the Beta molecular sieve and the reactants, and then improve the catalytic performance of the catalyst.

[0095] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A Beta molecular sieve catalyst, It is characterized in that The molecular sieve channel framework of the Beta molecular sieve catalyst The total concentration of acid sites is 0.077-0.101 mmol / g, among which the molecular sieve a-axis and b-axis pore skeleton The total concentration of acid sites accounts for 49-99% of the total concentration of acidic sites.

2. The Beta molecular sieve catalyst as claimed in claim 1, It is characterized in that The Beta molecular sieve catalyst has a molecular sieve a-axis and b-axis pore framework. The total concentration of acid sites accounts for 59-99% of the total concentration of acidic sites.

3. A method for preparing the Beta molecular sieve catalyst according to any one of claims 1 to 2, It is characterized in that The specific steps include: S1. dissolving tetraethylammonium hydroxide in a solvent to obtain a solution A; S2. Adding an aluminum source and a silicon source to the solution A obtained in step S1 in sequence, and aging to obtain a gel B; S3. The gel B obtained in step S2 is crystallized and calcined to obtain a Beta molecular sieve catalyst; In step S2, the molar ratio of the silicon source, the aluminum source and tetraethylammonium hydroxide is 100:(3-7):(40-70); the silicon source is fumed silica, and the aluminum source is aluminum isopropoxide.

4. The method for preparing the Beta molecular sieve catalyst according to claim 3, It is characterized in that In the step S1, a sodium source needs to be added; the molar ratio of the tetraethylammonium hydroxide to the sodium source is 5:(0-0.273); the sodium source is one or more of sodium chloride, sodium bromide, sodium sulfate and sodium thiocyanate.

5. The method for preparing the Beta molecular sieve catalyst according to claim 3, It is characterized in that In the step S2, the molar ratio of the silicon source, the aluminum source and tetraethylammonium hydroxide is 100:(4-6):(50-60).

6. The method for preparing the Beta molecular sieve catalyst according to claim 3, It is characterized in that In the step S2, a mesoporous template agent needs to be added to the solution A obtained in the step S1.

7. The method for preparing the Beta molecular sieve catalyst according to claim 6, It is characterized in that The molar ratio of the mesoporous template added in step S2 to the silicon source is (1-3):

50.

8. A method for preparing cyclohexylbenzene by catalyzing the alkylation reaction between benzene and cyclohexene, It is characterized in that The specific steps include: Benzene and cyclohexene are mixed to obtain a reaction liquid, and the reaction liquid is introduced into a reactor containing the Beta molecular sieve catalyst according to any one of claims 1 to 2 to carry out a reaction.

9. A method for preparing cyclohexylbenzene by catalyzing the alkylation reaction between benzene and cyclohexene as claimed in claim 8, It is characterized in that The molar ratio of benzene to cyclohexene in the reaction solution is (10-30):

1.