A method for preparing hot-rolled steel plates

By optimizing the preparation process of hot-rolled steel plates and controlling the heating temperature, rolling temperature, and cooling regime, the problem of poor quality of iron oxide scale on the surface of hot-rolled steel plates was solved, and high-quality iron oxide scale suitable for water-based paint descaling was achieved.

CN116493410BActive Publication Date: 2026-11-17SHOUGANG GROUP CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310473511.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2026-11-17
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

The quality of iron oxide scale on the surface of existing hot-rolled steel plates is poor, which cannot meet the needs of downstream users for water-based paint that eliminates scale.

Method used

By controlling the slab heating temperature, rolling temperature, and cooling regime, and optimizing the chemical composition, hot-rolled steel plates with appropriate iron oxide scale thickness, impedance value, and Fe3O4 and FeO content are prepared, ensuring that the quality of the surface iron oxide scale meets the requirements for water-based paint descaling.

Benefits of technology

It achieves the density and uniformity of iron oxide scale on the surface of hot-rolled steel plates, improves the adhesion and anti-peeling ability of iron oxide scale, and meets the quality requirements of water-based paint descaling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116493410B_ABST
    Figure CN116493410B_ABST
Patent Text Reader

Abstract

This application relates to the field of steel rolling technology, and more particularly to a method for preparing hot-rolled steel plates. A method for preparing hot-rolled steel plates, characterized in that the steel plates are used for water-based paint descaling, the method comprising: heating a slab with a predetermined chemical composition to a predetermined temperature; performing a first rolling process on the heated slab to obtain an intermediate slab; wherein the thickness of the intermediate slab is controlled to a predetermined thickness; performing a finish rolling process on the intermediate slab under predetermined entry and final rolling temperatures for a second rolling process to obtain a strip steel; and performing staged cooling on the strip steel, followed by coiling, to obtain a hot-rolled steel plate. This application solves the technical problem of poor quality of iron oxide scale on the surface of existing hot-rolled steel plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of steel rolling technology, and more particularly to a method for preparing hot-rolled steel plates. Background Technology

[0002] In recent years, the country has intensified its environmental protection efforts, leading to changes in the processing and usage methods of downstream users of steel products. This has placed higher demands on the raw steel plates. Some downstream manufacturers have switched from oil-based paint to water-based paint for steel plate surface treatment, eliminating the descaling process and changing the painting process from the original pickled substrate state to painting with the iron scale on. This aims to eliminate acid and dust pollution caused by pickling or shot blasting of steel plates, as well as air pollution from oil-based paint spraying, while reducing the process costs of shot blasting or pickling. This change places higher demands on the quality of hot-rolled steel plates, especially the quality of the surface iron oxide scale. The surface quality of iron oxide scale and other components in proportionally produced hot-rolled steel plates is insufficient to meet these customer requirements. Therefore, there is an urgent need to develop new production methods that can enable downstream users to directly spray water-based paint on hot-rolled box plates without descaling. Summary of the Invention

[0003] This application provides a method for preparing hot-rolled steel plates to solve the technical problem of poor quality of iron oxide scale on the surface of existing hot-rolled steel plates.

[0004] In a first aspect, this application provides a method for preparing a hot-rolled steel plate, the steel plate being used for water-based paint descaling spraying, the method comprising:

[0005] A slab with a set chemical composition is heated to bring the slab to a set temperature;

[0006] The heated slab is subjected to a first rolling process to obtain an intermediate slab; wherein the thickness of the intermediate slab is controlled to a set thickness.

[0007] Under the conditions of setting the inlet temperature and the final rolling temperature of the second rolling, the intermediate billet is finished rolled to obtain strip steel;

[0008] The strip steel is cooled in stages and then coiled to obtain a hot-rolled steel plate.

[0009] Optionally, the surface iron oxide scale quality parameters of the hot-rolled steel plate include:

[0010] The thickness of the iron oxide scale, the impedance value of the iron oxide scale, the corrosion current density of the iron oxide scale, the Fe3O4 content in the iron oxide scale, and the FeO content in the iron oxide scale; wherein,

[0011] The thickness of the iron oxide scale is ≤10μm, and the impedance value of the iron oxide scale is ≥5×10. 4 Ω.cm2 The corrosion current density of iron oxide scale is ≤3.86×10⁻⁶. -7 A.cm -2 The Fe3O4 content in the iron oxide scale is ≥50% by weight and the FeO content in the iron oxide scale is ≥10% by weight.

[0012] Optionally, the set temperature is 1170℃-1210℃.

[0013] Optionally, the set thickness is 30mm-35mm.

[0014] Optionally, the inlet temperature of the second rolling process is set to 1000℃-1050℃.

[0015] Optionally, the final rolling temperature of the second rolling process is set to 810℃-830℃.

[0016] Optionally, the step of finishing-rolling the intermediate billet to obtain strip steel under the conditions of setting the inlet temperature and the final rolling temperature of the second rolling process includes:

[0017] Under the conditions of setting the inlet temperature and the final rolling temperature of the second rolling, and controlling the opening ratio of the cooling water between the finishing mill stands, the intermediate billet is finished rolled to obtain strip steel; wherein,

[0018] The cooling water operating rate is 30%-60%.

[0019] Optionally, the step of cooling the strip in stages and then coiling it to obtain a hot-rolled steel plate includes:

[0020] The strip steel is subjected to a three-stage cooling process: ultra-fast cooling, laminar flow cooling, and air cooling, and then coiled to obtain a hot-rolled steel sheet; wherein,

[0021] The ultra-fast cooling pressure is 0.3MPa-0.6MPa, and the laminar flow cooling adopts a sparse cooling mode.

[0022] Optionally, the winding temperature is 550℃-580℃.

[0023] Optionally, the specified chemical composition includes:

[0024] C, Si, Mn, P, S, Alt, Cr, Ti, Fe; among which,

[0025] The C content is 0.08 wt% to 0.12 wt%, the Si content is 0.08 wt% to 0.12 wt%, the Mn content is 1.4 wt% to 1.7 wt%, the P content is ≤0.03 wt%, the S content is ≤0.07 wt%, the Alt content is 0.01 wt% to 0.03 wt%, the Cr content is 0.1 wt% to 0.2 wt%, and the Ti content is 0.1 wt% to 0.15 wt%.

[0026] The technical solutions provided in this application have the following advantages compared with the prior art:

[0027] The hot-rolled steel plate preparation method provided in this application involves: rationally designing the chemical composition of the steel plate to control its mechanical and oxidation resistance; controlling the slab heating temperature to obtain an iron oxide scale of appropriate thickness; controlling the hot rolling temperature to ensure not only the mechanical properties of the strip but also the thickness, interface flatness, and structural organization of the iron oxide scale; designing the cooling regime to control the growth of the surface iron oxide scale; and controlling the coiling temperature to achieve an appropriate ratio of FeO and Fe3O4 in the iron oxide scale while maintaining the steel plate's performance. This steel plate is suitable for water-based paint descaling without descaling, and its surface iron oxide scale quality is excellent, ultimately solving the technical problem of poor surface iron oxide scale quality in existing hot-rolled steel plates. Attached Figure Description

[0028] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.

[0029] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0030] Figure 1 A schematic flowchart illustrating a method for preparing hot-rolled steel sheet according to an embodiment of this application;

[0031] Figure 2 This application provides a comparative example of the macroscopic surface morphology of a hot-rolled steel plate;

[0032] Figure 3 This application provides an embodiment of a macroscopic surface morphology of a hot-rolled steel plate;

[0033] Figure 4 This application provides a comparative example of the surface morphology of a hot-rolled steel sheet after bending;

[0034] Figure 5This application provides an embodiment of the surface morphology of a hot-rolled steel sheet after bending;

[0035] Figure 6 This application provides a comparative example of the microstructure of iron oxide scale on the surface of a hot-rolled steel plate;

[0036] Figure 7 This application provides an embodiment of the microstructure of iron oxide scale on the surface of a hot-rolled steel plate. Detailed Implementation

[0037] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0038] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0039] In this application, unless otherwise stated, directional terms such as "upper" and "lower" specifically refer to the drawing directions in the accompanying drawings. Furthermore, in the description of this application, terms such as "comprising" and "including" mean "including but not limited to." In this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships can exist; for example, A and / or B can represent: A alone, A and B simultaneously, or B alone. A and B can be singular or plural. In this document, "at least one" means one or more, and "more than one" means two or more. "At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be a single or multiple.

[0040] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0041] Firstly, this application provides a method for preparing hot-rolled steel plates; please refer to [link to relevant documentation]. Figure 1 The method includes:

[0042] S1. Heating a slab with a set chemical composition to bring the slab to a set temperature;

[0043] S2. The heated slab is subjected to a first rolling process to obtain an intermediate slab; wherein the thickness of the intermediate slab is controlled to a set thickness.

[0044] S3. Under the conditions of setting the inlet temperature and the final rolling temperature of the second rolling, the intermediate billet is finished rolled to obtain strip steel.

[0045] S4. The strip steel is cooled in stages and then coiled to obtain a hot-rolled steel plate.

[0046] In some embodiments, the surface iron oxide scale quality parameters of the hot-rolled steel sheet include:

[0047] The thickness of the iron oxide scale, the impedance value of the iron oxide scale, the corrosion current density of the iron oxide scale, the Fe3O4 content in the iron oxide scale, and the FeO content in the iron oxide scale; wherein, the thickness of the iron oxide scale is ≤10μm, and the impedance value of the iron oxide scale is ≥5×10 4 Ω.cm 2 The corrosion current density of iron oxide scale is ≤3.86×10⁻⁶. -7 A.cm -2 The Fe3O4 content in the iron oxide scale is ≥50% by weight and the FeO content in the iron oxide scale is ≥10% by weight.

[0048] The positive effects of controlling the thickness of the iron oxide scale to ≤10μm: A suitable iron oxide scale can protect the steel plate surface and prevent rust, while also maintaining good adhesion and preventing breakage and peeling. If the thickness is too high, it can lead to a decrease in the adhesion of the scale, making it more prone to breakage and peeling. Specifically, this thickness can be 10μm, 9μm, 8μm, 7μm, etc.

[0049] The impedance value of the iron oxide scale is controlled to be ≥5×10. 4 Ω.cm 2 Positive effects: Based on practical results, the impedance value can quantitatively reflect the quality of iron oxide scale. If the impedance value is too low, it indicates that the iron oxide scale is too porous and has poor resistance to peeling. Specifically, the impedance value can be 5 × 10⁻⁶. 4 Ω.cm 2 5.2×10 4 Ω.cm 2 5.4×10 4 Ω.cm 2 5.6×10 4 Ω.cm 2 5.8×10 4 Ω.cm 2 6×10 4 Ω.cm 2 wait.

[0050] The corrosion current density of the iron oxide scale is controlled to be ≤3.86×10⁻⁶. -7 A.cm -2 Positive effects: Based on practical results, the impedance value can quantitatively reflect the quality of iron oxide scale. If the corrosion current density is too high, it indicates that the iron oxide scale is too porous and has poor resistance to peeling. Specifically, the corrosion current density can be 3.86 × 10⁻⁶. -7 A.cm -2 3.85×10 -7 A.cm -2 3.84×10 -7 A.cm-2 3.83×10 -7 A.cm -2 3.82×10 -7 A.cm -2 wait.

[0051] The positive effects of controlling the Fe3O4 content in the iron oxide scale to ≥50% by weight are as follows: A suitable Fe3O4 content makes the iron oxide scale denser and harder. If the Fe3O4 content is too low, it will, to some extent, lead to a loose and porous iron oxide scale. Specifically, this content can be 50% by weight, 51% by weight, 52% by weight, 53% by weight, 54% by weight, 55% by weight, etc.

[0052] The positive effects of controlling the FeO content in the iron oxide scale to ≥10% by weight are: it has a buffering effect against external forces, and when combined with Fe3O4, it can improve the adhesion of the iron oxide scale. If the FeO content is too low, it can lead to the iron oxide scale easily peeling off in large pieces. Specifically, this content can be 10% by weight, 11% by weight, 12% by weight, 13% by weight, 14% by weight, 15% by weight, etc.

[0053] In some embodiments, the set temperature is 1170℃-1210℃.

[0054] "Set temperature" refers to the furnace exit temperature of the slab. Controlling this temperature to 1170℃-1210℃ has the following positive effects: During the slab heating process, austenite transformation and dissolution of precipitates occur internally, while a thicker iron oxide scale forms on the surface. This type of steel contains 0.1-0.2% Cr. Studies have found that Cr accumulates at the interface between the iron oxide scale and the matrix at high temperatures, hindering the diffusion of iron and oxygen atoms, thus thinning and densifying the iron oxide scale. However, as the temperature increases, the accumulation and presence of Cr changes from continuous lamellar to discontinuous granular, weakening its inhibitory effect on oxidation. Therefore, the mechanical properties and surface quality of the product must be considered comprehensively. If the temperature is too high, it may be difficult to completely remove the primary furnace scale; if the temperature is too low, Cr may not accumulate sufficiently, affecting the oxidation resistance. Specifically, this temperature can be 1170℃, 1180℃, 1190℃, 1200℃, 1210℃, etc. The furnace time is 150-180 minutes.

[0055] In some embodiments, the set thickness is 30mm-35mm.

[0056] "Set thickness" refers to the thickness of the intermediate billet. Controlling this thickness to 30mm-35mm has the following advantages: it balances finishing rolling speed and reduction, reduces finishing rolling oxidation time, and minimizes sheet breakage. If the thickness is too high, it can lead to excessive finishing rolling reduction, easily causing sheet breakage and indentation; if the thickness is too low, it can cause instability in the rolling process. Specifically, this thickness can be 30mm, 31mm, 32mm, 33mm, 34mm, 35mm, etc.

[0057] In some embodiments, the inlet temperature of the second rolling is set to 1000°C-1050°C.

[0058] By controlling appropriate slab heating parameters and combining them with conventional descaling processes (initial descaling, rough descaling, and fine descaling) on ​​the production line, the furnace-grown iron oxide scale and secondary iron oxide scale generated during rough rolling can be effectively removed. However, new iron oxide scale will still form on the strip surface after entering the finishing rolling zone. At this stage, there is no descaling equipment, and the growth of iron oxide scale can only be influenced by the finishing rolling inlet temperature, rolling speed, reduction, and interstand cooling water. The "second rolling" is finishing rolling. Controlling the finishing rolling inlet temperature to 1000℃-1050℃ has the following positive effects: it results in a relatively straight interface morphology between the iron oxide scale and the matrix, which is beneficial for obtaining a uniform and dense iron oxide scale structure. If the temperature is too high, it will lead to excessively rapid iron oxide scale growth in the finishing rolling zone; if the temperature is too low, it will lead to instability in the finishing rolling process. Specifically, the finishing rolling inlet temperature can be 1000℃, 1010℃, 1020℃, 1030℃, 1040℃, 1050℃, etc.

[0059] In some embodiments, the final rolling temperature of the second rolling process is set to 810°C-830°C.

[0060] The positive effects of controlling the final rolling temperature of 810℃-830℃ are: it can control the thickness of the iron oxide scale and the straightness of the interface while ensuring the mechanical properties of the strip. If the temperature is too high, it will lead to an increase in the thickness of the iron oxide scale to some extent; if the temperature is too low, it will lead to excessive mechanical properties to some extent. Specifically, the final rolling temperature can be 810℃, 820℃, 830℃, etc.

[0061] In some embodiments, the step of finishing-rolling the intermediate billet to obtain strip steel under the conditions of setting the entry temperature and the final rolling temperature of the second rolling process includes:

[0062] Under the conditions of setting the inlet temperature and the final rolling temperature of the second rolling, and controlling the opening ratio of the cooling water between the finishing mill stands, the intermediate billet is finished rolled to obtain strip steel; wherein,

[0063] The cooling water operating rate is 30%-60%.

[0064] The positive effects of turning on the cooling water between the first three sets of finishing mill stands and controlling the cooling water opening ratio to 30%-60% are: it allows the strip to pass through the oxidation temperature-sensitive range quickly; if the opening amount of the cooling water is too large, it will lead to a rapid temperature drop to some extent, which may affect the final rolling temperature; if the opening amount of the cooling water is too small, it may lead to excessively rapid iron oxide scale growth to some extent. Specifically, the opening ratio can be 30%, 40%, 50%, 60%, etc.

[0065] In some embodiments, the step of cooling the strip in stages and then coiling it to obtain a hot-rolled steel sheet includes:

[0066] The strip steel is subjected to a three-stage cooling process: ultra-fast cooling, laminar flow cooling, and air cooling, and then coiled to obtain a hot-rolled steel sheet.

[0067] The ultra-fast cooling pressure is 0.3MPa-0.6MPa, and the laminar flow cooling adopts a sparse cooling mode.

[0068] After exiting the finishing mill, the strip steel needs to pass through the cooling roller table, and then be coiled into coils by the coiler. The temperature of the strip steel on the cooling roller table is still as high as 800℃, which is still in the temperature range where oxidation is easy. At this time, a suitable cooling system needs to be adopted to achieve an appropriate coiling temperature while minimizing the thickening of the iron oxide scale on the surface of the strip steel.

[0069] The positive effects of the three-stage cooling process—ultra-rapid cooling, laminar flow cooling, and air cooling—on the strip steel include: effectively controlling the growth of iron oxide scale during this stage. The positive effects of the initial ultra-rapid cooling stage include: enabling the strip steel to quickly pass through the high-temperature zone, reducing the tendency for iron oxide scale growth; and the positive effects of controlling the ultra-rapid cooling pressure to 0.3MPa-0.6MPa include: ensuring a suitable cooling rate. If the pressure is too high, it may lead to poor strip shape to some extent; if the pressure is too low, it may lead to insufficient cooling effect to some extent. Specifically, the ultra-rapid cooling pressure can be 0.3MPa, 0.4MPa, 0.5MPa, 0.6MPa, etc.

[0070] The positive effects of laminar flow cooling in the mid-section sparse cooling mode are: it is beneficial to the water seal on the steel plate surface and the uniform temperature control of the upper and lower surfaces.

[0071] The positive effects of end-of-line air cooling: precise control of the consistency of subsequent winding temperature throughout the winding process.

[0072] In some embodiments, the winding temperature is 550°C-580°C.

[0073] The final process before hot-rolled coils come off the production line is the coiling machine coiling the strip steel into coils. After coiling, the hot-rolled coil cools down slowly, requiring several days to reach room temperature. Because the strip steel temperature is still high during coiling, the internal phase structure of the iron oxide scale on the strip steel surface undergoes a eutectoid transformation during storage, affecting the quality of the iron oxide scale in the final product. Controlling the coiling temperature to 550℃-580℃ has the positive effect of achieving an appropriate FeO and Fe3O4 ratio while maintaining performance. If the temperature is too high, it can lead to excessive FeO transformation and low FeO content; if the temperature is too low, it can inhibit the FeO eutectoid transformation and result in high FeO content. Specifically, the coiling temperature can be 550℃, 560℃, 570℃, 580℃, etc.

[0074] In some embodiments, the specified chemical composition includes: C, Si, Mn, P, S, Alt, Cr, Ti, and Fe; wherein,

[0075] The C content is 0.08 wt% to 0.12 wt%, the Si content is 0.08 wt% to 0.12 wt%, the Mn content is 1.4 wt% to 1.7 wt%, the P content is ≤0.03 wt%, the S content is ≤0.07 wt%, the Alt content is 0.01 wt% to 0.03 wt%, the Cr content is 0.1 wt% to 0.2 wt%, and the Ti content is 0.1 wt% to 0.15 wt%.

[0076] The positive effects of controlling the carbon content to 0.08% to 0.12% by weight include: ensuring appropriate yield strength, tensile strength, and plasticity of the steel; excessively high carbon content can lead to excessively high material strength, while excessively low carbon content can lead to excessively low material strength. Specifically, the carbon content can be 0.08% by weight, 0.09% by weight, 0.10% by weight, 0.11% by weight, 0.12% by weight, etc.

[0077] The positive effects of controlling the Si content to be between 0.08 wt% and 0.12 wt% include: improving the hardenability of austenite and enhancing the purity of ferrite; however, excessively high Si content can lead to surface red rust defects to some extent; and excessively low Si content can reduce material strength to some extent. Specifically, the Si content can be 0.08 wt%, 0.09 wt%, 0.10 wt%, 0.11 wt%, 0.12 wt%, etc.

[0078] The positive effects of controlling the Mn content to 1.4% to 1.7% by weight include: acting as a deoxidizer and desulfurizer during the steelmaking process, and improving the hot working properties of steel; if the Mn content is too high, the strength will be too high to some extent; if the Mn content is too low, the strength will be too low to some extent. Specifically, the Mn content can be 1.4% by weight, 1.5% by weight, 1.6% by weight, 1.7% by weight, etc.

[0079] The positive effects of controlling the phosphorus (P) content to ≤0.03 wt% include: improving the strength of steel through solid solution strengthening; however, if the P content is too high, it will increase the brittleness of the material to some extent. Specifically, the P content can be 0.03 wt%, 0.02 wt%, 0.015 wt%, 0.025 wt%, etc.

[0080] The positive effects of controlling the sulfur content to ≤0.07% by weight are that sulfur is a residual element and should be minimized; if the sulfur content is too high, it can lead to edge cracking to some extent. Specifically, the sulfur content can be 0.07% by weight, 0.065% by weight, 0.06% by weight, 0.055% by weight, etc.

[0081] The positive effects of controlling the Alt content to 0.01% to 0.03% by weight are: it is a commonly used deoxidizer in steel, refining the grain size; if the Alt content is too high, it can lead to steelmaking defects to some extent; if the Alt content is too low, it can coarsen the grain size to some extent. Specifically, the Alt content can be 0.01% by weight, 0.02% by weight, 0.03% by weight, etc.

[0082] The positive effects of controlling the Cr content to 0.1% to 0.2% by weight include improved mechanical properties and oxidation resistance of steel. However, excessively high Cr content can lead to excessively high strength and increased costs, while excessively low Cr content can negatively impact surface quality. Specifically, the Cr content can be 0.1% by weight, 0.15% by weight, 0.2% by weight, etc.

[0083] The positive effects of controlling the Ti content to 0.1% to 0.15% by weight include: making the steel microstructure denser, refining the grains, and improving strength; if the Ti content is too high, it will lead to excessively high material strength, increasing costs; if the Ti content is too low, it will lead to insufficient material strength. Specifically, the Ti content can be 0.1% by weight, 0.15% by weight, 0.14% by weight, 0.13% by weight, 0.12% by weight, 0.11% by weight, etc.

[0084] The present application is further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to national standards. If there is no corresponding national standard, then general international standards, conventional conditions, or conditions recommended by the manufacturer are followed.

[0085] Table 1 Chemical composition (wt%) of 7mm hot-rolled steel plate

[0086] Serial Number C Si Mn P S Alt Cr Ti Example 1 0.08 0.08 1.4 0.03 0.07 0.01 0.1 0.1 Example 2 0.12 0.12 1.7 0.025 0.065 0.03 0.2 0.15 Example 3 0.09 0.095 1.5 0.028 0.062 0.02 0.15 0.12 Comparative Example 1 0.09 0.095 1.5 0.028 0.062 0.02 0.3 0.12

[0087] Table 2. Manufacturing process parameters for 7mm hot-rolled steel plates

[0088]

[0089] Table 3. Oxide Scale Test of 7mm Hot-Rolled Steel Plate

[0090]

[0091] The surface quality of 7mm hot-rolled steel sheets after production under the two process modes of the example and comparative examples. The macroscopic morphology of the strip surface is shown below. Figure 2-3 As shown, the strip produced in the comparative example exhibits uneven coloring and peeling of black and gray residue on its surface. The steel plate produced using the process described in the example, however, has a uniform and bright surface, indicating good quality. Bending tests were conducted on the cut strips, and the macroscopic morphology of the bent areas is shown below. Figure 4-5 As shown in the figure, the steel plate produced in the comparative example exhibits significant iron oxide scale peeling at the bent sections. Image processing calculations indicate that the peeling area accounts for approximately 65%, suggesting poor adhesion between the iron oxide scale and the substrate, which is detrimental to downstream processing with the scale. In contrast, the steel plate produced using the process described in the example exhibits better iron oxide scale integrity at the bent sections, with peeling accounting for only about 15%, demonstrating a significantly improved adhesion. Scanning electron microscopy was used to observe the microstructure of the iron oxide scale under the two processes, as shown below. Figure 6-7 As shown, the iron oxide scale produced in the comparative example exhibits a large number of eutectoid structures and microcracks within its interior, making it prone to breakage during subsequent use. Furthermore, the interface between the iron oxide scale and the matrix shows a distinctly uneven morphology, resulting in inconsistent scale thickness. In contrast, the steel plate produced using the example process demonstrates good density and high interface flatness. Table 3 compares the iron oxide scale tests obtained from the two processes. It is evident that the iron oxide scale obtained by the example process has a higher impedance value and a lower corrosion current density, indicating better chemical stability and greater uniformity and stability during use. Moreover, the scale contains a higher proportion of Fe3O4 and FeO phases. Fe3O4, with its higher strength, is a hard phase and therefore needs to be used in conjunction with the lower-strength FeO to better prevent cracking and peeling of the scale.

[0092] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method of producing a hot-rolled steel sheet, characterized by, The steel plate is used for water-based paint descaling spraying, and the method includes: A slab with a predetermined chemical composition is heated to a predetermined temperature. The predetermined chemical composition includes: C, Si, Mn, P, S, Alt, Cr, Ti, and Fe; wherein the content of C is 0.08 wt% to 0.12 wt%, the content of Si is 0.08 wt% to 0.12 wt%, the content of Mn is 1.4 wt% to 1.7 wt%, the content of P is ≤0.03 wt%, the content of S is ≤0.07 wt%, the content of Alt is 0.01 wt% to 0.03 wt%, the content of Cr is 0.1 wt% to 0.2 wt%, and the content of Ti is 0.1 wt% to 0.15 wt%. The heated slab is subjected to a first rolling process to obtain an intermediate slab; wherein the thickness of the intermediate slab is controlled to be 30mm-35mm. Under the conditions of setting the inlet temperature and the final rolling temperature of the second rolling, the intermediate billet is finished rolled to obtain strip steel. The inlet temperature of the second rolling is set to 1000℃-1050℃, and the final rolling temperature of the second rolling is set to 810℃-830℃. The strip steel is cooled in stages and then coiled to obtain a hot-rolled steel plate. The staged cooling includes three stages of cooling: ultra-fast cooling, laminar flow cooling and air cooling. The pressure of ultra-fast cooling is 0.3MPa-0.6MPa, and the laminar flow cooling adopts a sparse cooling mode. The surface iron oxide scale quality parameters of the hot-rolled steel plate include: iron oxide scale thickness ≤10μm, and iron oxide scale impedance value ≥5×10. 4 Ω·cm 2 The corrosion current density of iron oxide scale is ≤3.86×10⁻⁶. -7 A·cm -2 The Fe3O4 content in the iron oxide scale is ≥50% by weight and the FeO content in the iron oxide scale is ≥10% by weight.

2. The method of claim 1, wherein, The set temperature is 1170℃-1210℃.

3. The method of claim 1, wherein, The process of finishing-rolling the intermediate billet to obtain strip steel under the conditions of setting the inlet temperature and the final rolling temperature of the second rolling process includes: Under the conditions of setting the inlet temperature and the final rolling temperature of the second rolling, and controlling the opening ratio of the cooling water between the finishing mill stands, the intermediate billet is finished rolled to obtain strip steel; wherein, The cooling water operating rate is 30%-60%.

4. The method of claim 1, wherein, The winding temperature is 550℃-580℃.

Citation Information

Patent Citations

  • Hot rolled steel plate surface oxidation iron sheet control method for vanadium-containing automobile beam

    CN101147920A

  • Anti-stripping iron oxide scale structure on surface of hot rolled plate and control process for anti-stripping iron oxide scale structure

    CN105618507A

  • Manufacturing method of hot-rolled complex-phase steel for 590MPa-grade thick-specification high-fatigue-performance automobile spoke

    CN113073251A

  • Weathering steel with high corrosion resistance and preparation method

    CN115110006A