A microcrystalline permeable plate and its processing method

By using waste ceramic tile particles and feldspar particles as raw materials, combined with high-temperature sintering and secondary material pressing technology, the problems of monotonous appearance and easy clogging of permeable bricks have been solved, resulting in microcrystalline permeable boards with good permeability, strong weather resistance, and rich colors, which are suitable for sponge city construction.

CN116572598BActive Publication Date: 2026-11-17FANGNUO (YIXING) NEW MATERIAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310394398.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2026-11-17
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

Existing permeable bricks have limited color and texture options, making it difficult to meet decorative needs. Furthermore, traditional permeable bricks are prone to clogging and lack sufficient weather resistance.

Method used

Using waste ceramic tile particles, sodium feldspar particles, and potassium sodium feldspar particles as the main raw materials, microcrystalline permeable boards are formed through high-temperature sintering. The natural colors and fine processing of various feldspar particles create rich colors and textures, and a secondary fabric pressing technology is used to ensure unobstructed water channels.

Benefits of technology

The microcrystalline permeable board has a dense pore surface, excellent water permeability, is not easily clogged, has strong weather resistance, rich colors, good decorative properties and flexural strength. The water permeability coefficient reaches 2.0~3.0×10-2, and the flexural strength reaches 5.5~7.0MPa, which fully meets the national standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116572598B_ABST
    Figure CN116572598B_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of permeable panels, specifically relating to a microcrystalline permeable panel and its processing method. The microcrystalline permeable panel comprises one or more of a base material and a surface material; the base material comprises waste ceramic tile particles, an adhesive, a fluxing agent, and water; the surface material comprises albite particles, potassium-sodium feldspar particles, a fluxing agent, an adhesive, water, and a colorant; the albite particles contain 3-12% sodium; the potassium-sodium feldspar particles contain 3-12% potassium and 3-12% sodium; after high-temperature sintering, a microcrystalline permeable panel with dense pores, good permeability, high strength and stability, and strong weather resistance is produced, with a flexural strength of 5.5-7.0 MPa and a permeability coefficient of 2.0-3.0 × 10⁻⁶. ‑2 Furthermore, it has good frost resistance, excellent weather resistance and anti-aging ability, and fully meets national standards.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of permeable panels, specifically relating to a microcrystalline permeable panel and its processing method. Background Technology

[0002] With the nation's vigorous promotion of sponge city construction, a series of permeable brick products has emerged. The development from cement-bonded permeable bricks to sintered ceramic permeable bricks has significantly altered the chemical and physical properties of the products. For example, product strength and weather resistance have been greatly improved. However, this product series has been hampered by its limited variety of colors and textures. Therefore, continued efforts are needed to enhance the performance of permeable bricks and enrich their appearance, colors, and textures, so that permeable bricks not only possess permeability but also significant decorative functions, thus expanding their applications.

[0003] The applicant of this invention previously filed a patent CN202010136107.4 for a permeable granite-like panel and its processing method, which disclosed that the permeable panel is made by layering base material and fabric material, and then pressing and vitrifying sintering to form a dense permeable structure. Summary of the Invention

[0004] To address the above problems, the present invention aims to provide a microcrystalline permeable board and its processing method, forming a microcrystalline permeable board with a compact structure, permeability, and weather resistance.

[0005] The technical content of this invention is as follows:

[0006] The present invention provides a microcrystalline permeable board, wherein the microcrystalline permeable board comprises one or more of a base material and a surface material;

[0007] The base material comprises waste ceramic tile particles, binder, flux, and water. By mass fraction, with the amount of waste ceramic tile particles as unit 1, the binder accounts for 1-15 wt%, the flux accounts for 1-10 wt%, and the water accounts for 1-10 wt%.

[0008] The fabric is composed of sodium feldspar particles, potassium sodium feldspar particles, a solvent, a binder, water, and a colorant. By mass fraction, with the amount of sodium feldspar particles and potassium sodium feldspar particles as a unit, the solvent accounts for 1-10 wt%, the binder accounts for 1-15 wt%, the water accounts for 3-10 wt%, and the colorant accounts for 0-10 wt%.

[0009] The albite particles contain 3-12% sodium;

[0010] The potassium-sodium feldspar particles contain 3-12% potassium and 3-12% sodium.

[0011] The adhesive includes bentonite or other inorganic salt adhesives;

[0012] The fluxing agent includes glass powder and frit powder.

[0013] The present invention also provides a method for processing a microcrystalline permeable plate, comprising the following steps:

[0014] Prepare the base material and the outer material separately;

[0015] A) Press, calcine, and cool the fabric to obtain a microcrystalline permeable plate with a single layer structure.

[0016] B) Combine the base material and the fabric material, press, calcine, and cool to obtain a two-layer microcrystalline permeable board.

[0017] The pressing process employs a two-stage material feeding method. The press feeding trolley pushes the base material and the outer material into the mold according to a set thickness to form an overlapping state, and then presses them. Specifically, the prepared outer material and base material are transported to the hopper of the press feeding trolley. Then, the feeding trolley first pushes the base material into the mold according to a set thickness, and then the outer material is laid on top of the base material according to a set thickness to form an overlapping state, and then it can be pressed into shape.

[0018] The calcination temperature is 1000–1200℃;

[0019] Preparation of the base material: Waste ceramic tile particles, adhesive, co-solvent and water are mixed and stirred evenly to obtain the base material;

[0020] Preparation of the fabric material: Select 6 to 10 kinds of natural sodium feldspar and potassium sodium feldspar with different colors, and crush, ball mill, wash, dry and sieve them respectively to obtain sodium feldspar and potassium sodium feldspar particles with D50 of 0.2 to 0.3 mm. Mix sodium feldspar and potassium sodium feldspar particles, solvent, binder, water and colorant evenly to obtain the fabric.

[0021] The beneficial effects of this invention are as follows:

[0022] The microcrystalline permeable board of this invention is composed of tiny crystalline particles. After high-temperature sintering, it forms a large number of fine, even micro-sized, crystals that sparkle under sunlight or artificial light. These crystalline particles are small and rounded, resulting in a densely porous surface layer on the permeable board, providing excellent water permeability, preventing clogging, and facilitating cleaning. It also exhibits exceptional weather resistance, unlike traditional sand-based bricks which suffer from discoloration and peeling due to changes in sunlight, temperature, and weather. Conventional permeable bricks have a coarser surface texture and more noticeable pores between particles, making them more prone to clogging in the presence of sand, mud, or rainwater. The surface material used is albite and potassium-sodium feldspar. The mixture better utilizes the different melting states of the two feldspar particles during high-temperature firing, allowing the fabric and base material to fuse better while preventing excessive melting, thus keeping the permeable channels unobstructed and abundant. It also selects 6-10 different naturally colored sodium feldspar and potassium sodium feldspar ores, with natural colors including white, yellow, black, gray, brown, red, and other feldspars that develop different colors with heat. Through special fine processing, these colorful feldspar particles have a multi-layered particle size distribution, making their texture more layered and richer in color than most natural granite textures.

[0023] The processing method of the microcrystalline permeable board of the present invention first involves crushing feldspar material, gravity friction ball milling, washing, drying, and grading and sieving to obtain fine particles for batching. Then, the material is sintered at high temperature to produce a microcrystalline permeable board with dense pores, good permeability, high strength, good stability, and strong weather resistance. The flexural strength can reach 5.5–7.0 MPa, and the permeability coefficient can reach 2.0–3.0 × 10⁻⁶. -2 Furthermore, it has good frost resistance, excellent weather resistance and anti-aging ability, and fully meets national standards. Attached Figure Description

[0024] Figure 1 The microcrystalline permeable plate prepared in Example 1;

[0025] Figure 2 The microcrystalline permeable plate prepared in Example 2;

[0026] Figure 3 The microcrystalline permeable plate prepared in Example 3;

[0027] Figure 4 The microcrystalline permeable plate prepared in Example 4;

[0028] Figure 5 The microcrystalline permeable plate prepared in Example 5;

[0029] Figure 6 This is a comparison diagram of Example 1 and permeable ceramic bricks. Detailed Implementation

[0030] The present invention will be further described in detail below through specific implementation examples and accompanying drawings. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of protection of the present invention. After reading the present invention, any modifications of the present invention in various equivalent forms by those skilled in the art fall within the scope of the appended claims.

[0031] Unless otherwise specified, all raw materials and reagents used in this invention are from the conventional market.

[0032] Example 1

[0033] Preparation of a microcrystalline permeable plate

[0034] 1) Fabric material preparation: Select albite containing 3-12% sodium and potassium-sodium feldspar containing 3-12% sodium. Choose 6-10 different naturally colored albite and potassium-sodium feldspar (white, black, gray, yellow, brown, red, and coffee-colored), and process them separately as follows:

[0035] a) Crushing: The purchased sodium feldspar and potassium sodium feldspar are of different sizes and shapes, and need to be crushed in three stages: coarse crushing, fine crushing and fine crushing. At the same time, various particle sizes are screened out using 10 mesh, 16 mesh, 30 mesh, 40 mesh, 60 mesh, 80 mesh, 100 mesh and 120 mesh sieves, and finally particles with a particle size distribution of 16 to 120 mesh are selected.

[0036] b) Ball milling: Feldspar particles between 16 and 120 mesh are ball milled (without balls in the ball mill). The particles collide and rub against each other by their own gravity, which removes the burrs and sharp edges formed during the crushing process, making them relatively smooth. The finished product is like sand on a beach. The process takes about 0.5 to 3 hours.

[0037] c) Washing and drying: The finished particles after gravity friction ball milling are transported to a washing tank, where water is added and stirred to wash away the mud and dust. After dehydration by a dewatering machine (the moisture content of the particles after dehydration is 5-10%), they are transported to the drying process. The moisture content of the particles is dried to below 2% by a dryer. Finally, the dried particles are transported to an air classifier to remove dust smaller than 120 mesh. What remains are the feldspar particles in the range of 16-120 mesh required for microcrystalline permeable panels. The resulting feldspar particles have a diameter D50 of 0.2-0.3 mm, with a fine appearance and smooth feel.

[0038] Take 1 part of the treated sodium feldspar particles and potassium sodium feldspar particles (mixing mass ratio of 2:1), add 5 wt% co-solvent (glass powder), 6 wt% binder, 8 wt% water and 3 wt% colorant and mix to obtain fabric material;

[0039] 2) Preparation of microcrystalline permeable panels: The fabric material is fed into the press hopper and pressed into shape through a secondary pressing process. It is then sent to a kiln for high-temperature sintering at 1000–1200℃. After firing and cooling, a microcrystalline permeable panel (one-layer structure) with densely packed fine crystalline particles on its surface is produced. Figure 1 As shown;

[0040] The pigment is used to formulate the main color tone of the permeable panel according to requirements.

[0041] Example 2

[0042] Preparation of a microcrystalline permeable plate

[0043] 1) Preparation of fabric materials: Select sodium feldspar containing 3-12% sodium and potassium sodium feldspar containing 3-12% potassium and 3-12% sodium. Select 6-10 kinds of sodium feldspar and potassium sodium feldspar with different natural colors (white, black, gray, yellow, brown, red and coffee). The treatment is the same as in Example 1.

[0044] Take 1 part of the treated sodium feldspar particles and potassium sodium feldspar particles (mixing mass ratio of x:x), add 8wt% co-solvent, 10wt% binder, 4wt% water and 2wt% colorant and mix to obtain fabric material;

[0045] 2) Preparation of microcrystalline permeable panels: The fabric material is fed into the press hopper and pressed into shape through a secondary pressing process. It is then sent to a kiln for high-temperature sintering at 1000–1200℃. After firing and cooling, a microcrystalline permeable panel (one-layer structure) with densely packed fine crystalline particles on its surface is produced. Figure 2 As shown.

[0046] Example 3

[0047] Preparation of a microcrystalline permeable plate

[0048] 1) Preparation of base material: Take 1 part of waste ceramic tile particles, add 4wt% adhesive, 5wt% flux (glass powder) and 7wt% water, and stir evenly to obtain the base material;

[0049] 2) Preparation of fabric materials: Select sodium feldspar containing 3-12% sodium and potassium sodium feldspar containing 3-12% potassium and 3-12% sodium. Select 6-10 different natural colors (white, black, gray, yellow, brown, red and coffee) of sodium feldspar and potassium sodium feldspar, and treat them in the same way as in Example 1.

[0050] The treated sodium feldspar particles and potassium sodium feldspar particles (mixed in a mass ratio of 1:1) are mixed with 2wt% co-solvent, 3wt% binder, 5wt% water and 2wt% colorant, and stirred evenly to obtain the fabric material.

[0051] 2) Preparation of microcrystalline permeable panels: One portion is fed into the press hopper and pressed into shape through secondary material distribution. It is then sent to a kiln for high-temperature sintering at 1000–1200℃. After firing and cooling, a microcrystalline permeable panel (two-layer structure) with densely packed fine crystalline particles on its surface is produced. Figure 3 As shown.

[0052] Example 4

[0053] Preparation of a microcrystalline permeable plate

[0054] 1) Preparation of base material: Take 1 part of waste ceramic tile particles, add 15wt% adhesive, 10wt% flux (glass powder) and 10wt% water, and stir evenly to obtain the base material;

[0055] 2) Preparation of fabric materials: Select sodium feldspar containing 3-12% sodium and potassium sodium feldspar containing 3-12% potassium and 3-12% sodium. Select 6-10 different natural colors (white, black, gray, yellow, brown, red and coffee) of sodium feldspar and potassium sodium feldspar, and treat them in the same way as in Example 1.

[0056] The treated sodium feldspar particles and potassium sodium feldspar particles (mixed in a mass ratio of 3:1) are mixed with 10wt% co-solvent, 15wt% binder, 10wt% water and 10wt% colorant, and stirred evenly to obtain the fabric material.

[0057] 2) Preparation of microcrystalline permeable panels: One portion is fed into the press hopper and pressed into shape through secondary material distribution. It is then sent to a kiln for high-temperature sintering at 1000–1200℃. After firing and cooling, a microcrystalline permeable panel (two-layer structure) with densely packed fine crystalline particles on its surface is produced. Figure 4 As shown.

[0058] Example 5

[0059] Preparation of a microcrystalline permeable plate

[0060] 1) Preparation of base material: Take 1 part of waste ceramic tile particles, add 1 wt% adhesive, 1 wt% flux (glass powder) and 1 wt% water, and stir evenly to obtain the base material;

[0061] 2) Preparation of fabric materials: Select sodium feldspar containing 3-12% sodium and potassium sodium feldspar containing 3-12% potassium and 3-12% sodium. Select 6-10 different natural colors (white, black, gray, yellow, brown, red and coffee) of sodium feldspar and potassium sodium feldspar, and treat them in the same way as in Example 1.

[0062] The treated sodium feldspar particles and potassium sodium feldspar particles (mixed in a mass ratio of 4:1) are mixed with 1 wt% co-solvent, 1 wt% binder and 3 wt% water, and stirred evenly to obtain the fabric material.

[0063] 2) Preparation of microcrystalline permeable panels: One portion is fed into the press hopper and pressed into shape through secondary material distribution. It is then sent to a kiln for high-temperature sintering at 1000–1200℃. After firing and cooling, a microcrystalline permeable panel (two-layer structure) with densely packed fine crystalline particles on its surface is produced. Figure 5 As shown.

[0064] The performance of the microcrystalline permeable plate prepared above was tested, and the results are as follows:

[0065] Table 1 Performance test results of microcrystalline permeable panels

[0066]

[0067]

[0068] As shown in Table 1, the microcrystalline permeable bricks prepared by this invention exhibit excellent performance in terms of flexural strength, permeability, and frost resistance, fully meeting national standards, and also demonstrating superior weather resistance and anti-aging capabilities.

[0069] The performance of the microcrystalline permeable plate of the present invention was compared with that of the ceramic permeable brick (based on the ceramic permeable brick prepared by in-situ generation of high-temperature binder and its preparation method, as described in patent CN201410061365.5 of Jingdezhen Ceramic Institute). The results are as follows:

[0070] Table 2 Performance Comparison of Ceramic Permeable Bricks and Microcrystalline Permeable Boards

[0071]

[0072] like Figure 6 The table shows a comparison of the appearance of the microcrystalline permeable board of the present invention and ceramic permeable bricks. As can be seen from Table 2, compared to ceramic permeable bricks, the microcrystalline permeable board of the present invention exhibits superior flexural strength, permeability, and frost resistance. Its flexural strength can reach 5.5–7.0 MPa, and its permeability coefficient can reach 2.0–3.0 × 10⁻⁶. -2 It has a finer particle size, a smoother feel without losing its anti-slip function, and richer colors. After high-temperature sintering and cooling, it forms a dense layer of reflective crystalline particles that sparkle under light. Combined with various small crystalline particles of different colors, it forms a rich texture of natural granite, which is highly decorative and can completely replace and is superior to non-fired sand-based permeable brick products.

Claims

1. A method for processing a microcrystalline permeable plate, characterized in that, Includes the following steps: Prepare the base material and the outer material separately; Preparation of the fabric material: Select 6 to 10 kinds of natural sodium feldspar and potassium sodium feldspar with different colors, crush, ball mill, wash, dry and sieve them respectively to obtain sodium feldspar and potassium sodium feldspar particles with D50 of 0.2 to 0.3 mm. Mix sodium feldspar and potassium sodium feldspar particles, solvent, binder, water and colorant evenly to obtain the fabric. The ball milling process involves the frictional ball milling of sodium feldspar and potassium sodium feldspar particles by their own gravity. In the fabric, by mass fraction, with the total amount of sodium feldspar particles and potassium sodium feldspar particles as unit 1, the co-solvent accounts for 1~10 wt%, the binder accounts for 1~15 wt%, water accounts for 3~10 wt%, and the colorant accounts for 0~10 wt%. The albite particles contain 3-12% sodium. The potassium-sodium feldspar particles contain 3-12% potassium and 3-12% sodium. Preparation of the base material: Waste ceramic tile particles, adhesive, co-solvent and water are mixed and stirred evenly to obtain the base material; In the base material, by mass fraction (unit: waste ceramic tile particles), the adhesive accounts for 1-15 wt%, the co-solvent accounts for 1-10 wt%, and the water accounts for 1-10 wt%. Method A) Press, calcine, and cool the fabric to obtain a microcrystalline permeable plate with a single layer structure; or, Method B) Combine the base material and the fabric material, press, calcine, and cool to obtain a two-layer microcrystalline permeable plate.

2. The processing method of the microcrystalline permeable plate according to claim 1, characterized in that, In method A), the pressing is carried out by a two-stage fabric feeding method, in which the fabric is pushed into the mold to a set thickness by a press fabric feeding carriage and pressed into shape.

3. The processing method of the microcrystalline permeable plate according to claim 1, characterized in that, In Method B), the pressing is performed using a two-stage material feeding method. The base material and the outer material are pushed into the mold at a set thickness by the press feeding carriage to form an overlapping state, and then pressed and shaped.

4. The processing method of the microcrystalline permeable plate according to claim 1, characterized in that, The calcination temperature described in method A) or method B) is 1000~1200℃.

Citation Information

Patent Citations

  • Ceramic water permeable brick prepared by use of in-situ generated high-temperature binder and preparation method thereof

    CN103771864A

  • High-fracture resistance high-strength ceramic plate slab and manufacturing method thereof

    CN108314435A

  • Sintered water-permeable brick not prone to blockage and preparing method thereof

    CN108558358A

  • Granite-imitated water permeable plate and preparation method thereof

    CN113336531A