A gel profile control agent prepared from oily sludge for deep liquid flow diversion, and its preparation method and application
The gel profile control agent prepared through low-temperature biochemical drying and grinding technology solves the problems of liquid flow diversion and oily sludge treatment in deep oil fields, achieves high water flooding efficiency and high oily sludge reuse rate, and reduces production costs. cost.
Patent Information
- Application Number
- CN202310332043.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Among the existing oilfield profile control and water plugging technologies, the water flooding efficiency of old oil fields with high water content is low, deep liquid flow diversion is difficult to achieve, and the treatment and reuse rate of oily sludge is low. The production cost of existing gel profile control agents is high and Difficult to prepare quickly.
Low-temperature biochemical drying technology and grinding technology are used to prepare oily sludge powder. Through colloid mill treatment and mixing with cationic polymers, anionic polymers, etc., a gel profile control agent with good injectability and blocking effect is prepared. Simplify the preparation process and improve sludge reuse.
It achieves efficient deep flow diversion of gel profile control agent, improves recovery rate and plugging effect, reduces production costs, simplifies the preparation process, and improves the reuse rate of oily sludge.
Smart Images

Figure CN116574492B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oilfield profile control and water plugging, and particularly relates to a gel profile control agent prepared from oily sludge for deep liquid flow diversion, and a preparation method and application thereof. Background Art
[0002] Water flooding is an important way to develop oil fields, especially for the development of old oil fields with high water content in the late stage of exploitation. Therefore, improving the efficiency of water flooding is of great significance to the stable production of old oil fields. For oil fields dominated by continental sediments, the reservoir permeability varies greatly, and the intra-layer, inter-layer and plane heterogeneity is serious. Long-term water injection development has formed a dominant water flow channel, resulting in the sudden advance and ineffective circulation of injected water, and low water flooding efficiency. Deep liquid flow diversion is a key technology to improve deep problems in oil layers, inhibit inefficient and ineffective circulation of injected water, and expand the swept volume.
[0003] At present, three long-term deep flow diversion systems (technology for improving oil recovery in old oil fields with extremely high water cut period) have been formed, namely high-strength elastic slow-swelling particles, intercalated polymer gels, and native inorganic microgels. In addition, products such as gel microspheres and flexible diversion agents have been developed. These new products have their own characteristics, but also have many shortcomings:
[0004] High-strength elastic slow-swelling particles: They solve the problems of ordinary bulk-swelling particles, such as fast water absorption, easy breakage by shearing, and inability to penetrate deep into the formation to form effective plugging. The water absorption time is controllable from 10 to 90 days. The addition of rubber components greatly improves the strength. However, since it relies on particle size for plugging, its injectability and plugging ability are shortcomings.
[0005] Intercalation polymer gel system: The inorganic minerals are organically modified by the zwitterionic composite intercalation method, which realizes the stripping of the interlayer spacing of the organically modified clay minerals in aqueous solution and the intercalation polymerization with acrylamide monomers, thus solving the problems of weak strength and high cost of gel diverting agents based on cross-linked polyacrylamide. However, injectability and plugging ability are also shortcomings.
[0006] Benyuan inorganic microgel system: Benyuan inorganic microgel is based on modified sodium silicate, urea, and composite aluminum phosphate. It uses calcium and magnesium ions in formation water as crosslinking agents to overcome the effects of high-salt environments on chemical agents and form inorganic microgels in situ. By adsorbing and scaling on the surface of the rock formation to form a coating, the permeability of the dominant channel is reduced. Benyuan inorganic microgel solves the temperature and salt resistance problems of high-strength elastic slow-swelling particles and intercalated polymer gels, but the blocking ability of many high-permeability channels is not good.
[0007] Gel microspheres: micron or submicron microspheres polymerized in the oil phase by emulsion polymerization or microemulsion polymerization. They have high requirements on particle size. If the particle size is too large, the plugging effect is good but the injection is difficult. If the particle size is too small, the injectability is good but the plugging is poor.
[0008] At the same time, in recent years, with the continuous improvement of water quality standards for oilfield injection, sewage treatment technology has been continuously updated. Although the water quality has met the requirements, it has also brought about the problem of increasing sludge. As a hazardous waste, the treatment of oily sludge has always been a problem that has plagued oilfields.
[0009] To this end, CN105399907A proposes a gel profile control agent made from oily sludge as a raw material, which not only realizes the recycling and reuse of oily sludge, but also reduces the production cost of the gel profile control agent. However, the slurry mass of oily sludge in the gel profile control agent accounts for only 15-30%, and the actual sludge recycling rate is even lower. In addition, the straw raw material used needs to be processed in advance, and the components need to undergo cross-linking polymerization after mixing, which cannot achieve the purpose of rapid preparation on the construction site. Summary of the invention
[0010] The purpose of the present invention is to provide a deep liquid flow diversion gel profile control agent prepared with oily sludge as raw material and a preparation method thereof. The purpose of preparing the gel profile control agent from oily sludge is achieved through low-temperature biochemical drying technology and grinding technology. The obtained gel profile control agent not only has the advantages of good injectability, good selective plugging effect in deep oil layers, high utilization rate of oily sludge, but also greatly improves the reuse rate of oily sludge, simplifies the preparation process, and achieves the purpose of on-site preparation at the construction site.
[0011] To achieve the above object, the present invention provides the following technical solutions:
[0012] In a first aspect, the present invention provides a method for preparing a gel profile control agent, comprising the following steps:
[0013] S1, the oily sludge is subjected to low-temperature biochemical drying treatment to obtain oily sludge powder;
[0014] S2, subjecting the oily sludge powder to colloid mill treatment to obtain colloid mill particles;
[0015] S3, mixing the colloidal mill particles with a solution containing a cationic polymer under stirring and spraying conditions, and drying to obtain a cationic modified clay powder;
[0016] S4, mixing the cationic modified soil powder with anionic polymer, cross-linked polymer, cross-linking agent and stabilizer to obtain oil-containing sludge gel profile control agent.
[0017] In step S1, the oily sludge may be oil and gas field oily sludge, coal chemical industry oily sludge, fine chemical industry oily sludge and other light industry oily sludge.
[0018] In step S1, the water content of the oily sludge is 80-95%.
[0019] In step S1, the biochemical drying treatment conditions are: temperature of 55-70°C, time of 4-6 hours, air volume of 1800-2000m 3 / h, the pressure is slightly negative 90-100kPa.
[0020] In step S1, the moisture content of the oily sludge powder is 20-30%, and the particle size is 0.02-2.0 mm.
[0021] In step S1, the high-humidity waste gas generated during the biochemical drying process is sprayed to cool down, and then the gas enters the VOCs treatment system to remove harmful substances, and the sewage enters the sewage treatment system.
[0022] In step S2, the operating conditions of the colloid mill treatment are: normal temperature and pressure.
[0023] In step S2, the particle size of the colloidal mill particles is 2-5 μm.
[0024] In step S3, the cationic polymer is polydimethyldiallylammonium chloride and / or cationic polyacrylamide.
[0025] In step S3, in the solution, the mass concentration of the cationic polymer is 1-5%.
[0026] In step S3, the mass ratio of the colloidal mill particles to the solution containing the cationic polymer is 100:(3.6-4.5).
[0027] In step S3, the stirring condition is: a rotation speed of 50 to 80 r / min.
[0028] In step S3, the drying conditions are: temperature of 100-120°C and time of 18-24h.
[0029] In step S4, the anionic polymer is sodium polyacrylate and / or sodium lignin sulfonate.
[0030] In step S4, the cross-linked polymer is cross-linked sodium polyacrylate.
[0031] In step S4, the cross-linking agent is N,N'-methylenebisacrylamide and / or aluminum citrate.
[0032] In step S4, the stabilizer is sodium chloride.
[0033] In step S4, the mass ratio of the cationic modified clay powder, the anionic polymer, the cross-linked polymer, the cross-linking agent and the stabilizer is: (77-82): (8-12.5): (4.2-4.6): (2.3-2.7): (2.8-3.3).
[0034] In a second aspect, the present invention further provides a gel profile control agent obtained by the preparation method.
[0035] In a third aspect, the present invention further provides a deep plugging method for an oil reservoir, comprising the following steps:
[0036] (1) adding the gel profile control agent into the dispersion and stirring to obtain a gel;
[0037] (2) Injecting protective fluid into the deep reservoir of the oil reservoir, then injecting the gel, then the displacement fluid, and finally injecting clean water.
[0038] In step (1), the dispersion is a sodium chloride solution with a mass fraction of 8 to 15%, preferably 9 to 11%.
[0039] In step (1), based on the mass of the dispersion, the amount of the gel profile control agent added is 0.4-0.6%, preferably 0.5%.
[0040] In step (1), the stirring time is 30-60 min, preferably 60 min.
[0041] In step (2), the injection volume of the protective liquid is 10 to 50 m 3 , preferably 50m 3 ; The injection pressure depends on the actual working conditions.
[0042] In step (2), the injection volume of the gel is preferably such that the design pressure requirement is met, and the injection speed is 12 to 20 m / s. 3 / h, preferably 15m 3 / h; injection pressure depends on actual working conditions.
[0043] In step (2), the protective liquid and the displacement liquid are both sodium chloride solutions with a mass fraction of 8 to 15%, preferably 9 to 11%.
[0044] In step (2), the injection volume of the displacement fluid is 10 to 50 m 3 , preferably 50m 3 ; The injection pressure depends on the actual working conditions.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] 1. The gel profile control agent provided by the present invention can be evenly dispersed in the protective liquid, and can be distributed to the dominant liquid flow channel deep in the oil layer through the protective liquid. It has good portability and can reach the target site for plugging more accurately.
[0047] 2. After approaching the target site, the gel profile control agent provided by the present invention can be rapidly expanded into gel by injecting water, and rapidly expands at the target site, with rapid plugging effect, greatly improving construction efficiency; at the same time, deep selective plugging is produced, liquid flow is diverted, and the water drive swept volume is expanded, thereby achieving the purpose of improving the recovery rate.
[0048] 3. The gel profile control agent provided by the present invention has good plugging ability and anti-scouring performance, and can quickly restore to a gel state after being destroyed.
[0049] 4. The method provided by the present invention greatly improves the recycling rate of oily sludge, reduces the raw material cost and production cost of the gel profile control agent, and the method has a wide range of applications and can be used for oil and gas field oily sludge treatment, coal chemical oily sludge treatment, fine chemical oily sludge and other light industrial oily sludge.
[0050] 5. The method provided by the present invention is simple to operate and highly safe, and the gel profile control agent can be prepared on-site at the construction site. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is a photo of the round gel beads formed when the gel profile control agent described in Example 1 meets water in a glass sand-filled tube.
[0052] Figure 2 This is a microscopic photograph of the gel profile control agent described in Example 1 after swelling with water.
[0053] Figure 3 These are comparison diagrams of the plugging effects using different profile control agents; the profile control agent in the left figure is oil-containing sludge powder, and the profile control agent in the right figure is the gel profile control agent provided in Example 1.
[0054] Figure 4 This is a plugging curve diagram after the glass sand-filled pipe is plugged using the gel profile control agent described in Example 1.
[0055] Figure 5 This is the plugging curve diagram after using oily sludge powder to plug the glass sand-filled pipe.
[0056] Figure 6 This is a curve diagram of the horizontal well plugging construction effect. DETAILED DESCRIPTION
[0057] The present invention is further described below in conjunction with specific examples, but the present invention is not limited to the following examples. The methods described are conventional methods unless otherwise specified. The raw materials described can be obtained from public commercial channels unless otherwise specified.
[0058] The sources of the raw materials involved in the following examples are as follows:
[0059] The oily sludge is scum sludge from Liaohe Oilfield, and its water content is 82%.
[0060] Polydimethyldiallylammonium chloride: purchased from Wuhan Chengtian Fine Chemical Co., Ltd., high-grade pure GR;
[0061] Sodium polyacrylate: purchased from Jinan Zhiheng Zhiyuan Chemical Technology Co., Ltd., industrial grade;
[0062] Cross-linked sodium polyacrylate: prepared according to the method disclosed in CN1296981A.
[0063] Cross-linking agent: N,N'-methylenebisacrylamide: purchased from Tianjin Damao Chemical Reagent Factory, analytical grade AR;
[0064] Aluminum citrate: purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd., analytical grade AR;
[0065] Stabilizer sodium chloride: Tianjin Dingshengxin Chemical Co., Ltd., analytical grade AR.
[0066] The device models involved in the following embodiments are as follows:
[0067] Low temperature biochemical drying machine: as shown in CN210287104U.
[0068] Example 1. Preparation of gel profile control agent
[0069] Using Liaohe Oilfield scum sludge as raw material, the gel profile control agent was prepared according to the following steps:
[0070] (1) The scum oil sludge with a moisture content of 82% is directly transported to the low-temperature biochemical dryer through the mud bucket and screw, and then dried at a temperature of 65°C, a time of 5 hours, and an induced air volume of 1900m 3 / h, and drying under the condition of negative pressure of 95kPa to obtain oily sludge powder with a particle size of 0.02-2.0mm;
[0071] The absolute humidity coming out of the main fermentation chamber of the low-temperature biochemical dryer is 160g / m 3 The high-humidity gas is cooled by spraying and then enters the VOCs treatment system to remove harmful substances. The condensed water produced is further treated or returned to the factory sewage treatment system.
[0072] (2) subjecting the oily sludge powder to a colloid mill treatment to obtain colloid mill particles with a particle size of 2 to 5 μm; in this embodiment, the operating conditions of the colloid mill treatment are: normal temperature and pressure;
[0073] (3) adding the obtained colloidal mill particles into a kneader, spraying a 2.5% polydimethyldiallyl ammonium chloride solution while stirring, and drying to obtain a cationic modified clay powder;
[0074] The mass ratio of the colloidal grinding particles to polydimethyldiallylammonium chloride is 100:4.2;
[0075] (4) kneading the obtained cationic modified soil powder with sodium polyacrylate, cross-linked sodium polyacrylate, a cross-linking agent, and a stabilizer in a mass ratio of 78:12:4.4:2.7:2.9 to obtain an oily sludge gel profile control agent.
[0076] like Figure 1 As shown in the figure, the gel profile control agent becomes gel when it meets water and can fill the entire pore section of the glass sand-filled tube. The microscopic photo is shown in Figure 2 shown.
[0077] Application example 1: Glass sand-filled pipe plugging experiment
[0078] Here are the steps:
[0079] (1) Add 5 g of the gel profile control agent obtained in Example 1 to 1000 ml of a 10% sodium chloride solution protective solution, stir and disperse evenly, and stir for 60 min to obtain a mixed solution 1;
[0080] (2) Add 5 g of oily sludge powder to 1000 ml of 10% sodium chloride solution, stir and disperse evenly for 60 min to obtain mixed solution 2;
[0081] (3) Simulating the on-site operation of oil production construction, the glass sand-filled tube was sealed and tested using mixed liquid 1 and mixed liquid 2 respectively: about 2 / 3 of the volume of the glass sand-filled tube was filled with glass beads, the glass sand-filled tube was placed horizontally, 45 mL of a protective liquid with a mass concentration of 10% was injected into the glass sand-filled tube at a rate of 1.5 mL / min, and then 90 mL of mixed liquid 1 and mixed liquid 2 were injected at a rate of 1.5 mL / min, respectively, and then 50 mL of a displacement liquid with a mass concentration of 10% was injected at a rate of 0.8 mL / min. Finally, clean water was continuously injected at a rate of 0.08 mL / min.
[0082] The test results are as follows:
[0083] (1) Single plugging effect
[0084] like Figure 3 As shown in the left figure, the effluent from the glass sand-filled tube mouth injected with oily sludge powder contains oily sludge, indicating that the sealing effect of the oily sludge powder is poor; the effluent from the glass sand-filled tube mouth injected with gel profile control agent in the right figure is clear liquid, indicating that the sealing effect of the gel profile control agent is very good and can effectively prevent the outflow of sludge and oil.
[0085] (2) Anti-scouring performance and re-plugging effect
[0086] like Figure 4As shown, the horizontal axis is time and the vertical axis is pressure. In the initial stage of the test, the pressure fluctuation in the pipe rises to 274.7 kPa after the sludge gel is injected, indicating that the gel profile control agent has accumulated in the pipe; with subsequent water injection, the pressure drops to about 240 kPa, but is basically stable as a whole, indicating that the profile control agent quickly gels when it meets water, forming a plug in the pipe to restrain the sludge and prevent it from losing; as shown in the figure, under the action of continued water injection, the pressure in the pipe is in a sawtooth fluctuation state, representing plugging, breakthrough, and migration, that is, movable, that is, the plugging generated by the gel is destroyed and then quickly re-formed in the rear end channel, so that the pressure in the pipe continues to be stable, which shows that the gel profile control agent provided by the present invention not only has good plugging ability, but also has better anti-scouring performance.
[0087] Comparative Example 1
[0088] Compared with Example 1, the difference is that oily sludge is used instead as the profile control agent.
[0089] Using the test method in the above application example, the results are as follows Figure 5 As shown, the horizontal axis is time and the vertical axis is pressure. In the initial stage of the test, the pressure in the pipe changes slightly after the sludge is injected, indicating that the sludge accumulates in the pipe; then water injection begins, and the pressure in the pipe drops to about 0, indicating that the sludge is washed away by the water flow. Therefore, the plugging material has no plugging ability and poor anti-scouring ability. Due to the lack of gel adsorption, the sludge in the pipe is lost along the water flow channel.
[0090] Application example 2: Horizontal well plugging test
[0091] Taking the Jin 612-H101 horizontal well as an example, its high water content is affected by water seepage during injection, and it is urgent to implement water control through dominant channels.
[0092] Blocking plan order:
[0093] (1) Gel preparation: a sodium chloride solution with a mass concentration of 10% was prepared as a dispersion, and 0.5% of the gel profile control agent obtained in Example 1 was slowly added under stirring, and stirred for 60 minutes to form a gel.
[0094] (2) Pre-protection solution: 10% sodium chloride solution, 50 ml 3 , the pressure is 7MPa, to prevent the gel from reacting with the water in the bottom layer to form a colloid, test injection;
[0095] (3) Glue wall: Inject the gel obtained in step (1), 15m for the first car 3 , pressure: 8MPa;
[0096] (4) Glue wall: Inject the gel obtained in step (1), 15m for the first car 3 , pressure: 8MPa;
[0097] (5) Glue wall: Inject the gel obtained in step (1), 15m for the first car 3 , pressure: 9MPa;
[0098] (6) Glue wall: Inject the gel obtained in step (1), 15m for the first car 3 , pressure: 12MPa;
[0099] (7) Post-displacement fluid: 10% sodium chloride solution protective fluid, dosage: 25 ml 3 , the pressure is: 12MPa, to prevent the gel from reacting with water to form colloid in advance, and to clean the oil tank;
[0100] (8) Inject clean water: 350m 3 , pressure: 10MPa, so that the gel can reach the target position.
[0101] like Figure 6 As shown, the well was constructed on October 14, 2020, and took effect on November 17, 2020. The daily liquid production dropped from 40 tons to 28 tons, and the oil production increased from 0 tons / day to a maximum of 4 tons / day. The effect was seen in 3 months, and the oil production increased by 357 tons. This shows that by using the gel profile control agent provided by the present invention to block the crossflow channel, the plane water absorption quality can be significantly improved, the water content of the effective horizontal well can be suppressed, and the purpose of reducing water and increasing oil can be achieved.
[0102] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing a gel profile control agent, comprising the following steps: S1, the oily sludge is subjected to low-temperature biochemical drying treatment to obtain oily sludge powder; S2, subjecting the oily sludge powder to colloid mill treatment to obtain colloid mill particles; S3, mixing the colloidal mill particles with a solution containing a cationic polymer under stirring and spraying conditions, and drying to obtain a cationic modified clay powder; S4, mixing the cationic modified soil powder with an anionic polymer, a cross-linked polymer, a cross-linking agent, and a stabilizer to obtain an oily sludge gel profile control agent; In step S1, the conditions of the biochemical drying treatment are: temperature of 55-70°C; time of 4-6 hours; air volume of 1800-2000m 3 / h; the pressure is slightly negative 90-100kPa; In step S3, the cationic polymer is polydimethyldiallyl ammonium chloride and / or cationic polyacrylamide; in the solution, the mass concentration of the cationic polymer is 1-5%; the mass ratio of the colloidal grinding particles to the cationic polymer is 100:(3.6-4.5); In step S4, the anionic polymer is sodium polyacrylate and / or sodium lignin sulfonate; The cross-linked polymer is cross-linked sodium polyacrylate; The cross-linking agent is N,N'-methylenebisacrylamide and / or aluminum citrate; The stabilizer is sodium chloride; The mass ratio of the cationic modified clay powder, the anionic polymer, the cross-linked polymer, the cross-linking agent and the stabilizer is: (77-82): (8-12.5): (4.2-4.6): (2.3-2.7): (2.8-3.3).
2. The method for preparing the gel profile control agent according to claim 1, characterized in that: In step S1, the moisture content of the oily sludge is 80-95%.
3. The method for preparing the gel profile control agent according to claim 1 or 2, characterized in that: In step S1, the moisture content of the oily sludge powder is 20-30%, and the particle size is 0.02-2.0 mm.
4. The method for preparing the gel profile control agent according to claim 1 or 2, characterized in that: In step S2, the operating conditions of the colloid mill treatment are: normal temperature and pressure; The particle size of the colloidal mill particles is 2-5 μm.
5. The method for preparing the gel profile control agent according to claim 1 or 2, characterized in that: In step S3, the stirring condition is: the rotation speed is 50-80 r / min; The drying conditions are: temperature of 100-120° C. and time of 18-24 hours.
6. The gel profile control agent obtained by the preparation method according to any one of claims 1 to 5.
7. A deep plugging method for an oil reservoir, comprising the following steps: (1) adding the gel profile control agent described in claim 6 into the dispersion and stirring to form a gel; (2) Injecting protective fluid into the deep reservoir of the oil reservoir, then injecting the gel to form a gel wall, then injecting displacement fluid, and finally injecting clean water.
Citation Information
Patent Citations
Process for synthesizing cross-linked poly (sodium acrylate)
CN1296981A
Full-automatic sludge treatment equipment
CN210287104U
Oily sludge gel particle profile control agent and preparation method thereof
CN105399907A
Gel particles and preparation method thereof
CN105482794A