A graphene-conductive high electron mobility transistor logic circuit and its fabrication method

By forming a graphene layer on the diamond buffer layer and performing doping treatment, the problem of poor conductivity in diamond lateral HEMT devices was solved, achieving high electron mobility and improved stability, and enhancing the device's speed and material compatibility.

CN116544233BActive Publication Date: 2026-11-10SUZHOU MICROELECTRONICS IND TECH RES INST OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310573183.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2026-11-10
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

The poor conductivity of existing diamond lateral HEMT devices leaves room for improvement in the electron mobility of the two-dimensional electron gas.

Method used

A graphene layer is formed on a diamond buffer layer, and doped regions are formed through chemical vapor deposition and ion implantation. Combining the material advantages of diamond and graphene, a high electron mobility transistor logic circuit with graphene conductivity is fabricated.

Benefits of technology

This improved the carrier mobility of the device, overcame the limitations of the two-dimensional electron gas mobility in heterojunction HEMTs, enhanced the device speed and stability, reduced defects during fabrication, and improved material compatibility and device quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116544233B_ABST
    Figure CN116544233B_ABST
Patent Text Reader

Abstract

This invention discloses a graphene-conductive high electron mobility transistor logic circuit and its fabrication method. It includes an insulating substrate, a diamond buffer layer formed on either surface of the insulating substrate, and a first gate, a power electrode, and an output electrode formed on the other surface of the diamond buffer layer. It further includes: a graphene layer formed on the other surface of the diamond buffer layer; a second gate formed on the outer surface of the graphene layer; a first graphene modulation region and a second graphene modulation region formed on the graphene layer at locations corresponding to the first gate and the second gate, respectively; and a ground electrode formed on the outer surface of the graphene layer. This invention can achieve breakthroughs in the mobility of two-dimensional electron gas in heterojunction HEMTs, thereby improving device speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a HEMT device, specifically a high electron mobility transistor (HEMT) logic circuit, and more particularly to a graphene-conductive high electron mobility transistor logic circuit and its fabrication method. Background Technology

[0002] Diamond devices are outstanding representatives of ultra-wide bandgap semiconductors, possessing many characteristics that are difficult for other materials to match. They are mainly used for substrate heat dissipation and basic diamond diodes (which can be used to make lateral HEMT devices), and there is still relatively little development for subsequent devices.

[0003] Chinese invention patent application number 202211231907.X discloses a diamond-based lateral HEMT device and its manufacturing method. From bottom to top, it comprises an undoped insulating substrate, a buffer layer, an Al-diamond layer, and a source, gate, and drain electrode formed on the Al-diamond layer. The undoped insulating substrate and buffer layer are made of diamond. This device has a simple structure, simple manufacturing process, and low cost. Due to the good thermal conductivity of diamond, no additional heat dissipation device is needed, saving device and subsequent working module volume and increasing power density. However, the conductivity of this lateral HEMT device is poor, resulting in room for improvement in the electron mobility of the two-dimensional electron gas. Summary of the Invention

[0004] In view of this, the purpose of this invention is to overcome the shortcomings of the prior art and provide a graphene-conductive high electron mobility transistor logic circuit.

[0005] To achieve the aforementioned objectives, the technical solution adopted in this application includes: a graphene-conductive high electron mobility transistor logic circuit, comprising an insulating substrate, a diamond buffer layer formed on either surface of the insulating substrate, and a first gate, a power supply electrode, and an output electrode formed on the other surface of the diamond buffer layer, further comprising: A graphene layer is formed on another surface of the diamond buffer layer, and the first gate, the power electrode, and the output electrode are respectively formed on the outer surface of the graphene layer. The second gate is formed on the outer surface of the graphene layer; the graphene layer forms a first graphene modulation region and a second graphene modulation region at locations corresponding to the first gate and the second gate, respectively. A ground electrode is formed on the outer surface of the graphene layer.

[0006] Ideally, the graphene layer is formed by chemical vapor deposition with a deposition thickness of 0.1~0.3μm; the insulating substrate is an undoped diamond insulating substrate with a thickness of 300~500μm.

[0007] Ideally, the diamond buffer layer is made of a material with a doping concentration of 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 The N-type diamond material; the diamond buffer layer is formed by physical vapor deposition with a deposition thickness of 100~300μm, and the target material is diamond material with corresponding doping concentration.

[0008] Furthermore, the first graphene modulation region is an N-type doped region, and the first gate is turned on at a low level and turned off at a high level; the second graphene modulation region is a P-type doped region, and the second gate is turned off at a low level and turned on at a high level.

[0009] Furthermore, the doped element in the first graphene modulation region is P, and the doping concentration is 1×10⁻⁶. 15 cm -3 ~5×10 15 cm -3 The second graphene modulation region is doped with boron (B) at a concentration of 1 × 10⁻⁶. 15 cm -3 ~5×10 15 cm -3 .

[0010] Ideally, the deposited metals of the first gate and the second gate are independently Au, and the deposition method is physical vapor deposition with a deposition thickness of 5-10 μm; the first gate and the second gate are connected to form the inverter input terminal as gate control electrodes.

[0011] Another object of the present invention is to provide a method for fabricating the above-mentioned graphene-conductive high electron mobility transistor logic circuit, comprising the following steps: (a) A diamond buffer layer is deposited on any surface of an insulating substrate; (b) A graphene layer is deposited on the surface of the diamond buffer layer; (c) A first barrier layer is deposited on the outer surface of the graphene layer, a photoresist layer is coated on the first barrier layer, a portion of the photoresist layer is exposed, the photoresist at the exposed area is removed using a photolithography solution, and the first barrier layer is then etched to form at least one first via; subsequently, ion implantation is performed on the graphene layer through the first via to form a first graphene modulation region, and a gate metal is deposited above the first graphene modulation region to form a first gate; then the other areas of the photoresist layer are exposed, the photoresist at the exposed area is removed using a photolithography solution, and the other areas of the first barrier layer are then etched. (d) A second barrier layer is deposited on the outer surface of the graphene layer, a photoresist layer is coated on the second barrier layer, a portion of the photoresist layer is exposed, the photoresist at the exposed area is removed using a photolithography solution, and the second barrier layer is then etched to form at least one second via; subsequently, ion implantation is performed on the graphene layer through the second via to form a second graphene modulation region, and a gate metal is deposited above the second graphene modulation region to form a second gate; then the other areas of the photoresist layer are exposed, the photoresist at the exposed area is removed using a photolithography solution, and the other areas of the second barrier layer are then etched. (e) A third barrier layer is deposited on the outer surface of the graphene layer, a photoresist layer is coated on the third barrier layer, a portion of the photoresist layer is exposed, and the photoresist at the exposed area is removed using a photolithography solution to etch the third barrier layer to form multiple third vias; then, power, output, and ground electrodes are deposited on the graphene layer through the third vias to form power electrodes, output electrodes, and ground electrodes, respectively; then, the other areas of the photoresist layer are exposed, and the photoresist at the exposed area is removed using a photolithography solution to etch the other areas of the third barrier layer.

[0012] Optimally, in step (a), the insulating substrate is a diamond-undoped insulating substrate with a thickness of 300~500 μm; the diamond buffer layer is formed on the surface of the insulating substrate by physical vapor deposition, and its doping concentration is 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 The N-type diamond material is deposited with a thickness of 100~300μm, and the target material is diamond material with the corresponding doping concentration.

[0013] Further, in step (b), the graphene layer is formed on the surface of the diamond buffer layer by chemical vapor deposition, with a deposition thickness of 0.1~0.3μm.

[0014] Further, in step (c), the element implanted by the ions is P, and the doping type is N-type doping with a doping concentration of 1×10⁻⁶.15 cm -3 ~5×10 15 cm -3 The first gate is made of Au, deposited by physical vapor deposition, with a deposition thickness of 5-10 μm. In step (d), the element implanted is B, and the doping type is P-type doping with a doping concentration of 1×10⁻⁶. 15 cm -3 ~5×10 15 cm -3 The second gate is made of Au, deposited by physical vapor deposition, with a deposition thickness of 5-10 μm. In step (e), the power electrode, output electrode and ground electrode are independently Au, deposited by physical vapor deposition, with a deposition thickness of 5-10 μm.

[0015] This application presents a graphene-conductive high electron mobility transistor logic circuit. By adding a graphene layer and a second gate to the surface of a diamond buffer layer on an insulating substrate, the carrier mobility of the device at room temperature is approximately 15000 cm⁻¹. 2 / (V·s), under certain specific conditions (such as at low temperatures), the carrier mobility of the device can even reach as high as 250,000 cm⁻¹. 2 / (V·s) can break through the mobility of two-dimensional electron gas in heterojunction HEMT, thereby improving the device speed; moreover, diamond and graphene are both carbon-based materials, and the two materials have high compatibility, fewer defects during preparation, and high device quality.

[0016] The device's substrate and buffer layer are both made of diamond, a material with a large bandgap of 5.5 eV and a high thermal conductivity of 22 W / cm·K, offering significant material advantages that greatly enhance the heat dissipation and stability of HEMT devices. The first graphene modulation region is an N-type doped region, and the second graphene modulation region is a P-type doped region, complementing the first gate control region to achieve reverse output characteristics. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the high electron mobility transistor logic circuit with graphene conductivity of the present invention. Detailed Implementation

[0018] This invention discloses a graphene-conductive high electron mobility transistor logic circuit, comprising an insulating substrate, a diamond buffer layer formed on one surface of the insulating substrate, and a first gate, a power electrode, and an output electrode formed on the other surface of the diamond buffer layer. It further comprises: a graphene layer formed on the other surface of the diamond buffer layer; the first gate, the power electrode, and the output electrode respectively formed on the outer surface of the graphene layer; a second gate formed on the outer surface of the graphene layer; a first graphene modulation region and a second graphene modulation region formed on the graphene layer at locations corresponding to the first gate and the second gate, respectively; and a ground electrode formed on the outer surface of the graphene layer. By adding a graphene layer and a second gate on the surface of the diamond buffer layer on the insulating substrate, the carrier mobility of the device at room temperature is approximately 15000 cm⁻¹. 2 / (V·s) (Under certain specific conditions, the carrier mobility of the device can even reach 250,000 cm⁻¹) 2 Furthermore, the electron mobility of the device is less affected by temperature changes; at any temperature between 50 and 500 K, its electron mobility remains at 15000 cm⁻¹. 2 Approximately / (V·s). This breakthrough can improve the mobility of two-dimensional electron gas in heterojunction HEMTs, thereby increasing device speed; moreover, both diamond and graphene are carbon-based materials, exhibiting high compatibility, fewer defects during fabrication, and high device quality.

[0019] The graphene layer is formed by chemical vapor deposition, with a deposition thickness of 0.1~0.3 μm; the insulating substrate is an undoped diamond insulating substrate with a thickness of 300~500 μm. The diamond buffer layer is made of a material with a doping concentration of 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 The material used is N-type diamond; the diamond buffer layer is formed by physical vapor deposition with a thickness of 100~300μm, and the target material is diamond material with a corresponding doping concentration. Diamond material has a large bandgap of 5.5eV and a high thermal conductivity of 22W / cm▪K, which are excellent material advantages. These advantages significantly improve the heat dissipation characteristics and stability of HEMT devices. Diamond's good thermal conductivity eliminates the need for additional heat dissipation devices, saving device and subsequent working module volume and increasing power density. Both diamond and graphene are carbon-based materials, exhibiting high compatibility, fewer defects during fabrication, and high device quality.

[0020] The first graphene modulation region is an N-type doped region, with the first gate being on at a low level and off at a high level; the second graphene modulation region is a P-type doped region, with the second gate being off at a low level and on at a high level; that is, the first gate is N-type doped (P-type transistor), with the P-type transistor being on at a low level and off at a high level; the second gate is P-type doped (N-type transistor), with the N-type transistor being off at a low level and on at a high level. The doped element in the first graphene modulation region is P, with a doping concentration of 1 × 10⁻⁶. 15 cm -3 ~5×10 15 cm -3 The second graphene modulation region is doped with boron (B) at a concentration of 1 × 10⁻⁶. 15 cm -3 ~5×10 15 cm -3 The first and second graphene modulation regions complement each other to form the reverse output characteristic.

[0021] The deposited metals of the first gate and the second gate are independently Au, and the deposition method is physical vapor deposition with a deposition thickness of 5-10 μm; the first gate and the second gate are connected to form the inverter input terminal as gate control electrodes.

[0022] The fabrication method of the graphene-conductive high electron mobility transistor logic circuit includes the following steps: (a) depositing a diamond buffer layer on any surface of an insulating substrate; (b) depositing a graphene layer on the surface of the diamond buffer layer; (c) depositing a first barrier layer on the outer surface of the graphene layer, coating a photoresist layer on the first barrier layer, exposing a portion of the photoresist layer, removing the photoresist at the exposed area using a photolithography solution, and then etching the first barrier layer to form at least one first via; subsequently, ion implanting the graphene layer through the first via to form a first graphene modulation region, depositing a gate metal above the first graphene modulation region to form a first gate; then exposing other areas of the photoresist layer, removing the photoresist at the exposed area using a photolithography solution, and then etching other areas of the first barrier layer; (d) depositing a second barrier layer on the outer surface of the graphene layer, coating a photoresist layer on the second barrier layer, and exposing a portion of the photoresist layer... Exposure is performed in sections, and the photoresist at the exposed areas is removed using a photolithography solution to etch the second barrier layer and form at least one second via. Then, ion implantation is performed on the graphene layer through the second via to form a second graphene modulation region, and gate metal is deposited on the second graphene modulation region to form a second gate. Then, the other areas of the photoresist layer are exposed, and the photoresist at the exposed areas is removed using a photolithography solution to etch the other areas of the second barrier layer. (e) A third barrier layer is deposited on the outer surface of the graphene layer, and a photoresist layer is coated on the third barrier layer. A portion of the photoresist layer is exposed, and the photoresist at the exposed areas is removed using a photolithography solution to etch the third barrier layer and form multiple third vias. Then, power, output, and ground electrodes are deposited on the graphene layer through the third vias to form power electrodes, output electrodes, and ground electrodes, respectively. Then, the other areas of the photoresist layer are exposed, and the photoresist at the exposed areas is removed using a photolithography solution to etch the other areas of the third barrier layer.

[0023] In step (a), the insulating substrate is an undoped diamond insulating substrate with a thickness of 300~500μm; the diamond buffer layer is formed on the surface of the insulating substrate by physical vapor deposition, and its doping concentration is 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 The N-type diamond material is deposited with a thickness of 100~300 μm, and the target material is diamond material with a corresponding doping concentration. In step (b), the graphene layer is formed on the surface of the diamond buffer layer by chemical vapor deposition with a deposition thickness of 0.1~0.3 μm. In step (c), the ion implanted element is P, and its doping type is N-type doping with a doping concentration of 1×10⁻⁶.15 cm -3 ~5×10 15 cm -3 The first gate is Au, deposited by physical vapor deposition with a thickness of 5-10 μm; in step (d), the ion implanted element is B, doped with P-type doping at a concentration of 1 × 10⁻⁶. 15 cm -3 ~5×10 15 cm -3 The second gate is Au, deposited by physical vapor deposition, with a deposition thickness of 5-10 μm; in step (e), the power electrode, output electrode and ground electrode are independently Au, deposited by physical vapor deposition, with a deposition thickness of 5-10 μm.

[0024] The present invention will be further described below with reference to the embodiments shown in the accompanying drawings. Example 1

[0025] This embodiment provides a graphene-conductive high electron mobility transistor logic circuit and its fabrication method, as detailed below: (a) A diamond buffer layer is deposited on the surface of an insulating substrate (an undoped diamond insulating substrate with a thickness of 300 μm); the diamond buffer layer is formed on the surface of the insulating substrate by physical vapor deposition (controlled parameters: atmospheric pressure of 12 MPa, incident angle of 30°, and target material of diamond material with the required doping concentration), with a doping concentration of 3 × 10⁻⁶. 17 cm -3 N-type diamond material, with a deposition thickness of 100 μm; (b) A graphene layer is deposited on the surface of the diamond buffer layer; specifically, the graphene layer is formed on the surface of the diamond buffer layer by chemical vapor deposition (CVD) at atmospheric pressure of 0.9 MPa and temperature of 400 °C, with a deposition thickness of 0.1 μm. (c) A first barrier layer (50 nm thick silicon dioxide) is deposited on the outer surface of the graphene layer. Photoresist (Zhongxin Qiheng SU-8 2000, 100 nm) is coated on the first barrier layer to form a layer photoresist. A portion of the photoresist layer (to form at least one first via in subsequent steps; in this embodiment, one via is used, the same below) is exposed (UV exposure for 10 s). The photoresist at the exposed area is removed using a photolithography solution (xylene) to etch the first barrier layer and form at least one first via. Subsequently, ion implantation is performed on the graphene layer through the first via (the ion implanted element is P, the doping type is N-type doping, and the doping concentration is 1 × 10⁻⁶). 15 cm -3A first graphene modulation region is formed, and a gate metal is deposited on top of the first graphene modulation region to form a first gate (the first gate is Au, and the deposition method is physical vapor deposition (atmospheric pressure is 12MPa, incident angle is 30°, and deposition thickness is 5μm, the same below); then the other areas of the photoresist layer are exposed, and the photoresist at the exposed area is removed by using a photolithography solution, thereby etching the other areas of the first barrier layer to remove the photoresist layer and the first barrier layer. (d) A second barrier layer (50 nm thick silicon dioxide) is deposited on the outer surface of the graphene layer. A photoresist layer (Zhongxin Qiheng SU-8 2000, 100 nm) is coated on the second barrier layer. A portion of the photoresist layer (to form at least one second via in subsequent steps) is exposed (UV exposure for 10 s). The photoresist at the exposed area is removed using a photolithography solution (xylene), thereby etching the second barrier layer to form at least one second via. Subsequently, ion implantation is performed on the graphene layer through the second via (the ion implanted element is B, the doping type is P-type doping, and the doping concentration is 1 × 10⁻⁶). 15 cm -3 A second graphene modulation region is formed, and a gate metal is deposited on top of the second graphene modulation region to form a second gate (the second gate is Au, the deposition method is physical vapor deposition, and the deposition thickness is 5μm); then the other areas of the photoresist layer are exposed, and the photoresist at the exposed area is removed by using a photolithography solution, thereby etching the other areas of the second barrier layer to remove the photoresist layer and the second barrier layer. (e) A third barrier layer (50 nm thick silicon dioxide) is deposited on the outer surface of the graphene layer. A photoresist layer (Zhongxin Qiheng SU-8 2000, 100 nm) is coated on the third barrier layer. A portion of the photoresist layer (to form multiple third vias in subsequent steps) is exposed (UV exposure for 10 s). The photoresist at the exposed area is removed using a photolithography solution (xylene), and the third barrier layer is then etched to form multiple third vias. Subsequently, power, output, and ground electrodes are deposited on the graphene layer through the third vias to form power electrodes, output electrodes, and ground electrodes (the power electrodes, output electrodes, and ground electrodes are independently Au, deposited by physical vapor deposition, with a deposition thickness of 5 μm; at an atmospheric pressure of 12 MPa and an incident angle of 30°). The other areas of the photoresist layer are then exposed, and the photoresist at the exposed area is removed using a photolithography solution, and the other areas of the third barrier layer are then etched. Example 2

[0026] This embodiment provides a graphene-conductive high electron mobility transistor logic circuit and its fabrication method, which is basically the same as that in Embodiment 1, except that: In step (a), the thickness of the undoped diamond insulating substrate is 500 μm, and the doping concentration of the diamond buffer layer is 1 × 10⁻⁶. 17cm -3 N-type diamond material, with a deposition thickness of 300 μm; In step (b), the deposition thickness of the graphene layer is 0.3 μm; In step (c), ion implantation is performed on the graphene layer through the first via. The implanted element is P, and the doping type is N-type doping with a doping concentration of 5 × 10⁻⁶. 15 cm -3 The deposition thickness of the first gate is 10 μm; In step (d), ion implantation is performed on the graphene layer through the second via. The implanted element is boron, and the doping type is N-type doping with a doping concentration of 5 × 10⁻⁶. 15 cm -3 The deposition thickness of the first gate is 10 μm; In step (e), the power supply, output, and ground electrodes are deposited through the third through-hole to form the power supply electrode, output electrode, and ground electrode (the power supply electrode, output electrode, and ground electrode are independently Au, the deposition method is physical vapor deposition, and the deposition thickness is 10 μm). Example 3

[0027] This embodiment provides a graphene-conductive high electron mobility transistor logic circuit and its fabrication method, which is basically the same as that in Embodiment 1, except that: In step (a), the thickness of the undoped diamond insulating substrate is 400 μm, and the doping concentration of the diamond buffer layer is 3 × 10⁻⁶. 17 cm -3 N-type diamond material, with a deposition thickness of 200 μm; In step (b), the deposition thickness of the graphene layer is 0.2 μm; In step (c), ion implantation is performed on the graphene layer through the first via. The implanted element is P, and the doping type is N-type doping with a doping concentration of 3 × 10⁻⁶. 15 cm -3 The deposition thickness of the first gate is 8 μm; In step (d), ion implantation is performed on the graphene layer through the second via. The implanted element is boron, and the doping type is N-type doping with a doping concentration of 3 × 10⁻⁶. 15 cm -3 The deposition thickness of the first gate is 8 μm; In step (e), the power supply, output, and ground electrodes are deposited through the third through-hole to form the power supply electrode, output electrode, and ground electrode (the power supply electrode, output electrode, and ground electrode are independently Au, the deposition method is physical vapor deposition, and the deposition thickness is 8 μm).

[0028] Comparative Example 1 This example provides a high electron mobility transistor logic circuit that is basically the same as that in Example 1, except that it does not contain a graphene layer.

[0029] Comparative Example 2 This example provides a high electron mobility transistor logic circuit that is basically the same as that in Example 1, except that it does not contain a first graphene modulation region.

[0030] Comparative Example 3 This example provides a high electron mobility transistor logic circuit that is basically the same as that in Example 1, except that it does not contain a second graphene modulation region.

[0031] Diamond insulating substrates provide support for devices, and the thicker the substrate, the stronger the structural strength of the device. Diamond buffer layers of 100 μm and above have almost no effect on device characteristics. The thicker the graphene deposition layer, the stronger the current carrying capacity of the device.

[0032] The product in Example 1 has a stronger current capability, faster response speed, and stronger driving capability; the product in Example 2 is more energy-efficient, but has a weaker current capability, slower response speed, and weaker driving capability; the product in Example 3 has performance between that of the products in Example 1 and Example 2. The products in Comparative Examples 2 and 3 have lower current capabilities than the product in Example 1, higher on-resistance, and higher power consumption; Comparative Example 1 has the weakest current capability, the highest on-resistance, and the highest power consumption.

[0033] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A graphene-conductive high electron mobility transistor logic circuit, comprising an insulating substrate, a diamond buffer layer formed on either surface of the insulating substrate, and a first gate, a power supply electrode, and an output electrode formed on the other surface of the diamond buffer layer, characterized in that, It also includes: A graphene layer is formed on another surface of the diamond buffer layer, and the first gate, the power electrode, and the output electrode are respectively formed on the outer surface of the graphene layer. The second gate is formed on the outer surface of the graphene layer; the graphene layer forms a first graphene modulation region and a second graphene modulation region at locations corresponding to the first gate and the second gate, respectively. Ground electrode, which is formed on the outer surface of the graphene layer; The graphene layer is formed by chemical vapor deposition, with a deposition thickness of 0.1~0.3μm; the insulating substrate is an undoped diamond insulating substrate with a thickness of 300~500μm. The diamond buffer layer is made of a material with a doping concentration of 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 The N-type diamond material; the diamond buffer layer is formed by physical vapor deposition with a deposition thickness of 100~300μm, and the target material is diamond material with corresponding doping concentration.

2. The graphene-conductive high electron mobility transistor logic circuit according to claim 1, characterized in that: The first graphene modulation region is an N-type doped region, and the first gate is turned on at a low level and turned off at a high level; the second graphene modulation region is a P-type doped region, and the second gate is turned off at a low level and turned on at a high level.

3. The graphene-conductive high electron mobility transistor logic circuit according to claim 2, characterized in that: The first graphene modulation region is doped with P at a concentration of 1×10⁻⁶. 15 cm -3 ~5×10 15 cm -3 The second graphene modulation region is doped with boron (B) at a concentration of 1 × 10⁻⁶. 15 cm -3 ~5×10 15 cm -3 .

4. The graphene-conductive high electron mobility transistor logic circuit according to claim 1, characterized in that: The deposited metals of the first gate and the second gate are independently Au, and the deposition method is physical vapor deposition with a deposition thickness of 5-10 μm; the first gate and the second gate are connected to form the inverter input terminal as gate control electrodes.

5. A method for fabricating a graphene-conductive high electron mobility transistor logic circuit, characterized in that, Includes the following steps: (a) A diamond buffer layer is deposited on any surface of an insulating substrate; (b) A graphene layer is deposited on the surface of the diamond buffer layer; (c) A first barrier layer is deposited on the outer surface of the graphene layer, a photoresist layer is coated on the first barrier layer, a portion of the photoresist layer is exposed, the photoresist at the exposed area is removed using a photolithography solution, and the first barrier layer is then etched to form at least one first via; subsequently, ion implantation is performed on the graphene layer through the first via to form a first graphene modulation region, and a gate metal is deposited above the first graphene modulation region to form a first gate; then the other areas of the photoresist layer are exposed, the photoresist at the exposed area is removed using a photolithography solution, and the other areas of the first barrier layer are then etched. (d) A second barrier layer is deposited on the outer surface of the graphene layer, a photoresist layer is coated on the second barrier layer, a portion of the photoresist layer is exposed, the photoresist at the exposed area is removed using a photolithography solution, and the second barrier layer is then etched to form at least one second via; subsequently, ion implantation is performed on the graphene layer through the second via to form a second graphene modulation region, and a gate metal is deposited above the second graphene modulation region to form a second gate; then the other areas of the photoresist layer are exposed, the photoresist at the exposed area is removed using a photolithography solution, and the other areas of the second barrier layer are then etched. (e) A third barrier layer is deposited on the outer surface of the graphene layer, a photoresist layer is coated on the third barrier layer, a portion of the photoresist layer is exposed, and the photoresist at the exposed area is removed using a photolithography solution to etch the third barrier layer to form multiple third vias; then, power, output, and ground electrodes are deposited on the graphene layer through the third vias to form power electrodes, output electrodes, and ground electrodes, respectively; then, the other areas of the photoresist layer are exposed, and the photoresist at the exposed area is removed using a photolithography solution to etch the other areas of the third barrier layer.

6. The method for fabricating the graphene-conductive high electron mobility transistor logic circuit according to claim 5, characterized in that: In step (a), the insulating substrate is an undoped diamond insulating substrate with a thickness of 300~500μm; the diamond buffer layer is formed on the surface of the insulating substrate by physical vapor deposition, and its doping concentration is 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 The N-type diamond material is deposited with a thickness of 100~300μm, and the target material is diamond material with the corresponding doping concentration.

7. The method for fabricating a graphene-conductive high electron mobility transistor logic circuit according to claim 5 or 6, characterized in that: In step (b), the graphene layer is formed on the surface of the diamond buffer layer by chemical vapor deposition, and the deposition thickness is 0.1~0.3μm.

8. The method for fabricating the graphene-conductive high electron mobility transistor logic circuit according to claim 5, characterized in that: In step (c), the element implanted by the ions is P, and the doping type is N-type doping with a doping concentration of 1×10⁻⁶. 15 cm -3 ~5×10 15 cm -3 The first gate is made of Au, deposited by physical vapor deposition, with a deposition thickness of 5-10 μm. In step (d), the element implanted is B, and the doping type is P-type doping with a doping concentration of 1×10⁻⁶. 15 cm -3 ~5×10 15 cm -3 The second gate is made of Au, deposited by physical vapor deposition, with a deposition thickness of 5-10 μm. In step (e), the power electrode, output electrode and ground electrode are independently Au, deposited by physical vapor deposition, with a deposition thickness of 5-10 μm.

Citation Information

Patent Citations

  • A diamond-based lateral HEMT device and method of manufacturing the same

    CN115440812B

  • Complementary logical gate device

    CN102113114A

  • High-mobility transistor and preparation method thereof

    CN106783997A

  • Diamond-based transverse HEMT device and manufacturing method thereof

    CN115440812A