Preparation method of wet-modified silica, wet-modified silica, masterbatch and vulcanizate

By modifying silica by first adding a silane coupling agent to an organic solvent and then adding tea polyphenols, the problem of limited reactivity of the coupling agent was solved, and good dispersion of silica in the rubber matrix and improved performance of composite materials were achieved.

CN116515169BActive Publication Date: 2026-11-17BEIJING UNIV OF CHEM TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210064271.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-20
Publication Date
2026-11-17
Estimated Expiration
2042-01-20

AI Technical Summary

Technical Problem

In existing wet-process methods for modifying silica, the coupling agent has limited reactivity, resulting in poor dispersion and interfacial interaction of silica in the rubber matrix, which affects the performance of the composite material.

Method used

Silica was modified in an organic solvent by using a combination of tea polyphenols and silane coupling agents. The silane coupling agent was added first, followed by the tea polyphenols, to form hydrogen bonds, thereby improving the oleophilicity and dispersibility of silica and enhancing its dispersion stability in a rubber matrix.

Benefits of technology

It improves the dispersibility and interfacial interaction of silica in the rubber matrix, enhances the abrasion resistance and compression heat generation performance of vulcanizates, and reduces energy consumption and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003479503980000061
    Figure BDA0003479503980000061
  • Figure BDA0003479503980000071
    Figure BDA0003479503980000071
  • Figure BDA0003479503980000072
    Figure BDA0003479503980000072
Patent Text Reader

Abstract

This invention discloses a method for preparing wet-process modified silica, the wet-process modified silica, masterbatch, and vulcanizate. The method for preparing the wet-process modified silica includes: uniformly dispersing silica in an organic solvent to form a slurry; adding a silane coupling agent and reacting; and then adding tea polyphenols to obtain the wet-process modified silica. This invention uses both tea polyphenols and a silane coupling agent to modify silica in an organic solvent, which improves the uniformity of silica dispersion and maintains its stability in the organic solvent, reduces the hydrophilicity of silica, and reduces agglomeration. The modified silica exhibits better dispersion in the rubber matrix. With the addition of tea polyphenols, the abrasion resistance and compression heat generation properties of the vulcanizate are significantly improved, and it also has higher 100% and 300% tensile stresses, resulting in better applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rubber nanocomposite materials technology, specifically to a method for preparing wet-modified silica, wet-modified silica, masterbatch, and vulcanizate. Background Technology

[0002] Carbon black and silica are the most commonly used reinforcing fillers in elastomer composites, especially silica, which is a promising candidate to replace traditional carbon black. This is important for the green tire industry because silica has been used as a filler in tires to reduce fuel consumption in passenger cars and special-purpose vehicles. However, silica has a highly polar surface and a large number of hydroxyl groups on its surface; this makes it prone to aggregation and interaction with rubber. Fortunately, these issues can be overcome by surface modification of silica with organic compounds to reduce the number of active hydroxyl groups on the surface.

[0003] The modification processes for silica can be mainly divided into three types: in-situ modification, dry modification, and wet modification. In-situ modification is the simplest, involving mixing silica, a coupling agent, and the matrix together, and then using methods such as catalysts or vacuum to allow the silica and coupling agent to react and complete the modification. However, this method also results in less than ideal modification effects, and the difficulty in ensuring uniform mixing and reaction of the three raw materials makes the modification process difficult to control, subject to various constraints. Wet modification, as described in Chinese patents CN103203810A and CN105602047A, involves mixing the coupling agent with silica in a liquid solvent and modifying it under specific conditions. Compared to dry modification, this modification method results in a more uniform mixture of silica and coupling agent, and the reaction is more controllable. However, the reactivity of the coupling agent limits the further modification of silica, restricting its dispersion in the rubber matrix and its interfacial interaction with rubber. Therefore, it is necessary to develop and explore a new silica modification method to further improve the dispersibility of silica in the rubber matrix in order to prepare higher performance composite materials. Summary of the Invention

[0004] To address the problems existing in the prior art, this invention provides a method for preparing wet-modified silica, the wet-modified silica, masterbatch, and vulcanizate. The method for preparing wet-modified silica includes: uniformly dispersing silica in an organic solvent to form a slurry; adding a silane coupling agent and reacting; and then adding tea polyphenols to obtain the wet-modified silica. This invention uses both tea polyphenols and a silane coupling agent to modify silica in an organic solvent, which improves the uniformity of silica dispersion and maintains its stability in the organic solvent, reduces the hydrophilicity of silica, and reduces agglomeration. The modified silica exhibits better dispersion in the rubber matrix. With the addition of tea polyphenols, the abrasion resistance and compression heat generation properties of the vulcanizate are significantly improved, and it also has higher 100% and 300% tensile stresses, resulting in better applications.

[0005] One of the objectives of this invention is to provide a method for preparing wet-modified silica.

[0006] The method includes:

[0007] The silica was uniformly dispersed in an organic solvent to form a slurry. After the reaction was completed by adding a silane coupling agent, tea polyphenols were added and reacted to obtain the wet-process modified silica.

[0008] In a preferred embodiment of the present invention,

[0009] The silane coupling agent can be added either in one step or dropwise.

[0010] In a preferred embodiment of the present invention,

[0011] The silica can be precipitated or fumed silica, which are conventional in the art and have a specific surface area of ​​50–300 m². 2 / g, preferably 100-200m 2 / g, with an oil absorption value of 0.3–3 ml / g, preferably 0.5–1.5 ml / g; and / or,

[0012] The organic solvent is a good solvent for rubber and can dissolve silane coupling agents without participating in the reaction; preferably, it is cyclohexane or n-hexane.

[0013] The reasons for choosing organic solvents as the modification solvent in this invention are as follows: considering that organic solvents are mostly used in the actual solution polymerization process of rubber, the solvents used in the rubber production process are selected in this invention, which can avoid the rubber manufacturer from removing the solvent and also avoid the silica from removing the solvent after modification. In this process, energy consumption can be reduced and the cost of finished rubber products can be reduced.

[0014] The silane coupling agent may be a conventional silane coupling agent in the art, preferably at least one of bis-[γ-(triethoxysilane)propyl]tetrasulfide (Si69), bis-[γ-(triethoxysilane)propyl]disulfide (Si75), 3-thiocyanopropyltriethoxysilane, γ-mercaptopropyltriethoxysilane (KH580), γ-aminopropyltriethoxysilane (KH550), and γ-methacryloyloxypropyltrimethoxysilane (KH570).

[0015] In a preferred embodiment of the present invention,

[0016] The solid content of the silica in the organic solvent is 5% to 20%, preferably 14% to 16%;

[0017] The amount of the silane coupling agent is 3% to 15% of the mass of the silica, preferably 8% to 12%.

[0018] The amount of tea polyphenols used is 1-5% of the mass of the precipitated silica, preferably 1-4%, and more preferably 1.4-2.1%.

[0019] In a preferred embodiment of the present invention,

[0020] The reaction temperature after the addition of the silane coupling agent is 10℃~80℃, and the reaction time is 0.1~5h, preferably 0.5~3h, and more preferably 0.5~1.5h;

[0021] The reaction temperature after the addition of tea polyphenols is 5℃~50℃, and the reaction time is 0.1~3h, preferably 0.1~1.5h, and more preferably 0.5~1h.

[0022] Silane coupling agents are soluble in organic solvents. There are currently two mechanisms for modifying silica with silane coupling agents: one is that the ethoxy group on the silane coupling agent reacts directly with the silanol group on the silica (high activation energy, difficult reaction); the other is that the ethoxy group first hydrolyzes to generate silanol groups, which then react with the silanol groups on the silica (simple reaction). If tea polyphenols and silane coupling agents are added simultaneously, competition occurs on the silica surface: firstly, the hydroxyl groups of tea polyphenols form hydrogen bonds with the hydroxyl groups on the silica; secondly, the silane coupling agent reacts with the hydroxyl groups on the silica, and the hydroxyl groups on the silica, after forming hydrogen bonds with the tea polyphenols, will not react with the coupling agent, resulting in reduced coupling agent efficiency and consequently, a significant decrease in the properties of the prepared rubber. This application, however, involves adding the coupling agent to an organic solvent first for reaction, followed by the addition of tea polyphenols for further modification, without affecting the coupling agent's modification efficiency. The adjacent phenolic hydroxyl groups on the surface of tea polyphenols can form five-membered rings with the silica surface, and no large molecular long chains are released into the rubber to act as plasticizers.

[0023] The purpose of wet-process modified silica is to further enhance the modification effect of silica based on coupling agent-modified silica. Adding tea polyphenols can improve the oleophilicity of silica, further enhancing its compatibility with rubber and improving its dispersion. Using tea polyphenols alone to modify silica only improves its dispersibility in rubber but does not establish an interaction between the rubber and silica (tea polyphenols cannot be bonded to the rubber), resulting in vulcanizates that do not meet application requirements. The main function of the wet-process modified silica of this invention is to further improve the performance of vulcanizates based on current main production processes. Adding tea polyphenols to coupling agent-modified silica can further improve its performance.

[0024] A second objective of this invention is to provide a wet-modified silica prepared by a method according to one objective of this invention.

[0025] The third objective of this invention is to provide a masterbatch containing wet-modified silica, which is the second objective of this invention.

[0026] The masterbatch is prepared from a rubber solution and the wet-modified silica.

[0027] In a preferred embodiment of the present invention,

[0028] The rubber solution is a solution polymerized rubber solution or a solution obtained by dissolving rubber in an organic solvent;

[0029] The solution-polymerized rubber may be a conventional solution-polymerized rubber in the art, preferably at least one of solution-polymerized styrene-butadiene rubber, polyisoprene rubber, and cis-butadiene rubber; and / or,

[0030] The rubber may be any conventional rubber in the art, preferably at least one of natural rubber and butyl rubber, with a molecular weight ranging from 50,000 to 5,000,000, preferably from 100,000 to 2,000,000; and / or,

[0031] The organic solvent may be the same as or different from the organic solvent used in the preparation of the wet-modified silica, and each is preferably cyclohexane or n-hexane.

[0032] In a preferred embodiment of the present invention,

[0033] The solid content of the rubber solution is 10% to 50%, preferably 10% to 15%; the mass of the silica is 1% to 100% of the mass of the rubber or solution-polymerized rubber, preferably 50% to 100%, and more preferably 65% ​​to 75%.

[0034] The fourth objective of this invention is to provide a method for preparing the masterbatch that is the objective of the third objective of this invention.

[0035] The method includes:

[0036] The wet-modified silica and the rubber solution are mixed evenly at the specified mass ratio, and the solvent is removed to obtain the masterbatch.

[0037] In a preferred embodiment of the present invention,

[0038] Solvent removal can be performed using any method known in the art.

[0039] The fifth objective of this invention is to provide a vulcanizate comprising the masterbatch of the third objective of this invention or the masterbatch prepared by the method of the fourth objective of this invention.

[0040] The vulcanized rubber is obtained by mixing and vulcanizing components including the masterbatch, activator, antioxidant, accelerator and vulcanizing agent.

[0041] In a preferred embodiment of the present invention,

[0042] The activator, antioxidant, accelerator, and vulcanizing agent can be conventional activators, antioxidants, accelerators, and vulcanizing agents in the art, and their dosages are also conventional. Technicians can adjust them according to the actual situation.

[0043] The present invention may preferably adopt the following specific technical solutions:

[0044] First, the silica is dispersed in an organic solvent. Under mechanical grinding or stirring conditions, it is first modified in the liquid phase using a silane coupling agent. After modification, tea polyphenols are added for further modification, and finally, a uniformly dispersed wet-modified silica is obtained.

[0045] The beneficial effects of this invention are as follows:

[0046] Because the coupling agent has limited activity, the hydroxyl groups on the surface of silica do not react completely. Under certain conditions, the residual hydroxyl groups will form hydrogen bonds, causing silica agglomeration and reducing macroscopic properties (such as compression heat generation). In order to maintain the stable dispersion of silica particles after grinding, it is necessary to further cover its surface hydroxyl groups to prevent agglomeration.

[0047] This invention utilizes a combination of tea polyphenols and silane coupling agents to modify silica in an organic solvent. Building upon traditional silica modification with coupling agents, the use of tea polyphenols to form hydrogen bonds with the silanol groups on the silica surface further reduces the hydrophilicity of the silica. This improves the uniformity of silica dispersion and maintains its stability in the organic solvent, reducing agglomeration. The wet-modified silica exhibits better dispersion in a rubber matrix. Simultaneously, the entanglement of the long-chain macromolecules of tea polyphenols also enhances interfacial interactions and silica dispersion. The combined use of tea polyphenols (macromolecules) and silane coupling agents complements each other, resulting in better modification effects. Compared to using silane coupling agents alone, the combined use of both further improves the dispersion of silica in the rubber matrix.

[0048] This invention employs a wet-process modification of silica using a one-step liquid-phase mixing method. Specifically, silane coupling agents, tea polyphenols, and silica are sequentially modified in an organic solvent liquid phase environment to obtain uniform and stable wet-modified silica. This modified silica is then directly mixed with a rubber solution, eliminating the step of separating the modified silica from the liquid phase, thus reducing energy consumption and shortening the masterbatch preparation cycle. Furthermore, modification in an organic phase environment reduces the self-polymerization process of the coupling agent. Considering that organic solvents are predominantly used in the actual solution polymerization of rubber, this invention selects the organic solvents used in rubber production. This avoids solvent release by rubber manufacturers and prevents silica from releasing solvent after modification. The entire process is simple and efficient, reducing energy consumption and the cost of the finished rubber product.

[0049] This invention has a good modification effect on silica, which can effectively improve the dispersibility of silica in rubber matrix, thereby improving the dynamic performance of composite materials. With the addition of tea polyphenols, the wear resistance of vulcanized rubber is effectively improved, the heat generated during compression is reduced, and it has higher 100% and 300% tensile stress, resulting in better applications.

[0050] Furthermore, tea polyphenols can enhance the heat resistance and aging resistance of tire tread rubber, and the higher the amount used, the better the improvement. Moreover, tea polyphenols are low in cost and easy to extract; if they significantly improve the performance of tire tread rubber, they can be directly used as a modifier to reduce costs. Detailed Implementation

[0051] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.

[0052] All raw materials used in the examples are commercially available.

[0053] The main raw material specifications are as follows:

[0054]

[0055]

[0056] The relevant performance testing methods and instruments used in the embodiments are shown in Table 1:

[0057] Table 1. Relevant performance testing methods and instruments

[0058]

[0059] Table 2 Rubber Formulations for Examples and Comparative Examples

[0060]

[0061]

[0062] Example 1

[0063] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 15℃ for 1 hour. Then, the temperature was raised to 30℃, and 1.4g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0064] Example 2

[0065] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 1 hour. Then, the temperature was lowered to 30℃, and 1.4g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0066] Example 3

[0067] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 75℃ for 1 hour. Then, the temperature was lowered to 30℃, and 1.4g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0068] Comparative Example 1

[0069] 70g of silica was added to cyclohexane and stirred to prepare a silica-cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 1 hour. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch and 1.4g of tea polyphenols were mixed evenly in an internal mixer. Then, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were added and mixed evenly. The mixture was then discharged and heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0070] Comparative Example 2

[0071] 70g of silica was added to cyclohexane and stirred to prepare a silica-cyclohexane dispersion with a solid content of 15%. 1.4g of tea polyphenols was added to the dispersion at 30℃ and stirred for 30 minutes. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃ to allow precipitation and coagulation, yielding SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in an internal mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0072] Table 3 Physical properties of vulcanizates from Examples 1-3 and Comparative Examples 1-2

[0073]

[0074] The difference between Examples 1, 2, and 3 is that the coupling agent-modified silica was applied at temperatures of 15°C, 55°C, and 75°C, respectively. The difference between Comparative Example 1 and the Examples is only that the tea polyphenols in Examples 1, 2, and 3 were added during the silica modification process, while the tea polyphenols in Comparative Example 1 were added during the mixing process. The difference between Comparative Example 2 and the Examples is that, compared to Examples 1, 2, 3, and Comparative Example 1, Comparative Example 2 did not include a coupling agent.

[0075] Table 3 shows that among the vulcanizates prepared in Examples 1, 2, and 3, Example 2 exhibits the best mechanical properties, compression heat generation, Akron abrasion performance, and wet skid resistance. This is because modifying silica with a liquid-phase coupling agent requires a certain temperature, but excessively high temperatures can lead to coupling agent loss and reduced modification efficiency. Furthermore, the tensile strength, 100% elongation stress, and 300% elongation stress of Examples 1, 2, and 3 are significantly higher than those of Comparative Example 1, with Example 2 showing the best mechanical properties. The elongation at break and tear strength are essentially the same for both processes. Considering all properties, the vulcanizates of Examples 1, 2, and 3 possess better mechanical properties. The vulcanizates modified in Examples 1, 2, and 3 exhibit lower compression heat generation and lower Akron abrasion volume, with a maximum reduction of 5.9°C in compression heat generation compared to Comparative Example 1. The loss factor at 0°C is significantly increased, indicating better wet skid resistance. As can be seen from the table, the vulcanized rubber obtained by using tea polyphenols alone in Comparative Example 2 has lower mechanical properties, worse compression heat generation and abrasion resistance, and poorer performance compared to the examples.

[0076] Example 4

[0077] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 30 minutes. Then, the temperature was lowered to 30℃, and 1.4g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.8g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0078] Example 5

[0079] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 2 hours. Then, the temperature was lowered to 30℃, and 1.4g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0080] Table 4 Physical properties of vulcanizates from Examples 2, 4 and 5

[0081]

[0082] The difference between Examples 2, 4, and 5 is that the coupling agent modification time for silica is 1h, 0.5h, and 2h, respectively.

[0083] Table 4 shows that the modification of silica with coupling agent at 55℃ requires a certain amount of time. Among the tested samples, 1 hour yielded the best modification effect, exhibiting better mechanical properties, compression heat generation properties, wear resistance, and wet skid resistance. This is because a shorter time would not allow the coupling agent to fully modify the silica, while a longer time would lead to the loss of self-polymerization of the coupling agent, resulting in a reduction in the monomer coupling agent content during the heat treatment stage and a decrease in the silica modification effect.

[0084] Comparative Example 3

[0085] 70g of silica was added to cyclohexane and stirred to prepare a silica-cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 1 hour. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in an internal mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0086] Example 6

[0087] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 1 hour. Then, the temperature was lowered to 30℃, and 2.1g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0088] Example 7

[0089] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 1 hour. Then, the temperature was lowered to 30℃, and 2.8g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0090] Table 5 Physical properties of vulcanizates from Examples 2, 6, 7 and Comparative Example 3

[0091]

[0092] The only difference between Examples 2, 6, and 7 is the amount of tea polyphenols used: 1.4g, 2.1g, and 2.8g, respectively. The mechanical properties of vulcanizates modified with different amounts of tea polyphenols are shown in Table 5. From the data in Examples 2, 6, and 7, it can be seen that after introducing tea polyphenols into the composite system, increasing the amount of tea polyphenols leads to a decreasing trend in the 100% and 300% elongation of the vulcanizates. When the amount of tea polyphenols added is small, the abrasion volume of the rubber compound decreases, i.e., the abrasion resistance is improved. However, with the increase of the amount, the abrasion resistance deteriorates but is still higher than that of Comparative Example 3 without added tea polyphenols. The compression heat generation properties of fumed silica / solution styrene-butadiene composite vulcanizates with different amounts of tea polyphenols are shown in the table. Analysis of the data in the table shows that with the increase of tea polyphenols, the bottom temperature rise continuously decreases, and the dynamic heat generation properties of the rubber compound improve.

[0093] Example 8

[0094] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 8.4g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 1 hour. Then, the temperature was lowered to 30℃, and 1.4g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0095] Table 6 Physical properties of vulcanizates in Examples 2 and 8

[0096]

[0097] The difference between Examples 2 and 8 lies in the amount of coupling agent used in the modification of silica: 10% and 12% of the silica mass, respectively. Under conditions of a small amount of coupling agent, the amount of coupling agent is directly proportional to the mechanical properties and abrasion resistance. As the amount of coupling agent increases to an excess, the mechanical properties and abrasion resistance tend to first increase and then decrease. Too little coupling agent cannot complete the modification of silica, while excessive coupling agent disperses in the rubber matrix and acts as a plasticizer, causing a decrease in mechanical properties and abrasion resistance. Compression heat generation decreases with increasing coupling agent content, because the dispersibility of silica in the rubber is improved.

[0098] Example 9

[0099] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 1 hour. Then, the temperature was lowered to 10℃, and 1.4g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0100] Example 10

[0101] 70g of silica was added to cyclohexane and stirred to prepare a silica cyclohexane dispersion with a solid content of 15%. 7g of Si69 was added dropwise to the dispersion, and the mixture was stirred at 55℃ for 1 hour. Then, the temperature was lowered to 40℃, and 1.4g of tea polyphenols was added. The mixture was stirred for 30 minutes, and the resulting slurry was the wet-modified silica. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (SBR) cyclohexane solution (SBR mass: 100g), and stirred until homogeneous to obtain a modified mixed rubber solution. The mixed rubber solution was poured into hot water at a temperature above 95℃, allowing precipitation and coagulation to obtain SSBR / silica masterbatch. Subsequently, the dried masterbatch, 3g of zinc oxide, 2g of stearic acid, and 2g of antioxidant 4020 were mixed homogeneously in a Banbury mixer, discharged, and then heat-treated at 150℃ for 5 minutes to obtain the compound. On a two-roll mill, 1.7g of accelerator CZ, 1.8g of accelerator DPG and 1.7g of sulfur were added to the cooled compound. After mixing evenly, the compound was sheeted out and left to stand for 12 hours. It was then vulcanized on a 150℃ flat vulcanizing machine until it reached the correct vulcanization temperature to obtain vulcanized rubber.

[0102] Table 7 Physical properties of vulcanizates from Examples 2, 9 and 10

[0103]

[0104] The difference between Examples 2, 9, and 10 is that the temperatures for modifying the polyphenol-modified silica are 30°C, 10°C, and 40°C, respectively. As can be seen from Table 7, within the set temperature range, changing the temperature has little effect on the polyphenol-modified silica.

[0105] Comparative Example 4

[0106] 70g of silica was added to cyclohexane and stirred to prepare a silica-cyclohexane dispersion with a solid content of 15%. 7g of Si69 and 2.8g of tea polyphenols were added to the dispersion, and the mixture was stirred at 55°C for 1 hour. This slurry was then added to 833g of solution-polymerized styrene-butadiene rubber (100g of solution-polymerized styrene-butadiene rubber) cyclohexane solution and stirred until homogeneous, yielding a modified mixed adhesive. The mixed adhesive was poured into hot water at a temperature above 95°C, causing precipitation and coagulation. During this process, silica precipitated. 4g of the obtained masterbatch was heated to 700°C under a nitrogen atmosphere in a muffle furnace and held for 30 minutes, yielding an ash content of 1.3g. In contrast, the masterbatches of Examples 1-10 and Comparative Examples 1-3, under the same testing conditions, had 1.7g of residual ash (only silica leaves residual ash at 700°C). This indicates that the co-addition method will result in some loss of silica during solvent removal (if the modification effect is good, silica will not precipitate during solvent removal).

[0107] As can be seen from Examples 1-10 and Comparative Examples 1-4, the present invention has a good modification effect on silica, which can effectively improve the dispersibility of silica in rubber matrix, thereby improving the dynamic performance of composite material. With the addition of tea polyphenols, the wear resistance of vulcanized rubber is effectively improved, the heat generated during compression is reduced, and it has higher 100% and 300% tensile stress, resulting in better applications.

Claims

1. A method for preparing a wet-modified white carbon black, characterized in that The method includes: The silica was uniformly dispersed in an organic solvent to form a slurry. After the reaction was completed by adding a silane coupling agent, tea polyphenols were added and reacted to obtain the wet-modified silica. The amount of tea polyphenols used is 1-5% of the mass of the precipitated silica; The organic solvent is a good solvent for rubber; The silane coupling agent is at least one of bis-[γ-(triethoxysilane)propyl]tetrasulfide, bis-[γ-(triethoxysilane)propyl]disulfide, 3-thiocyanopropyltriethoxysilane, γ-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane.

2. The preparation method according to claim 1, characterized in that: The white carbon black has a specific surface area of 50-300 m 2 / g, an oil absorption value of 0.3-3 ml / g; and / or, The organic solvent is cyclohexane or n-hexane.

3. The production method according to claim 2, characterized by: The white carbon black has a specific surface area of 100-200 m 2 / g and an oil absorption value of 0.5-1.5 ml / g.

4. The preparation method according to claim 1, characterized in that: The solid content of the silica in the organic solvent is 5% to 20%; The amount of the silane coupling agent is 3% to 15% of the mass of the silica; The amount of tea polyphenols used is 1 to 4% of the mass of the precipitated silica.

5. The preparation method according to claim 1, characterized in that: The reaction temperature after the addition of the silane coupling agent is 10℃~80℃, and the reaction time is 0.1~5h; the reaction temperature after the addition of the tea polyphenols is 5℃~50℃, and the reaction time is 0.1~3h.

6. A wet-modified silica prepared by the method according to any one of claims 1-5.

7. A masterbatch comprising the wet-modified silica as described in claim 6, characterized in that: The masterbatch is prepared from a rubber solution and the wet-modified silica.

8. The masterbatch as described in claim 7, characterized in that: The rubber solution is a solution polymerized rubber solution or a solution obtained by dissolving rubber in an organic solvent; The solution polymerized rubber is at least one of solution polymerized styrene-butadiene rubber, polyisoprene rubber, and cis-butadiene rubber; and / or... The rubber is at least one of natural rubber and butyl rubber.

9. The masterbatch as described in claim 8, characterized in that: The solid content of the rubber solution is 10% to 50%; the mass of the silica is 1% to 100% of the mass of the rubber or solution-polymerized rubber.

10. The masterbatch of claim 9, wherein: The mass of the silica is 50% to 100% of the mass of the rubber or solution rubber.

11. A process for the preparation of a masterbatch as claimed in any one of claims 7 to 10, characterised in that The method includes: The wet-modified silica and the rubber solution are mixed evenly at the specified mass ratio, and the solvent is removed to obtain the masterbatch.

12. A vulcanizate comprising the masterbatch according to any one of claims 7-10 or the masterbatch prepared by the method of claim 11, characterized in that: The vulcanized rubber is obtained by mixing and vulcanizing components including the masterbatch, activator, antioxidant, accelerator and vulcanizing agent.

Citation Information

Patent Citations

  • Continuous manufacturing method for rubber masterbatch, rubber masterbatch prepared by using continuous manufacturing method and rubber product

    CN103203810A

  • Continuous making method of rubber masterbatch and rubber masterbatch prepared by the same

    CN105602047A

  • Method for preparing white carbon black / solution polymerized styrene-butadiene rubber masterbatch by wet process

    CN106750389A

  • Rubber composition for tire tread

    JP2010031261A