A kind of formaldehyde-free color fixing agent and preparation method thereof

By designing a formaldehyde-free color-fixing agent formula composed of monomers, cross-linking agents, initiators and deionized water, the problems of high cost and complex process of existing formaldehyde-free color-fixing agents are solved, and a low-cost, safe solution is achieved. The color-fixing effect improves the utilization rate and color-fixing performance of diallylamine.

CN116463868BActive Publication Date: 2024-10-01NINGBO AOXIANG FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310375602.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-01
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

Existing formaldehyde-free color-fixing agents are expensive, have complex production processes and safety hazards, and have poor color-fixing effects. In particular, color-fixing agents obtained by copolymerizing diallylamine and dimethyldiallylammonium chloride are High temperatures can easily cause diallylamine to volatilize and cause excessive viscosity, affecting dispersion.

Method used

Use a formaldehyde-free fixative formula composed of monomers, cross-linking agents, initiators and deionized water. The monomer is a high-concentration dimethyldiallylammonium chloride aqueous solution. The reaction is adjusted by controlling the pH and temperature. Conditions, reduce the volatilization and viscosity of diallylamine, improve its utilization, and form a thin film on the fabric through the network structure of the copolymer to fix the color.

Benefits of technology

A low-cost, safe and easy-to-prepare formaldehyde-free color fixing agent is realized, which improves the utilization rate of diallylamine, reduces energy consumption and motor load, significantly improves the color-fixing effect, reduces production costs and reduces safety issues. Hidden danger.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004170311740000061
    Figure BDA0004170311740000061
  • Figure BDA0004170311740000071
    Figure BDA0004170311740000071
Patent Text Reader

Abstract

The present application discloses a formaldehyde-free color fixing agent and a preparation method thereof, and relates to the technical field of color fixing agents; the formaldehyde-free color fixing agent of the present application is made of the following components in parts by weight: 130-140 parts of monomer; 8-11 parts of cross-linking agent; 4-5.5 parts of initiator: 290-300 parts of deionized water; wherein the monomer is a dimethyldiallyl ammonium chloride aqueous solution with a mass percentage concentration of 60% or more. The present application is that the nucleophilic group NH contained in the polydimethyldiallyl ammonium chloride polymer can be covalently bonded with the active chlorine in the active dye molecule, reducing the water solubility of the dye, and the copolymer is strongly cationic, and is ionically bonded with anions to form a color lake, and the network structure formed by the long chain structure can form a film on the surface of the fabric to coat the dye molecules to prevent the loss of the dye molecules, thereby achieving a color fixing effect, and under the action of an equal amount of diallylamine, the utilization rate of diallylamine is improved, saving costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of color-fixing agents, and in particular to a formaldehyde-free color-fixing agent and its preparation method. Background Technology

[0002] Currently, color-fixing agents are one of the important auxiliaries in the printing and dyeing industry. They form insoluble colored substances with dyes on fabrics, thereby improving the color fastness to washing and perspiration. There are many types of color-fixing agents on the market, most of which contain formaldehyde, and their color-fixing effect is not ideal. With the development of science and technology, the improvement of people's living standards and environmental awareness, and the successive improvement of laws and regulations, the development of formaldehyde-free color-fixing agents meets people's needs.

[0003] Diallylamine is one of the important raw materials for the industrial production of formaldehyde-free fixing agents. However, there are few domestic manufacturers and only a few manufacturers abroad that produce it, and the output is difficult to meet market demand.

[0004] Currently, formaldehyde-free fixing agents obtained by copolymerizing diallylamine and dimethyl diallyl ammonium chloride are expensive. Furthermore, the high temperature during preparation can easily lead to the following issues: the volatilization of toxic substances from diallylamine, posing a safety hazard; excessive viscosity, resulting in excessive motor load and high energy consumption; and impaired copolymer dispersibility, leading to poor fixing effect. Summary of the Invention

[0005] In order to solve at least one of the above-mentioned technical problems and to develop an environmentally friendly, low-cost, and effective formaldehyde-free color-fixing agent, this application provides a formaldehyde-free color-fixing agent and its preparation method.

[0006] On the one hand, the formaldehyde-free fixing agent provided in this application is made of the following components in parts by weight: 130-140 parts of monomer; 8-11 parts of crosslinking agent; 4-5.5 parts of initiator; and 290-300 parts of deionized water; wherein the monomer is an aqueous solution of dimethyl diallyl ammonium chloride with a mass percentage concentration of 60% or more.

[0007] By adopting the above technical solution, the formaldehyde-free fixing agent designed in this application has the advantage that the nucleophilic group -NH- contained in the polydimethyl diallyl ammonium chloride polymer can form a covalent bond with the active chlorine in the reactive dye molecule, thereby reducing the water solubility of the dye. In addition, the copolymer has strong cationicity, which can combine with anions by ionic bonds to form a lake. Furthermore, the network structure formed by the long chain structure can form a thin film on the fabric surface to coat the dye molecules and prevent the dye molecules from being lost, thereby achieving the color fixing effect. Moreover, with this formula, the monomer conversion rate is maximized under the action of an equal amount of diallylamine, which greatly improves the utilization rate of diallylamine and saves the cost of producing formaldehyde-free fixing agents.

[0008] Optionally, the crosslinking agent is diallylamine.

[0009] Optionally, the initiator is a sodium persulfate solution with a mass percentage concentration of 15%.

[0010] Secondly, this application provides a method for preparing the above-mentioned formaldehyde-free fixing agent, comprising the following steps:

[0011] S1: Add deionized water to the reactor, along with crosslinking agent and 30-50 wt% monomer, and stir to react;

[0012] S2: Add hydrochloric acid dropwise to the reaction vessel to adjust the pH;

[0013] S3: Increase the temperature and add 30-50 wt% initiator dropwise while stirring. After increasing the temperature, maintain the temperature of the reactor and continue the reaction.

[0014] S4: Keep the temperature inside the reactor constant, add the remaining initiator and monomer dropwise into the reactor, and continue the reaction while maintaining the temperature after the dropwise addition is complete;

[0015] S5: Cool down, add liquid alkali to adjust pH and sugar content, and obtain the target product.

[0016] By adopting the above technical solution, the overall preparation process of the formaldehyde-free color-fixing agent is simple, easy to prepare, has mild process conditions, and achieves the best color-fixing effect.

[0017] Optionally, the hydrochloric acid in S2 has a mass percentage concentration of 37%; the liquid alkali in S5 is an aqueous sodium hydroxide solution with a mass percentage concentration of 48-51%.

[0018] By adopting the above technical solution and using specific concentrations of hydrochloric acid and liquid alkali, a suitable acid-base environment for the copolymerization of monomers and crosslinking agents is created under the neutralization effect of the two. This can efficiently adjust the pH of the product, which is beneficial to the reaction.

[0019] Optionally, in step S2, hydrochloric acid is added dropwise until the pH value in the reaction vessel is 2.0-3.0; the dropwise addition time is 1-1.5 hours.

[0020] By adopting the above technical solution, the dripping rate of hydrochloric acid is controlled, the exothermic reaction is controlled, the volatilization of diallylamine toxic substances is avoided, and poisoning is prevented. At the same time, the hazards caused by material overflow or equipment pressure buildup due to unsealed equipment or lack of pressure relief devices are also avoided.

[0021] Optionally, in step S3, the initiator is added dropwise after the temperature is raised to 40°C.

[0022] By adopting the above technical solution, when heated to 40°C, the exothermic reaction mechanism is controlled by adding an initiator, thereby reaching the reaction temperature of this reaction, saving production costs and reducing energy consumption.

[0023] Optionally, in step S3, after adding the initiator, the temperature inside the reactor is raised to 65-75°C and maintained at 65-75°C to continue the reaction.

[0024] Optionally, in step S4, the monomer and the initiator are added dropwise simultaneously, with the monomer being added over a time of 3-4 hours; the initiator being added over a time of 10-15 minutes longer than the monomer addition time, and the incubation time being 2 hours.

[0025] By adopting the above scheme, controlling the dropping rate of monomers and initiators, and controlling the exothermic reaction, the product can be kept in a good viscosity range and the color-fixing effect can be optimized.

[0026] Optionally, in step S5, the temperature is lowered to 40-50℃, the pH value is adjusted to 4.0-6.0, and the sugar content is adjusted to 42.0-43.0.

[0027] The environment is adjusted to be acidic. Under this environment, the amines in this product exist as cationic ammonium salts, and the long molecular chains are densely covered with positively charged amine or ammonium ions. The neutral dye ionizes in the aqueous solution, causing the dye matrix to become negatively charged. The interaction between the two forms an insoluble solid precipitate that is deposited on the fabric surface, preventing the loss of dye molecules.

[0028] In summary, the present invention has at least one of the following beneficial technical effects:

[0029] 1. The formaldehyde-free fixing agent of this application improves the utilization rate of diallylamine, saves the raw material cost of producing formaldehyde-free fixing agents, and has a good fixing effect;

[0030] 2. The formaldehyde-free fixing agent of this application has a simple preparation process. By controlling the addition of crosslinking agent and initiator, the exothermic reaction is controlled, thereby controlling the reaction temperature, reducing energy consumption, ensuring the viscosity range of the fixing agent, reducing the motor load, and saving the production cost of the formaldehyde-free fixing agent.

[0031] 3. The formaldehyde-free color-fixing agent of this application has a safe production process and reduces safety hazards. Detailed Implementation

[0032] The present application will be further described in detail below with reference to the embodiments.

[0033] This application designs a formaldehyde-free fixing agent, which is made of the following components in parts by weight: 130-140 parts of monomer; 8-11 parts of crosslinking agent; 4-5.5 parts of initiator; and 290-300 parts of deionized water; wherein the monomer is an aqueous solution of dimethyl diallyl ammonium chloride with a mass percentage concentration of 60% or more.

[0034] Prior to this application, existing color-fixing agents were mainly divided into cationic color-fixing agents and resin-based color-fixing agents. Most resin-based color-fixing agents contained formaldehyde, which did not comply with current laws and the concept of green and environmentally friendly products. Therefore, the development of formaldehyde-free color-fixing agents was pursued. Diallylamine, as one of the important raw materials for formaldehyde-free color-fixing agents, suffers from high costs due to the limited number of manufacturers, insufficient production volume to meet market demand.

[0035] The inventors of this application discovered in experiments that by selecting a specific formulation, the monomer conversion rate can be optimized and the utilization rate of diallylamine can be maximized, greatly saving raw material costs, and the produced formaldehyde-free fixing agent has excellent fixing performance. Based on the above findings, the inventors of this application designed the formaldehyde-free fixing agent of this application.

[0036] The formaldehyde-free fixing agent of this application is prepared by the following method, including the following steps:

[0037] S1: Add deionized water to the reactor, along with crosslinking agent and 30-50 wt% monomer, and stir to react;

[0038] S2: Add hydrochloric acid dropwise to the reaction vessel to adjust the pH;

[0039] S3: Increase the temperature and add 30-50 wt% initiator dropwise while stirring. After increasing the temperature, maintain the temperature of the reactor and continue the reaction.

[0040] S4: Keep the temperature inside the reactor constant, add the remaining initiator and monomer dropwise into the reactor, and continue the reaction while maintaining the temperature after the dropwise addition is complete;

[0041] S5: Cool down, add liquid alkali to adjust pH and sugar content, and obtain the target product.

[0042] Unless otherwise specified, all components involved in the formulation of this application are purchased from commercially available products.

[0043] Dimethyl diallyl ammonium chloride: purchased from Hubei Dongcao Chemical Technology Co., Ltd., with a purity of not less than 99%;

[0044] Diallylamine: Purchased from Zouping Mingxing Chemical Co., Ltd., with a purity of not less than 99%;

[0045] Sodium persulfate: purchased from Jinan Jinhao Chemical Co., Ltd., with a purity of not less than 99%;

[0046] Hydrochloric acid: purchased from Sinopharm Reagent Network, brand name: Hushi, concentration: 37%; Specific Implementation

[0048] Example 1

[0049] Add 29.5 kg of deionized water to the reactor, along with 0.8 kg of diallylamine and 3.9 kg of a 60% (w / w) dimethyl diallyl ammonium chloride aqueous solution, and stir to react. Within 1 hour, add hydrochloric acid dropwise to the reactor to adjust the pH to 2. Raise the temperature inside the reactor to 40°C, and while stirring, add 0.225 kg of sodium persulfate aqueous solution (15% (w / w)) dropwise, and raise the temperature to 65°C. Maintain the reactor temperature to continue the reaction.

[0050] While keeping the temperature inside the reactor constant, simultaneously add 0.225 kg of sodium persulfate aqueous solution (15% by mass) and 9.1 kg of dimethyl diallyl ammonium chloride aqueous solution (60% by mass) dropwise into the reactor. The addition time of the dimethyl diallyl ammonium chloride aqueous solution is 3 hours, and the addition time of the sodium persulfate aqueous solution is 10 minutes longer than that of the dimethyl diallyl ammonium chloride aqueous solution. After the addition is complete, maintain the temperature and continue the reaction for 2 hours.

[0051] Cool to 40℃, add 48% sodium hydroxide aqueous solution to adjust pH to 4, adjust sugar content to 42, and obtain aldehyde-free fixing agent.

[0052] Example 2

[0053] Add 30 kg of deionized water to the reactor, along with 0.9 kg of diallylamine and 5.28 kg of a 65% (w / w) dimethyl diallyl ammonium chloride aqueous solution, and stir to react. Over 1.2 h, add hydrochloric acid dropwise to the reactor to adjust the pH to 2.2. Raise the temperature inside the reactor to 40°C, and while stirring, add 0.165 kg of sodium persulfate aqueous solution (15% (w / w)) dropwise, and raise the temperature to 67°C. Maintain the reactor temperature to continue the reaction.

[0054] While maintaining a constant temperature inside the reactor, simultaneously add 0.385 kg of sodium persulfate aqueous solution (15% by mass) and 7.92 kg of dimethyl diallyl ammonium chloride aqueous solution (65% by mass) dropwise into the reactor. The addition time of the dimethyl diallyl ammonium chloride aqueous solution is 3.5 h, and the addition time of the sodium persulfate aqueous solution is 12 min longer than that of the dimethyl diallyl ammonium chloride aqueous solution. After the addition is complete, maintain the temperature and continue the reaction for 2 h.

[0055] Cool to 45°C, add 49% sodium hydroxide aqueous solution to adjust pH to 5, adjust sugar content to 42, and obtain aldehyde-free fixing agent.

[0056] Example 3

[0057] Add 29 kg of deionized water to the reactor, along with 1 kg of diallylamine and 6.7 kg of a 70% (w / w) dimethyl diallyl ammonium chloride aqueous solution, and stir to react. Over 1.3 h, add hydrochloric acid dropwise to the reactor to adjust the pH to 2.4. Raise the temperature inside the reactor to 40°C, and while stirring, add 0.2 kg of sodium persulfate aqueous solution (15% (w / w)) dropwise, and raise the temperature to 69°C. Maintain the reactor temperature to continue the reaction.

[0058] While maintaining a constant temperature inside the reactor, simultaneously add 0.3 kg of sodium persulfate aqueous solution (15% by mass) and 6.7 kg of dimethyl diallyl ammonium chloride aqueous solution (70% by mass) dropwise into the reactor. The addition time of the dimethyl diallyl ammonium chloride aqueous solution is 3.7 h, and the addition time of the sodium persulfate aqueous solution is 13 min longer than that of the dimethyl diallyl ammonium chloride aqueous solution. After the addition is complete, maintain the temperature and continue the reaction for 2 h.

[0059] The temperature was lowered to 47°C, and a 50% sodium hydroxide aqueous solution was added to adjust the pH to 5.2 and the sugar content to 42 to obtain an aldehyde-free fixing agent.

[0060] Example 4

[0061] Add 29.5 kg of deionized water to the reactor, along with 1.1 kg of diallylamine and 5.44 kg of a 75% (w / w) dimethyl diallyl ammonium chloride aqueous solution, and stir to react. Over 1.5 h, add hydrochloric acid dropwise to the reactor to adjust the pH to 2.5. Raise the temperature inside the reactor to 40°C, and while stirring, add 0.2 kg of sodium persulfate aqueous solution (15% (w / w)) dropwise, and raise the temperature to 72°C. Maintain the reactor temperature to continue the reaction.

[0062] While maintaining a constant temperature inside the reactor, simultaneously add 0.2 kg of sodium persulfate aqueous solution (15% by mass) and 8.16 kg of dimethyl diallyl ammonium chloride aqueous solution (75% by mass) dropwise into the reactor. The addition time of the dimethyl diallyl ammonium chloride aqueous solution is 3.9 h, and the addition time of the sodium persulfate aqueous solution is 15 min longer than that of the dimethyl diallyl ammonium chloride aqueous solution. After the addition is complete, maintain the temperature and continue the reaction for 2 h.

[0063] Cool to 50℃, add 51% sodium hydroxide aqueous solution to adjust pH to 5.5, adjust sugar content to 43, and obtain aldehyde-free fixing agent.

[0064] Example 5

[0065] Add 30 kg of deionized water to the reactor, along with 0.8 kg of diallylamine and 4.14 kg of 80% dimethyl diallyl ammonium chloride aqueous solution, and stir to react. Over 1.2 h, add hydrochloric acid dropwise to the reactor to adjust the pH to 2.7. Raise the temperature inside the reactor to 40°C, and while stirring, add 0.2 kg of sodium persulfate aqueous solution (15% concentration), and raise the temperature to 75°C. Maintain the reactor temperature to continue the reaction.

[0066] While maintaining a constant temperature inside the reactor, simultaneously add 0.3 kg of sodium persulfate aqueous solution (15% by mass) and 9.66 kg of dimethyl diallyl ammonium chloride aqueous solution (80% by mass) dropwise into the reactor. The addition time of the dimethyl diallyl ammonium chloride aqueous solution is 4 hours, and the addition time of the sodium persulfate aqueous solution is 12 minutes longer than that of the dimethyl diallyl ammonium chloride aqueous solution. After the addition is complete, maintain the temperature and continue the reaction for 2 hours.

[0067] The temperature was lowered to 45°C, and a 49% sodium hydroxide aqueous solution was added to adjust the pH to 5.8 and the sugar content to 43, thus obtaining a formaldehyde-free fixing agent.

[0068] Example 6

[0069] Add 29 kg of deionized water to the reactor, along with 1 kg of diallylamine and 7 kg of 85% dimethyl diallyl ammonium chloride aqueous solution, and stir to react. Within 1 hour, add hydrochloric acid dropwise to the reactor to adjust the pH to 3. Raise the temperature inside the reactor to 40°C, and while stirring, add 0.12 kg of sodium persulfate aqueous solution (15% concentration), and raise the temperature to 73°C. Maintain the reactor temperature to continue the reaction.

[0070] While keeping the temperature inside the reactor constant, simultaneously add 0.28 kg of sodium persulfate aqueous solution (15% by mass) and 7 kg of dimethyl diallyl ammonium chloride aqueous solution (85% by mass) dropwise into the reactor. The dropwise addition time of the dimethyl diallyl ammonium chloride aqueous solution is 3.8 h, and the dropwise addition time of the sodium persulfate aqueous solution is 15 min longer than that of the dimethyl diallyl ammonium chloride aqueous solution. After the addition is complete, maintain the temperature and continue the reaction for 2 h.

[0071] Cool to 50℃, add 50% sodium hydroxide aqueous solution to adjust pH to 6, adjust sugar content to 42, and obtain aldehyde-free fixing agent.

[0072] Comparative Example 1

[0073] This comparative example uses T-21 formaldehyde-free fixing agent from Ningbo Aoxiang Fine Chemical Co., Ltd.

[0074] Comparative Example 2

[0075] This comparative example uses the color-fixing agent (RD) from Xinrunde Chemical.

[0076] Comparative Example 3

[0077] This comparative example uses Hengchang Chemical's fixing agent (26062-79-3).

[0078] Performance tests were conducted on Examples 1-6 and Comparative Examples 1-3. The experimental fabric was 100% cotton knitted fabric (bright red). The experimental process was 40℃ × 20°C.

[0079] The test method for fastness to rubbing was determined according to GB / T3920-2008 "Textiles - Tests for color fastness - Fastness to rubbing".

[0080] The test method for color fastness to washing was performed in accordance with GB / T3921-2008 "Textiles - Tests for color fastness - Color fastness to washing".

[0081] The experimental results are shown in Table 1:

[0082] Table 1. Performance test results of Examples 1-6 and Comparative Examples 1-3

[0083]

[0084]

[0085] As can be seen from Examples 1-6, Comparative Examples 1-3, and Table 1, the formaldehyde-free fixing agent prepared by the formulation of this application, when applied to woven fabric, results in a dry friction grade, a wet friction grade, and a staining grade that are no lower than those of the prior art. As can be seen from Examples 1 / 3 / 5, the amount of formaldehyde-free fixing agent prepared by the formulation of this application is 0.4 g / L, which is lower than the amount of 0.5 g / L in Comparative Example 1, but the effect is no lower than that of Comparative Example 1 and better than that of Comparative Examples 2-3. Therefore, it can be seen that the formaldehyde-free fixing agent prepared by the formulation of this application has high efficiency and good fixing effect.

[0086] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A formaldehyde-free color fixing agent, characterized in that: It is made of the following components in parts by weight: 130-140 parts of monomer; 8-11 parts of cross-linking agent; 4-5.5 parts of initiator; 290-300 parts of deionized water; wherein the monomer is a dimethyldiallylammonium chloride aqueous solution with a mass percentage concentration of 60% or more; the cross-linking agent is diallylamine; The preparation method of the formaldehyde-free color fixing agent comprises the following steps: S1: Add deionized water, a crosslinking agent and 30-50 wt% of a monomer into a reaction kettle, and stir to react; S2: Add hydrochloric acid dropwise into the reactor to adjust the pH; S3: After the temperature is raised to 40°C, 30-50 wt% of initiator is added dropwise under stirring, the temperature in the reactor is raised to 65-75°C, and the temperature of the reactor is maintained at 65-75°C to continue the reaction; S4: Keep the temperature in the reactor unchanged, add the remaining initiator and monomer to the reactor, and keep the temperature to continue the reaction after the addition is complete; S5: cooling, adding liquid alkali to adjust pH and sugar content, and obtaining the target product; Wherein, the initiator is a sodium persulfate solution with a mass percentage concentration of 15%; The mass percentage concentration of the hydrochloric acid in S2 is 37%; the liquid alkali in S5 is a sodium hydroxide aqueous solution with a mass percentage concentration of 48-51%.

2. The formaldehyde-free color fixing agent according to claim 1, characterized in that: In the step S2, hydrochloric acid is added dropwise until the pH value in the reaction kettle reaches 2.0-3.0; the adding time is 1-1.5 hours.

3. The formaldehyde-free color fixing agent according to claim 1, characterized in that: In the S4, the monomer and the initiator are added dropwise at the same time, and the monomer addition time is 3-4 hours; the initiator addition time is extended by 10-15 minutes based on the monomer addition time, and the insulation time is 2 hours.

4. The formaldehyde-free color fixing agent according to claim 1, characterized in that: In S5, the temperature is lowered to 40-50°C, the pH value is adjusted to 4.0-6.0, and the sugar content is adjusted to 42.0-43.0.