Electrode slurry and preparation method thereof, electrode sheet and photovoltaic cell
By modifying the electrode slurry that combines silver-based conductive material with thermoplastic polyurethane, the damage problem of high-temperature baking of heterojunction solar cells to the conductive film layer during sintering is solved, and the use of solvent is reduced, thereby improving the conversion efficiency and battery. Lifespan reduces the harm to workers and the environment.
Patent Information
- Application Number
- CN202310571211.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-05-17
AI Technical Summary
The high-temperature baking of existing heterojunction solar cells when sintering electrode pastes results in damage to the transparent conductive thin film layer of amorphous silicon, reducing conversion efficiency, and the solvent in the conductive silver paste is harmful to workers and the environment.
Using modified silver-based conductive material combined with thermoplastic polyurethane, the electrode slurry with a glass transition temperature between 50°C and 150°C, the flexible block polymer characteristics of thermoplastic polyurethane are complexed with the amorphous silicon transparent conductive film layer to reduce sintering Temperature and increase binding force to avoid solvent use.
It effectively reduces the sintering temperature, avoids damage to the battery surface, improves conversion efficiency and battery life, and reduces the harm to workers and the environment.
Smart Images

Figure CN116525175B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to an electrode slurry and a preparation method thereof, an electrode sheet and a photovoltaic cell. Background Art
[0002] The theoretical efficiency of heterojunction solar cells can reach 28%, which is much higher than conventional PERC crystalline silicon solar cells, and therefore has become one of the development directions of the next generation of solar cells. At present, the surface of heterojunction solar cells is mainly amorphous silicon transparent conductive film layer, and the temperature resistance is lower than 250℃.
[0003] In the existing technology, when producing amorphous silicon transparent conductive film layers, the main curing process is generally to sinter at 150℃-220℃ for 10min-30min to obtain a heterojunction solar cell. Due to the high sintering temperature, the conductive layer on the surface of the heterojunction cell is damaged, resulting in an increase in contact resistivity and a decrease in conversion efficiency. On the other hand, since the existing conductive silver paste for heterojunction cells contains certain solvents, there is a certain risk of damage to the health of workers at the production site and the environment around the factory during the production of solar cells. Summary of the invention
[0004] The object of the present invention is to provide an electrode slurry and a preparation method thereof, an electrode sheet and a photovoltaic cell, which can avoid damage to the amorphous silicon transparent conductive film layer on the cell surface caused by excessively high sintering temperature when sintering the electrode slurry during the cell manufacturing process.
[0005] In a first aspect, the present invention provides an electrode slurry, comprising a modified silver-based conductive material and an organic carrier, wherein the modified silver-based conductive material comprises a silver-based conductive material and a thermoplastic polyurethane wrapped on the surface of the silver-based conductive material, and the glass transition temperature of the thermoplastic polyurethane is 50°C to 150°C.
[0006] Compared with the prior art, the electrode slurry provided by the present invention has the following advantages:
[0007] The electrode slurry provided by the present invention includes a modified silver-based conductive material and an organic carrier, wherein the modified silver-based conductive material includes a silver-based conductive material and a thermoplastic polyurethane wrapped on the surface of the silver-based conductive material. When a grid line is formed on a solar cell, since the surface of the silver-based conductive material is wrapped with thermoplastic polyurethane, the problem of normal printing caused by the agglomeration of the silver-based conductive material can be avoided. At the same time, since the glass transition temperature of thermoplastic polyurethane is 50°C to 150°C, the silver-based conductive material modified by thermoplastic polyurethane dispersed in the organic carrier can be cured with the solar cell at 50°C to 150°C, which reduces the curing sintering temperature and avoids the problem of high-temperature baking of the electrode slurry for curing during the production of heterojunction batteries, thereby damaging the amorphous silicon transparent conductive film layer of the heterojunction battery. Moreover, since thermoplastic polyurethane is a flexible block polymer, it can complex the ions of the amorphous silicon transparent conductive film layer, thereby improving the bonding force of the silver grid line on the solar cell after curing, reducing the contact resistivity, improving the conversion efficiency, and helping to extend the service life of the battery.
[0008] In addition, the electrode slurry of the embodiment of the present invention can be cured without adding a solvent, which can reduce damage to the health of workers and damage to the environment during the production process of heterojunction solar cells.
[0009] It can be seen from the above that the electrode slurry provided by the present invention can reduce the sintering temperature and environmental pollution when forming grid lines on a battery cell.
[0010] In a second aspect, the present invention further provides a method for preparing an electrode slurry, comprising:
[0011] The silver-based conductive material and thermoplastic polyurethane are uniformly mixed and then heated to prepare a modified silver-based conductive material;
[0012] An organic carrier is mixed with the modified silver conductive material to obtain an electrode slurry, wherein the organic carrier comprises a vinyl compound, a mercapto compound and a photoinitiator.
[0013] Compared with the prior art, the beneficial effects of the method for preparing the electrode slurry provided by the present invention are the same as the beneficial effects of the electrode slurry of the first aspect, which will not be described in detail here.
[0014] In a third aspect, the present invention further provides an electrode sheet, wherein the electrode sheet comprises the electrode slurry provided by the present invention.
[0015] Compared with the prior art, the electrode sheet provided by the present invention includes the electrode slurry provided by the present invention, so the beneficial effects are the same as the beneficial effects of the electrode slurry in the first aspect, which will not be described in detail here.
[0016] In a fourth aspect, the present invention further provides a photovoltaic cell, wherein the photovoltaic cell comprises the electrode slurry provided by the present invention.
[0017] Compared with the prior art, the photovoltaic cell provided by the present invention includes the electrode slurry provided by the present invention, so the beneficial effects are the same as the beneficial effects of the electrode slurry in the first aspect, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0019] Figure 1 A schematic diagram of the structure of a battery according to an embodiment of the present invention;
[0020] Figure 2 The figure is a flow chart of the preparation of the electrode slurry according to an embodiment of the present invention.
[0021] Reference numerals:
[0022] 100-battery, 101a-positive electrode, 101b-negative electrode, 102a-first amorphous silicon transparent conductive film layer, 102b-second amorphous silicon transparent conductive film layer, 103a-first intrinsic amorphous silicon film, 103b-second intrinsic amorphous silicon film, 104-P-type amorphous silicon film, 105-N-type amorphous silicon film. DETAILED DESCRIPTION
[0023] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0024] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.
[0025] Conventional crystalline silicon solar cells are made on a complete silicon wafer, using different doping processes to form an N-type semiconductor on one side and a P-type semiconductor on the other side, and a PN junction is formed in the area near the interface of the two semiconductors. The full name of heterojunction solar cells is intrinsic thin-film heterojunction cells (HJT, Heterojunction with Intrinsic Thin-layer), which is a special PN junction formed by amorphous silicon and crystalline silicon materials. It is a type of N-type cell that deposits an amorphous silicon thin film on crystalline silicon. Since the theoretical efficiency of heterojunction cells can reach 28%, which is much higher than conventional crystalline silicon solar cells, it has become one of the development directions of the next generation of solar cells.
[0026] Since the surface of the heterojunction solar cell is mainly an amorphous silicon transparent conductive film layer, and the temperature resistance of the amorphous silicon transparent conductive film layer is lower than 250°C, the surface of the heterojunction solar cell needs to be printed with a conductive silver paste with a curing temperature below 220°C. However, the curing process of the conductive silver paste in the prior art is generally sintered at 150°C to 220°C for 10min to 30min. The curing temperature is relatively high, which has the risk of damaging the surface amorphous silicon transparent conductive film layer of the heterojunction solar cell. In addition, the sintering time is relatively long compared to the sintering time of conventional crystalline silicon solar cells, which is not conducive to improving production efficiency and reducing the cost of heterojunction solar cells.
[0027] In view of the above problems, an embodiment of the present invention provides a heterojunction battery, which may include the electrode material of the embodiment of the present invention to avoid damage to the amorphous silicon transparent conductive film layer on the battery surface due to excessively high sintering temperature when sintering the electrode slurry. It should be understood that the heterojunction battery may include an electrode material, a substrate, an amorphous silicon transparent conductive film layer, a P-type amorphous silicon film, an intrinsic amorphous silicon film, and an N-type amorphous silicon film. Figure 1 The schematic diagram of the structure of the battery of the embodiment of the present invention is shown as follows: Figure 1 As shown, the heterojunction battery 100 of the embodiment of the present invention comprises, from the front side of the battery from top to bottom, a positive electrode 101a, a first amorphous silicon transparent conductive film layer 102a, a P-type amorphous silicon film 104, a first intrinsic amorphous silicon film 103a, a substrate 106, a second intrinsic amorphous silicon film 103b, an N-type amorphous silicon film 105, a second amorphous silicon transparent conductive film layer 102b and a negative electrode 101b.
[0028] An electrode slurry provided in an embodiment of the present invention can be applied to the above-mentioned battery. It includes: a modified silver-based conductive material and an organic carrier, wherein the modified silver-based conductive material includes a silver-based conductive material and a thermoplastic polyurethane wrapped on the surface of the silver-based conductive material, and the glass transition temperature of the thermoplastic polyurethane is 50°C to 150°C. It should be understood that the glass transition temperature of the thermoplastic polyurethane is preferably 80°C to 120°C. The silver-based conductive material can be silver powder or silver alloy powder, which is not limited here.
[0029] The electrode slurry provided by the present invention includes a modified silver-based conductive material and an organic carrier, wherein the modified silver-based conductive material includes a silver-based conductive material and a thermoplastic polyurethane wrapped on the surface of the silver-based conductive material. When forming a grid line on a solar cell, since the surface of the silver-based conductive material is wrapped with thermoplastic polyurethane, the problem of normal printing failure caused by the agglomeration of the silver-based conductive material can be avoided. At the same time, since the glass transition temperature of thermoplastic polyurethane is 50°C to 150°C, the silver-based conductive material modified by thermoplastic polyurethane dispersed in the organic carrier can be cured with the solar cell at 50°C to 150°C, thereby avoiding the problem of high-temperature baking of the electrode slurry for curing during the production of heterojunction batteries, thereby damaging the amorphous silicon transparent conductive film layer of the heterojunction battery. Moreover, since thermoplastic polyurethane is a flexible block polymer, it can complex the ions of the amorphous silicon transparent conductive film layer, thereby improving the bonding force of the silver grid line on the solar cell after curing, reducing the contact resistivity, improving the conversion efficiency, and being conducive to extending the service life of the solar cell.
[0030] In addition, the electrode slurry of the embodiment of the present invention can be cured without adding a solvent, which can reduce damage to the health of workers and damage to the environment during the production process of heterojunction solar cells.
[0031] In an achievable manner, in the electrode slurry of the embodiment of the present invention, the modified silver-based conductive material accounts for 75% to 95% of the electrode slurry by mass, and the organic carrier accounts for 5% to 25% of the electrode slurry by mass. At this ratio, the modified silver conductive material can be fully dispersed in the organic carrier. Since the glass transition temperature of the thermoplastic polyurethane contained in the modified silver conductive material is 50°C to 150°C, the modified silver conductive material and the organic carrier can be cross-linked and cured at low temperature (50°C to 150°C), reducing the risk of excessively high baking temperatures that easily destroy the bonding force between the silver grid lines on the surface of the heterojunction battery and the battery cell, reducing the contact resistivity, and improving the conversion efficiency.
[0032] In an optional manner, in the electrode slurry of the embodiment of the present invention, the mass percentage of thermoplastic polyurethane to the modified silver-based conductive material is 1% to 10%, and the mass percentage of silver-based conductive material to the modified silver-based conductive material is 90% to 99%. In other words, the electrode slurry of the embodiment of the present invention can wrap the silver-based conductive material with a small amount of thermoplastic polyurethane.
[0033] Exemplarily, for thermoplastic polyurethane, it may include a polymer containing repeated carbamate groups in its molecular structure, or a modified polymer containing repeated carbamate groups in its molecular structure, or a combination of the two. Preferably, the thermoplastic polyurethane may be a polymer containing repeated carbamate groups with a glass transition temperature of 80°C to 120°C or a modified polymer thereof, or a combination of the two. Thermoplastic polyurethane may be selected from thermoplastic polyurethanes having a number average molecular weight between 10,000 Da and 500,000 Da. The thermoplastic polyurethane of the embodiment of the present invention is an elastic material, which can greatly enhance the tensile strength of the electrode sheet, thereby improving the puncture resistance of the conductive film layer, reducing the probability of battery short circuit caused by puncture, and improving the efficiency of the battery.
[0034] In an optional manner, the organic carrier of the embodiment of the present invention includes a vinyl compound, a thiol compound and a photoinitiator, and the mass ratio of the vinyl compound, the thiol compound and the photoinitiator is (75-90): (5-25): (1-10).
[0035] Exemplarily, the vinyl compound includes at least one of modified epoxy resin, modified polyurethane resin and acrylate compound. Among them, the acrylate compound includes at least one of methyl methacrylate, butyl methacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate and pentaerythritol tetraacrylate. The thiol compound includes at least one of 2-mercaptoethanol, 1,6-hexanedithiol and N-acetylthiolactone. The photoinitiator includes at least one of 1-hydroxy-cyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone and benzoin dimethyl ether.
[0036] The carbon-carbon double bonds contained in the vinyl compound of the embodiment of the present invention and the thiol compound undergo chain polymerization under the action of a photoinitiator to form a thiol-vinyl system, thereby rapidly crosslinking and curing. Among them, since the modified epoxy resin and polyurethane resin have good toughness and low-temperature curing performance, the toughness and low-temperature curing performance of the organic carrier can be enhanced, thereby promoting the low-temperature curing of the modified silver-based conductive material, so that the electrode slurry can be cured under low temperature conditions, and the cured electrode has strong toughness and is not easy to break.
[0037] In an optional embodiment, the particle size distribution D50 of the modified silver-based conductive material implemented in the present invention is 0.1 μm to 5 μm, and the specific surface area of the modified silver-based conductive material is less than 3 m 2 / g, the silver-based conductive material includes spherical silver powder and / or flaky silver powder. The spherical silver powders in the embodiment of the present invention contact each other in a point-to-point manner, and the contact area is relatively small. The flaky silver powder contains a large amount of surface-to-surface contact or surface-line contact, and the contact area is relatively large. When the particle size and specific surface area of the modified silver-based conductive material are within the above range, it has a greater internal friction during relative displacement, so that the viscosity of the configured slurry is large and the curing time is reduced. At the same time, when the modified silver-based conductive material in the embodiment of the present invention contains both spherical silver powder and flaky silver powder, the spherical silver powder can fill the gaps between the flaky silver powders, so that the adjacent flaky silver powders that were originally not in contact contact each other, increase the conductive path, and thus improve the conductivity.
[0038] Exemplarily, the fineness of the electrode slurry in the embodiment of the present invention is less than 5 μm, and the viscosity is 100 Pa·S to 300 Pa·S. When the fineness and viscosity of the electrode slurry are within the above range, during the production and processing, the problem of difficult stirring due to excessive viscosity of the slurry can be avoided, thereby ensuring good printing performance, and the problem of sedimentation of suspended particles due to low viscosity, which is not conducive to the uniformity and stability of the slurry, can be avoided, thereby improving the curing rate.
[0039] Figure 2 The preparation flow chart of the electrode slurry provided by the embodiment of the present invention is shown as follows: Figure 2 As shown, the present invention also provides a method for preparing the electrode slurry, comprising:
[0040] Step 201: The silver-based conductive material and thermoplastic polyurethane are mixed evenly and then heated to prepare a modified silver-based conductive material.
[0041] Exemplarily, the thermoplastic polyurethane compound and the silver powder are mixed and stirred, the temperature is raised to 200° C., the stirring is continued for 0.5 h to h hours, and the modified silver-based conductive material is obtained. The silver-based conductive material uniformly encapsulating the thermoplastic polyurethane compound can be obtained by mixing and stirring the polyurethane compound and the silver powder at 200° C.
[0042] Step 202: Mixing an organic carrier with the modified silver-based conductive material to obtain an electrode slurry, wherein the organic carrier includes a vinyl compound, a thiol compound and a photoinitiator.
[0043] For example: First, a vinyl compound, a thiol compound and a photoinitiator are mixed and stirred to obtain an organic carrier. Then, the organic carrier is mixed with a modified silver-based conductive material, stirred, and placed on a three-roll mill for grinding and rolling, and further dispersed and homogenized. When the scraper fineness of the three-roll mill is less than 5 μm, an electrode slurry is obtained. At the same time, the viscosity at a speed of 10 rpm is tested at room temperature 25°C using a Brookfield viscometer and is 100 Pa·S to 300 Pa·S.
[0044] The electrode slurry provided by the present invention can evenly disperse the silver conductive material in the organic carrier because the organic carrier is a liquid. The organic carrier includes a vinyl compound, a thiol compound and a photoinitiator. Since the photoinitiator can absorb energy of a certain wavelength under ultraviolet light irradiation, and then undergoes chemical changes to produce free radicals or cations, the vinyl compound and the thiol compound contained in the organic carrier undergo chain polymerization under the action of free radicals or cations to form a thiol-vinyl system, thereby rapidly crosslinking and curing. Since the glass transition temperature of the thermoplastic polyurethane contained in the modified silver conductive material is 50°C to 150°C, the modified silver conductive material and the organic carrier can be crosslinked and cured at low temperatures (50°C to 150°C), reducing the risk of excessively high baking temperatures easily destroying the bonding force between the silver grid lines on the surface of the heterojunction battery and the battery cell, reducing the contact resistivity, and improving the conversion efficiency. At the same time, in the process of ultraviolet light curing of the mercapto-vinyl system, when the photoinitiator decomposes into free radicals or cations, the free radicals or cations easily react with oxygen in the air to form peroxy radicals with low reaction activity. At this time, the peroxy radicals can capture the hydrogen atoms on the mercapto group to produce mercapto radicals, thereby ensuring the continuation of the polymerization reaction, avoiding the termination of the polymerization reaction due to the presence of peroxy radicals, increasing the curing rate, and shortening the curing time.
[0045] The electrode slurry provided by the present invention includes a modified silver-based conductive material and an organic carrier, wherein the modified silver-based conductive material includes a silver-based conductive material and a thermoplastic polyurethane wrapped on the surface of the silver-based conductive material. When forming a grid line on a battery cell, since the surface of the silver-based conductive material is wrapped with thermoplastic polyurethane, the problem of normal printing failure caused by the agglomeration of the silver-based conductive material can be avoided. At the same time, since the glass transition temperature of thermoplastic polyurethane is 50°C to 150°C, the silver-based conductive material modified with thermoplastic polyurethane dispersed in the organic carrier can be cured with the battery cell at 50°C to 150°C, thereby reducing the curing and sintering temperature, and avoiding the problem of high-temperature baking of the electrode slurry for curing during the production of heterojunction batteries, thereby damaging the amorphous silicon transparent conductive film layer of the heterojunction battery.
[0046] In order to verify the effect of the electrode slurry provided by the embodiment of the present invention, the embodiment of the present invention is demonstrated by comparing the embodiment with the comparative example.
[0047] Embodiment 1
[0048] The electrode slurry provided in an embodiment of the present invention includes, by weight: 85.5 parts by weight of spherical silver powder (model: GS753, produced by Zhejiang Guangda Electronic Technology Co., Ltd.), 4.5 parts by weight of polyurethane (model: 5778, produced by Lubrizol Corporation), 6 parts by weight of 1,6-hexanediol diacrylate, 2 parts by weight of epoxy acrylate, 1 part by weight of 2-mercaptoethanol, and 1 part by weight of 1-hydroxy-cyclohexyl-phenyl ketone.
[0049] The method for preparing the electrode slurry provided in the first embodiment of the present invention comprises the following steps:
[0050] The first step is to prepare a modified silver-based conductive material: 85.5 parts by weight of commercially available spherical silver powder (model: GS753, produced by Zhejiang Guangda Electronic Technology Co., Ltd.) and 4.5 parts by weight of a polyurethane compound (model: 5778, produced by Lubrizol) are mixed and stirred evenly, the temperature is raised to 200°C, and the stirring is continued for 45 minutes. The temperature is lowered to obtain polyurethane-coated silver powder, i.e., a modified silver-based conductive material.
[0051] The second step is to prepare an organic carrier: 1,6-hexanediol diacrylate, epoxy acrylate (model: CN104NS, produced by Sartomer), 2-mercaptoethanol, and 1-hydroxy-cyclohexyl-phenyl ketone are mixed and stirred to obtain an organic carrier.
[0052] The third step is to prepare electrode slurry: the modified silver-based conductive material and the organic carrier mixture are mixed, stirred, and passed through a three-roll mill to obtain an electrode slurry with a fineness of less than 5 μm.
[0053] Embodiment 2
[0054] The electrode slurry provided in an embodiment of the present invention includes, by weight: 80 parts by weight of spherical silver powder (model: GS753, produced by Zhejiang Guangda Electronic Technology Co., Ltd.), 10 parts by weight of polyurethane (model: 5778, produced by Lubrizol Corporation), 5 parts by weight of 1,6-hexanediol diacrylate, 3 parts by weight of epoxy acrylate, 1 part by weight of 2-mercaptoethanol, and 1 part by weight of 1-hydroxy-cyclohexyl-phenyl ketone.
[0055] The method for preparing the electrode slurry provided in the second embodiment of the present invention comprises the following steps:
[0056] The first step is to prepare a modified silver-based conductive material: 80 parts by weight of commercially available spherical silver powder (model: GS753, produced by Zhejiang Guangda Electronic Technology Co., Ltd.) and 10 parts by weight of a polyurethane compound (model: 5778, produced by Lubrizol Corporation) are mixed and stirred evenly, the temperature is raised to 200°C, and the stirring is continued for 45 minutes at a temperature-keeping level, and the temperature is lowered to obtain polyurethane-coated silver powder, i.e., a modified silver-based conductive material.
[0057] The second step is to prepare an organic carrier: 1,6-hexanediol diacrylate, epoxy acrylate (model: CN104NS, produced by Sartomer), 2-mercaptoethanol, and 1-hydroxy-cyclohexyl-phenyl ketone are mixed and stirred to obtain an organic carrier.
[0058] The third step is to prepare electrode slurry: the modified silver-based conductive material and the organic carrier mixture are mixed, stirred, and passed through a three-roll mill to obtain an electrode slurry with a fineness of less than 5 μm.
[0059] Embodiment 3
[0060] The electrode slurry provided in an embodiment of the present invention includes, by weight: 82 parts by weight of spherical silver powder (model: GS753, produced by Zhejiang Guangda Electronic Technology Co., Ltd.), 8 parts by weight of polyurethane (model: 5778, produced by Lubrizol Corporation), 3 parts by weight of 1,6-hexanediol diacrylate, 5 parts by weight of epoxy acrylate, 1 part by weight of 2-mercaptoethanol, and 1 part by weight of 1-hydroxy-cyclohexyl-phenyl ketone.
[0061] The method for preparing the electrode slurry provided in the third embodiment of the present invention comprises the following steps:
[0062] The first step is to prepare a modified silver-based conductive material: 82 parts by weight of commercially available spherical silver powder (model: GS753, produced by Zhejiang Guangda Electronic Technology Co., Ltd.) and 8 parts by weight of a polyurethane compound (model: 5778, produced by Lubrizol) are mixed and stirred evenly, the temperature is raised to 200°C, and the stirring is continued for 45 minutes. The temperature is lowered to obtain polyurethane-coated silver powder, i.e., the modified silver-based conductive material.
[0063] The second step is to prepare an organic carrier: 1,6-hexanediol diacrylate, epoxy acrylate (model: CN104NS, produced by Sartomer), 2-mercaptoethanol, and 1-hydroxy-cyclohexyl-phenyl ketone are mixed and stirred to obtain an organic carrier.
[0064] The third step is to prepare electrode slurry: the modified silver-based conductive material and the organic carrier mixture are mixed, stirred, and passed through a three-roll mill to obtain an electrode slurry with a fineness of less than 5 μm.
[0065] Embodiment 4
[0066] The electrode slurry provided by an embodiment of the present invention includes, by weight: 60 parts by weight of spherical silver powder, 23 parts by weight of flaky silver powder, 7 parts by weight of a polyurethane compound, 6 parts by weight of methyl methacrylate, 2 parts by weight of epoxy acrylate, 1 part by weight of 1,6-hexanedithiol and 1 part by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0067] The method for preparing the electrode slurry provided in the fourth embodiment of the present invention comprises the following steps:
[0068] The first step is to prepare a modified silver-based conductive material: 60 parts by weight of spherical silver powder, 23 parts by weight of flaky silver powder, 7 parts by weight of a polyurethane compound, 6 parts by weight of methyl methacrylate, 2 parts by weight of epoxy acrylate, 1 part by weight of 1,6-hexanedithiol and 1 part by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone are mixed and stirred evenly, the temperature is raised to 200°C, the stirring is continued at the temperature for 45 minutes, and the temperature is lowered to obtain polyurethane-coated silver powder, i.e., the modified silver-based conductive material.
[0069] The second step is to prepare an organic carrier: methyl methacrylate, epoxy acrylate, 1,6-hexanedithiol and 1 part by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone are mixed and stirred to obtain an organic carrier.
[0070] The third step is to prepare electrode slurry: add the modified silver-based conductive material to the above organic carrier and stir well, place the mixed electrode slurry on a three-roll mill for dispersion and grinding, and obtain electrode slurry.
[0071] Embodiment 5
[0072] The electrode slurry provided by an embodiment of the present invention includes, by weight: 65 parts by weight of spherical silver powder, 15 parts by weight of flaky silver powder, 10 parts by weight of a polyurethane compound, 6 parts by weight of butyl methacrylate, 2 parts by weight of epoxy acrylate, 1 part by weight of 1,6-hexanedithiol and 1 part by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0073] The method for preparing the electrode slurry provided in the fifth embodiment of the present invention comprises the following steps:
[0074] The first step is to prepare a modified silver-based conductive material: 65 parts by weight of spherical silver powder, 15 parts by weight of flaky silver powder, 10 parts by weight of a polyurethane compound, 6 parts by weight of butyl methacrylate, 2 parts by weight of epoxy acrylate, 1 part by weight of 1,6-hexanedithiol and 1 part by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone are mixed and stirred evenly, the temperature is raised to 200°C, the stirring is continued at the temperature for 45 minutes, and the temperature is lowered to obtain polyurethane-coated silver powder, i.e., the modified silver-based conductive material.
[0075] The second step is to prepare an organic carrier: butyl methacrylate, epoxy acrylate, 1,6-hexanedithiol and 1 part by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone are mixed and stirred to obtain an organic carrier.
[0076] The third step is to prepare electrode slurry: add the modified silver-based conductive material to the above organic carrier and stir well, place the mixed electrode slurry on a three-roll mill for dispersion and grinding, and obtain electrode slurry.
[0077] Embodiment 6
[0078] The electrode slurry provided by an embodiment of the present invention includes, by weight: 70 parts by weight of spherical silver powder, 20 parts by weight of flaky silver powder, 5 parts by weight of a polyurethane compound, 2 parts by weight of trimethylolpropane triacrylate, 1 part by weight of methyl methacrylate, 1 part by weight of N-acetylthiolactone and 1 part by weight of benzoin dimethyl ether.
[0079] The method for preparing the electrode slurry provided in the sixth embodiment of the present invention comprises the following steps:
[0080] The first step is to prepare a modified silver-based conductive material: 70 parts by weight of spherical silver powder, 20 parts by weight of flaky silver powder, 5 parts by weight of a polyurethane compound, 2 parts by weight of trimethylolpropane triacrylate, 1 part by weight of methyl methacrylate, 1 part by weight of N-acetylthiolactone and 1 part by weight of benzoin dimethyl ether are mixed and stirred evenly, the temperature is raised to 200° C., the stirring is continued at the temperature for 45 minutes, and the temperature is lowered to obtain polyurethane-coated silver powder, i.e., the modified silver-based conductive material.
[0081] The second step is to prepare an organic carrier: trimethylolpropane triacrylate, methyl methacrylate, N-acetylthiolactone and 1 part by weight of benzoin dimethyl ether are mixed and stirred evenly to obtain an organic carrier.
[0082] The third step is to prepare electrode slurry: add the modified silver-based conductive material to the above organic carrier and stir well, place the mixed electrode slurry on a three-roll mill for dispersion and grinding, and obtain electrode slurry.
[0083] Comparative Example 1
[0084] The electrode slurry of the comparative example of the present invention does not contain the modified silver-based conductive material of the present application.
[0085] The preparation method of the electrode slurry provided in the comparative example of the present invention comprises the following steps:
[0086] The first step is to prepare an organic carrier: 3 parts by weight of 1,6-hexanediol diacrylate, 5 parts by weight of epoxy acrylate (model: CN104NS, produced by Sartomer), 1 part by weight of 2-mercaptoethanol, and 1 part by weight of 1-hydroxy-cyclohexyl-phenyl ketone are mixed and stirred evenly to obtain an organic carrier.
[0087] The second step is to prepare electrode slurry: 90 parts by weight of spherical silver powder (model: GS753, produced by Zhejiang Guangda Electronic Technology Co., Ltd.) is added to the above organic carrier and stirred evenly, and the mixed electrode slurry is placed on a three-roll mill for dispersion and grinding to obtain electrode slurry.
[0088] Comparative Example 2
[0089] The electrode slurry of Comparative Example 2 of the present invention does not contain the modified silver-based conductive material of the present application.
[0090] The preparation method of the electrode slurry provided in Comparative Example 2 of the present invention comprises the following steps:
[0091] The first step is to prepare an organic carrier: 7 parts by weight of hydrogenated epoxy resin (model: HE2025, manufacturer: Shanghai Luohe High-tech Materials Co., Ltd.), 1 part by weight of dicyandiamide, and 2 parts by weight of diethylene glycol butyl ether acetate are mixed and stirred evenly to obtain an organic carrier.
[0092] The second step is to prepare the electrode slurry: 90 parts by weight of spherical silver powder (average particle size D50 = 1.5 μm, specific surface area 0.2 m 2 / g) add the above organic carrier and stir well, place the mixed electrode slurry on a three-roll mill for dispersion and grinding to obtain electrode slurry.
[0093] The preparation process of the heterojunction battery formed by the electrode slurry provided in the embodiment of the present invention is as follows:
[0094] The first step is to clean and texturize the silicon wafer.
[0095] The second step is amorphous silicon deposition: the intrinsic amorphous silicon film and the P-type amorphous silicon film are prepared by the amorphous silicon front PECVD method, and the intrinsic amorphous silicon film and the N-type amorphous silicon film are prepared by the back PECVD method.
[0096] The third step is to deposit a transparent conductive film by sputtering a transparent conductive oxide film on both sides.
[0097] The fourth step is screen printing low temperature curing electrode slurry.
[0098] The fifth step is to irradiate the electrode slurry with a mercury lamp with a power of 60 W / cm for no more than 1 min to obtain a heterojunction battery.
[0099] This example tests the performance of the low temperature curing conductive silver paste in Examples 1-3 and Comparative Examples 1-2. The specific results are shown in Table 1. The specific tests include:
[0100] 1. Viscosity test
[0101] The viscosity test was performed using a Brookfield viscometer at a speed of 10 revolutions per minute to test the viscosity value after 2 minutes.
[0102] 2. Contact resistivity test
[0103] A four-probe ohmmeter was used to test the contact resistivity between the gate line and the cell after curing.
[0104] 3. Adhesion test
[0105] Use 3M6100 tape to stick to the grid line at a 90° angle, press repeatedly with the index finger 3 times, pull the tape at a constant speed at 180°, and observe the grid line falling off.
[0106] 4. Electrical performance test
[0107] Solar simulator, 25°C, M1.5 spectrum, 1.000KW / m 2 .
[0108] The test results of the electrode slurries provided in Examples 1-3 of the present invention and Comparative Examples 1-2 are as follows:
[0109]
[0110] As can be seen from the above table, the heterojunction battery made of the electrode slurry in Examples 1 to 3 has a contact resistivity much lower than that of Comparative Examples 1 to 2 that do not contain modified silver-based conductive materials, and a conversion efficiency greater than that of Comparative Examples 1 to 2. At the same time, the grid lines formed by sintering the electrode slurry in the embodiments of the present invention are not easy to fall off. In other words, the grid lines formed by sintering the click slurry in the embodiments of the present invention have greatly improved bonding strength with the solar cell after curing, greatly reduced contact resistivity, better conversion efficiency, and are conducive to extending the service life of the cell.
[0111] The above is only a specific embodiment of the present invention. Obviously, various modifications and combinations can be made without departing from the spirit and scope of the present invention. Accordingly, this specification and the drawings are only exemplary illustrations of the present invention as defined by the attached claims, and are deemed to have covered any and all modifications, changes, combinations or equivalents within the scope of the present invention. Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is intended to include these changes and variations. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope of protection of the claims.
Claims
1. A method for preparing an electrode slurry, characterized in that: include: The silver-based conductive material and thermoplastic polyurethane are uniformly mixed and then heated to prepare a modified silver-based conductive material, wherein the glass transition temperature of the thermoplastic polyurethane is 50° C. to 150° C., the mass percentage of the thermoplastic polyurethane in the modified silver-based conductive material is 1% to 10%, the mass percentage of the silver-based conductive material in the modified silver-based conductive material is 90% to 99%, and the number average molecular weight of the thermoplastic polyurethane is 10000Da to 500000Da; An organic carrier is mixed with the modified silver-based conductive material to obtain an electrode slurry, wherein the organic carrier comprises a vinyl compound, a mercapto compound and a photoinitiator.
2. An electrode slurry prepared according to the method for preparing an electrode slurry according to claim 1, characterized in that: The invention comprises a modified silver-based conductive material and an organic carrier. The modified silver-based conductive material comprises a silver-based conductive material and thermoplastic polyurethane wrapped on the surface of the silver-based conductive material. The glass transition temperature of the thermoplastic polyurethane is 50°C to 150°C.
3. The electrode slurry according to claim 2, characterized in that: In terms of mass percentage, the modified silver-based conductive material accounts for 75% to 95% of the electrode slurry, and the organic carrier accounts for 5% to 25% of the electrode slurry.
4. The electrode slurry according to claim 2, characterized in that: In terms of mass percentage, the mass percentage of the thermoplastic polyurethane in the modified silver-based conductive material is 1% to 10%, and the mass percentage of the silver-based conductive material in the modified silver-based conductive material is 90% to 99%.
5. The electrode slurry according to claim 2, characterized in that: The thermoplastic polyurethane includes a polymer containing repeated urethane groups in its molecular structure and / or a modified polymer containing repeated urethane groups in its molecular structure.
6. The electrode slurry according to claim 2, characterized in that: The organic carrier comprises a vinyl compound, a thiol compound and a photoinitiator, and the mass ratio of the vinyl compound, the thiol compound and the photoinitiator is (75-90): (5-25): (1-10).
7. The electrode slurry according to claim 6, characterized in that: The vinyl compound includes at least one of a modified epoxy resin, a modified polyurethane resin, and an acrylate compound; The thiol compound includes at least one of 2-mercaptoethanol, 1,6-hexanedithiol and N-acetylthiolactone; The photoinitiator includes at least one of 1-hydroxy-cyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone and benzoin dimethyl ether.
8. The electrode slurry according to any one of claims 2 to 7, characterized in that: The particle size distribution D50 of the modified silver-based conductive material is 0.1 μm to 5 μm, and the specific surface area of the modified silver-based conductive material is less than 3 m 2 / g; The silver-based conductive material includes spherical silver powder and / or flaky silver powder.
9. An electrode sheet, characterized in that: The electrode sheet comprises the electrode slurry according to any one of claims 2 to 8.
10. A photovoltaic cell, characterized in that: The photovoltaic cell comprises the electrode sheet according to claim 9.