A Sc2O3 / MXene-derived TiO2 photocatalytic material and preparation method thereof
Through the preparation of Sc2O3/MXene derived TiO2 photocatalytic materials, the problem of wide TiO2 band gap and rapid electron hole recombination is solved through Sc2O3 doping and calcining technology, the photocatalytic efficiency and reaction efficiency are improved, and it is suitable for industrial production.
Patent Information
- Application Number
- CN202310570282.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-08
- Filing Date
- 2023-05-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-19
AI Technical Summary
The photocatalytic efficiency of existing TiO2@MXene photocatalytic materials is limited by the problem of wide TiO2 band gap and rapid photogenerated electron hole recombination, which affects the catalytic efficiency.
The preparation method of Sc2O3/MXene derived TiO2 photocatalytic material is adopted. By uniformly stirring the Sc2O3 powder with the MXene dispersion, it is calcined to form TiO2 of Sc2O3 composite on the surface of MXene, inhibiting electron hole recombination, reducing band gap, and improving photo response strength.
The band gap of TiO2 is effectively reduced, the photoresponse range and photocatalytic efficiency are enhanced, and the TiO2 particles doped after Sc2O3 are refined, the reaction efficiency is improved, and the operation is simple, which is suitable for industrial production.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photocatalytic degradation of pollutant materials, and specifically relates to a Sc2O3 / MXene-derived TiO2 photocatalytic material and a preparation method thereof. Background Art
[0002] In recent years, with the in-depth study of the physical properties of MXene materials such as resistivity, conductivity, and elastic properties, it has been found that they have great application potential in nanodevices. In addition, MXene materials also have excellent chemical stability and heat resistance. Due to the large specific surface area of the two-dimensional layered structure of MXene, they are also widely used in supercapacitors, lithium-ion batteries, and heavy metal adsorption applications. In addition, as a new type of two-dimensional material, MXene has a large specific surface area, good electrical conductivity and transmission properties, so its application in the field of photocatalysis has great prospects. TiO2 is a photocatalytic material that has been widely studied. It has the characteristics of good light response, low cost, pollution-free, and stable chemical properties. It is widely used in the field of photoelectrocatalysis.
[0003] Calcining MXene to generate TiO2 can improve the photocatalytic performance of MXene. Furthermore, compared to physical or chemical composites, the in-situ growth of TiO2 on the MXene surface during the calcination process offers a better composite effect (embedded in the MXene surface) and electron transport properties, resulting in better photocatalytic performance. However, in existing research, the photocatalytic efficiency of prepared TiO2@MXene has been limited, primarily due to the wide band gap of TiO2 in the photocatalyst and the rapid recombination of its photogenerated electrons and holes, which in turn affects the catalytic efficiency of the photocatalyst. Summary of the Invention
[0004] In view of the problems and shortcomings in the prior art, the object of the present invention is to provide a Sc2O3 / MXene-derived TiO2 photocatalytic material and a preparation method thereof.
[0005] Based on the above purpose, the present invention adopts the following technical solutions:
[0006] A first aspect of the present invention provides a method for preparing a Sc2O3 / MXene-derived TiO2 photocatalytic material, wherein the preparation method comprises the following steps: adding Sc2O3 powder to a MXene dispersion and stirring the mixture uniformly; and then centrifuging, drying, and calcining the mixture in sequence to obtain the obtained material.
[0007] Preferably, the mass ratio of the Sc2O3 powder to the MXene in the MXene dispersion is (0.5-4):100. More preferably, the mass ratio of the Sc2O3 powder to the MXene in the MXene dispersion is (0.5-3):100.
[0008] Preferably, the MXene is Ti3C2T X or Ti2CT X , T X represents a surface functional group, wherein the surface functional group is at least one of -O, -OH or -F. More preferably, the MXene is Ti3C2 or Ti2C.
[0009] More preferably, the MXene dispersion is obtained by adding MXene powder to water and uniformly dispersing it; the MXene powder is dispersed in water by magnetic stirring for 30 minutes.
[0010] Preferably, the preparation method of the MXene powder is: adding a fluoride salt to concentrated hydrochloric acid to dissolve it to obtain a fluoride salt solution; adding MAX to the fluoride salt solution and etching it at 35° C. to obtain a mixed solution; washing the mixed solution and then centrifuging to collect the precipitate, and then drying the precipitate and grinding it to obtain the MXene powder.
[0011] Preferably, the mass volume ratio of the fluoride salt to concentrated hydrochloric acid is 2 g:30 mL; the mass volume ratio of the fluoride salt to MAX is 1:1.
[0012] More preferably, the fluoride salt is lithium fluoride (LiF); the concentrated hydrochloric acid has a concentration of 12 mol / L; and 2 g of lithium fluoride is added to every 30 mL of concentrated hydrochloric acid in the fluoride salt solution. Furthermore, the fluoride salt is ultrasonically treated for 15 minutes during the dissolution process in the concentrated hydrochloric acid to promote dissolution.
[0013] Preferably, the MAX is Ti3AlC2 or Ti2AlC.
[0014] More preferably, the etching treatment condition is: using a heat-collecting constant temperature magnetic stirrer to stir the material at 35° C. for 48-72 hours.
[0015] More preferably, the washing step of the mixed solution is specifically as follows: deionized water, dilute hydrochloric acid and ethanol are added to the mixed solution in this order for rinsing and centrifugation until no fluoride salt solids are left and the supernatant is neutral; the concentration of the dilute hydrochloric acid is 2 mol / L.
[0016] More preferably, the drying condition of the precipitate is vacuum drying at 80° C. for 12 h.
[0017] Preferably, during the calcination process, the calcination temperature is 350° C. and the calcination time is 4 hours.
[0018] The second aspect of the present invention provides a Sc2O3 / MXene-derived TiO2 photocatalytic material prepared by any of the preparation methods described in the first aspect above.
[0019] The third aspect of the present invention provides the application of the Sc2O3 / MXene-derived TiO2 photocatalytic material described in the second aspect in the field of photocatalysis.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The present invention composites Sc2O3 on the surface of MXene two-dimensional material with high specific surface area by physical mixing and calcination, inhibiting the recombination of photogenerated electrons and holes in the material, reducing the band gap of the material and increasing the light response intensity, thereby improving the photocatalytic efficiency. Furthermore, during the calcination stage, some Sc 3+ Ions enter the gaps in the TiO2 lattice, and some are on the surface of TiO2 particles and MXene. The ions entering the lattice cause the diffraction peak of the (101) crystal plane of TiO2 to shift to the left, and at the same time its band gap decreases, effectively separating photogenerated electrons and holes and enhancing the light response range. The Sc element loses its original three electrons in the outermost orbital d and transforms into Sc 3+ ion, Sc 3+ There are no electrons in the d orbital of the ion, so under the action of the d orbital, it can act as a shallow potential capture trap for photogenerated electrons, which is more conducive to the separation of photogenerated electron and hole pairs. In addition, MXene, as an efficient transmission channel, is more conducive to the rapid transport and separation of electrons, thereby accelerating the efficiency of photocatalysis. In one embodiment, compared with the photocatalytic material with a Sc2O3 doping amount of 3% and the photocatalytic material without Sc2O3 doping, the Sc2O3 / MXene-derived TiO2 photocatalytic material prepared by the present invention has a lower electrochemical impedance and a higher photocurrent when the Sc2O3 addition amount is 2% of MXene.
[0022] (2) After the present invention is compounded with Sc2O3, Sc 3+ The anatase TiO2 did not undergo any crystal transformation after ion doping, but the TiO2 lattice was distorted and the grains were refined, which inhibited grain growth and limited the contact between TiO2 grains, resulting in a finer particle size of TiO2 on the MXene surface. This improved the reaction efficiency during the photocatalytic reaction.
[0023] (3) The present invention uses MAX material to prepare MXene two-dimensional material using a constant temperature etching temperature of 35°C and a constant temperature time of 72 hours. Under these reaction conditions, the MAX material can be completely etched, so that the A layer of metal is completely etched away from the MAX material to prepare a two-dimensional MXene material. At the same time, the LiF in the reaction process can fully participate in the reaction, reducing the generation of impurities.
[0024] (4) The present invention mainly adopts etching, physical compounding and calcination methods. The operation process is relatively simple, with less three wastes, suitable for industrial large-scale production, and has good economic and environmental benefits.
[0025] Other advantages, objects, and features of the present invention will be described in part in the following description and, in part, will be apparent to those skilled in the art upon examination of the following description or may be learned from practice of the present invention. The objects and other advantages of the present invention may be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 XRD diffraction patterns of the photocatalytic materials prepared in Example 4 of the present invention (Sc2O3 doping amount is 2%) and Comparative Example 1 (Sc2O3 doping amount is 0%);
[0027] Figure 2 The photocurrent test spectrum of the photocatalytic materials prepared in Example 4, Example 6 and Comparative Example 1 of the present invention. In the figure, the black solid line indicates that the added mass of Sc2O3 is 2% of MXene, the red solid line indicates that the added mass of Sc2O3 is 3% of MXene, and the blue solid line indicates that the added mass of Sc2O3 is 0% of MXene;
[0028] Figure 3 Electrochemical impedance spectroscopy was performed on the photocatalytic materials prepared in Example 4, Example 6 and Comparative Example 1 of the present invention. In the figure, the blue balls indicate that the added mass of Sc2O3 is 0% of MXene, the red balls indicate that the added mass of Sc2O3 is 3% of MXene, and the black balls indicate that the added mass of Sc2O3 is 2% of MXene. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below through embodiments in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0030] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments in this application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0031] Example 1
[0032] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0033] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0034] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.0025 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly, the precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0035] Example 2
[0036] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0037] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0038] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.005 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly, the precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0039] Example 3
[0040] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0041] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0042] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.0075 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly. The precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0043] Example 4
[0044] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0045] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0046] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.01 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly, the precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0047] Example 5
[0048] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0049] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0050] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.0125 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly, the precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0051] Example 6
[0052] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0053] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0054] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.015 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly, the precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0055] Example 7
[0056] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0057] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0058] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.0175 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly. The precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0059] Example 8
[0060] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0061] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0062] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.02 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly, the precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0063] Example 9
[0064] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0065] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0066] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.0025 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly, the precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0067] Example 10
[0068] This embodiment provides a Sc2O3 / MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0069] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0070] (2) Preparation of Sc2O3 / MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; 0.015 g of Sc2O3 powder was then added to the MXene dispersion and stirred thoroughly, the precipitate was centrifuged, dried, and then calcined at 350°C for 4 h.
[0071] Comparative Example 1
[0072] This embodiment provides a MXene-derived TiO2 photocatalytic material, which includes the following steps:
[0073] (1) Preparation of MXene material: Weigh 2 g of lithium fluoride and dissolve it in 30 mL of 12 mol / L concentrated hydrochloric acid (HCl). Ultrasonicate for 15 min to completely dissolve the lithium fluoride to obtain a fluoride salt solution. Then add 2 g of Ti3AlC2 sample and stir at 35 °C using a heat-collecting constant temperature magnetic stirrer for 60 h to obtain a mixed solution. Add deionized water, dilute hydrochloric acid and ethanol to the mixed solution in this order for washing and centrifugation until there is no white lithium fluoride solid and the pH value of the supernatant is neutral. Finally, place the precipitate obtained after centrifugation in a vacuum drying oven and dry it at 80 °C for 12 h. Grind it to obtain MXene powder.
[0074] (2) Preparation of MXene-derived TiO2 photocatalytic material: 0.5 g of the MXene powder prepared in step (1) was uniformly dispersed in water and magnetically stirred for 30 min to obtain a MXene dispersion; the MXene dispersion was then centrifuged to obtain a precipitate, which was dried and then calcined at 350°C for 4 h.
[0075] Performance testing:
[0076] The Sc2O3 / MXene-derived TiO2 photocatalytic materials prepared in Example 4 and Comparative Example 1 were subjected to XRD testing. The XRD diffraction patterns are shown in Figure 2. Figure 1 As shown. Figure 1 TiO2 and Ti3C2 peaks can be clearly seen. When the Sc2O3 doping level is 2%, the Ti3C2 peak height at around 6.9° is more pronounced. This may be because Sc2O3 was added prior to calcination during the preparation process. Compared to the sample without Sc2O3, the oxidation content of Ti3C2 is reduced. At the same time, at around 25°, the diffraction peak of anatase TiO2 in the sample without Sc2O3 is slightly higher, also reflecting more complete oxidation of Ti3C2. The Sc2O3 peak can be clearly seen in the spectrum with a Sc2O3 doping level of 2%, indicating that the Sc2O3 composite is intact.
[0077] The photocatalytic materials prepared in Example 4, Example 6, and Comparative Example 1 were tested for photocurrent intensity using an electrochemical analysis instrument CHI 660D (purchased from Shanghai Chenhua Instrument Co., Ltd.). The test conditions were: a three-electrode system (working electrode, platinum wire electrode, and reference electrode), 50 mL of Na2SO4 (0.2 mol / L) electrolyte, and xenon lamp irradiation. The results are shown in Figure 2. Figure 2 As shown. Figure 2 It can be seen that the photocurrent response intensity of the composite photocatalytic material with a Sc2O3 doping amount of 2% is higher than the photocurrent response intensities of the composite material with a doping amount of 3% and 0%, indicating that the photocurrent response of the composite material with a doping amount of 2% is the strongest.
[0078] The electrochemical impedance spectroscopy (ECI) test was performed on the photocatalytic materials prepared in Example 4, Example 6 and Comparative Example 1 using an electrochemical analysis instrument CHI 660D. The results are shown in Figure 2. Figure 3 As shown. Figure 3 It can be seen that since the smaller the radius of the EIS curve, the smaller the resistance to charge transfer of the material, it can be seen that after the composite Sc2O3 is added, the impedance of the composite material decreases, the charge transfer resistance of the material decreases, and the composite material with a Sc2O3 doping amount of 2% has the smallest impedance and the smallest charge transfer resistance.
[0079] comprehensive Figure 2 and Figure 3 The results show that when the addition amount of Sc2O3 is 2% of MXene, the prepared Sc2O3 / MXene-derived TiO2 photocatalytic material has a smaller electrochemical impedance and a larger photocurrent. This is because as the Sc2O3 content increases, the active sites on the surface of the composite material remain unchanged. When the addition amount exceeds 2%, Sc2O3 particles and aggregation of Sc2O3 and TiO2 particles appear, thus affecting the photocatalytic performance of the composite material. Therefore, the preferred addition amount of Sc2O3 in this application is 2% of MXene.
[0080] In summary, the present invention effectively overcomes the deficiencies in the prior art and has a high industrial application value. The above embodiments serve to illustrate the substantial content of the present invention, but are not intended to limit the scope of protection of the present invention. Those skilled in the art will appreciate that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of protection of the technical solutions of the present invention.
Claims
1. A method for preparing a Sc2O3 / MXene-derived TiO2 photocatalytic material, characterized in that: The preparation method comprises the following steps: adding Sc2O3 powder to a MXene dispersion and stirring the mixture evenly, and then sequentially centrifuging, drying, and calcining the mixture at 350°C to obtain the MXene dispersion; the mass ratio of the Sc2O3 powder to the MXene in the MXene dispersion is (0.5-4):
100.
2. The preparation method according to claim 1, characterized in that: The MXene is Ti3C2T X or Ti2CT X , T X represents a surface functional group, wherein the surface functional group is at least one of -O, -OH or -F.
3. The preparation method according to claim 2, characterized in that: The MXene dispersion is obtained by adding MXene powder into water and dispersing it uniformly; the preparation method of the MXene powder is: adding fluoride salt into concentrated hydrochloric acid to dissolve to obtain a fluoride salt solution; adding MAX into the fluoride salt solution for etching treatment to obtain a mixed solution; washing the mixed solution and then centrifuging to collect the precipitate, and then grinding the precipitate to obtain the MXene dispersion.
4. The preparation method according to claim 3, characterized in that: The mass volume ratio of the fluoride salt to concentrated hydrochloric acid is 2 g:30 mL; the mass volume ratio of the fluoride salt to MAX is 1:
1.
5. The preparation method according to claim 4, characterized in that: The fluoride salt is lithium fluoride; the concentration of the concentrated hydrochloric acid is 12 mol / L.
6. The preparation method according to claim 3, characterized in that: The etching temperature is 35°C.
7. Sc2O3 / MXene-derived TiO2 photocatalytic material prepared by the preparation method described in any one of claims 1-6.
8. Application of the Sc2O3 / MXene-derived TiO2 photocatalytic material according to claim 7 in the field of photocatalysis.