Treatment agent for forming chemical film layer on metal surface and preparation method thereof

By using a treatment agent formed by synthetic phosphate nanoparticles and acrylate polymers on the metal surface, the problem of poor binding ability of existing chemical film-forming agents and paint films is solved, achieving better corrosion resistance and adhesion, and significantly Improves the protective effect of metal surfaces.

CN116590698BActive Publication Date: 2024-10-25SHANDONG DONGRONG INFORMATION INDUSTRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310438101.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-25
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

Existing relatively environmentally friendly chemical film-forming agents have poor bonding ability with subsequent paint films, resulting in poor metal surface treatment effects.

Method used

A treatment agent based on the synergy of synthetic phosphate nanoparticles and acrylate polymer to form a chemical film layer on the metal surface is used. Through the synergistic effect of components A, B, C, and D, a highly active nanoparticle dispersion is formed, and is deposited on the metal surface. Forms a colored film layer to enhance the bonding ability with subsequent paint films.

Benefits of technology

It improves the bonding ability between the metal surface and the paint film, enhances corrosion resistance and adhesion, and significantly improves the protective effect of the metal surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004192877080000031
    Figure BDA0004192877080000031
  • Figure BDA0004192877080000061
    Figure BDA0004192877080000061
Patent Text Reader

Abstract

The invention discloses a treatment agent for forming a corrosion-resistant conversion film on a metal surface and a preparation method thereof, and belongs to the technical field of metal surface treatment. The main components of the treatment agent are phosphate nanoparticles, acrylate and its derivative polymer and heteropoly acid composite modified material, zinc salt and neutralizer. Acrylate and zinc salt are combined on the metal surface to form a polymer to form protection. In addition to being able to chelate with metal ions, the phosphate nanoparticles can also be evenly distributed on the metal surface, increase the surface roughness, and enhance the ability to combine with subsequent paint films. Introducing heteropoly acids into the system of the invention can enhance the adsorption capacity of phosphate nanoparticles on the metal surface, thereby enhancing the subsequent adhesion capacity with the paint film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a treatment agent capable of forming a corrosion-resistant conversion film on a metal surface and a preparation method thereof, belonging to the technical field of metal surface treatment. Background Art

[0002] In the field of metal surface pretreatment, most metal substrates (such as cold-rolled steel plates, galvanized steel plates, aluminum alloys, etc.) need to undergo a chemical pretreatment process before coating. By immersing or spraying the metal substrate in a chemical bath, a chemical conversion film is formed on the surface, which enhances corrosion resistance on the one hand and adhesion with subsequent coatings on the other.

[0003] Phosphating process is commonly used in chemical pretreatment, but it is gradually being banned due to its pollution problem. In recent years, relatively environmentally friendly chemical film-forming agents have also appeared. For example, film-forming liquid with silane coupling agent as the main film-forming substance, and "ceramic" process with inorganic zirconate as the main film-forming substance. However, the above-mentioned film-forming agents all have the problems of poor environmental adaptability, narrow application range, and poor bonding ability with subsequent paint film. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problem that relatively environmentally friendly chemical film-forming agents in the prior art have poor bonding ability with subsequent paint films, and to provide a chemical treatment agent based on synthetic phosphate nanoparticles and acrylate polymers to synergistically form a chemical film layer on a metal surface and a preparation method of the chemical treatment agent.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A treatment agent for forming a chemical film layer on a metal surface, characterized in that it contains component A: 1-3%, component B: 8-15%, component C: 10-15%, component D: 2-5%, and the balance is water; the percentages are mass percentages;

[0007] The preparation method of component A comprises the following steps: adding citric acid to a raw acid aqueous solution, adding alcohol amine after the citric acid is dissolved to obtain a mixed system, continuously stirring the mixed system under the condition of 60-90° C. in a water bath, cooling the mixed system to 20±5° C. when the aggregate size of nanoparticles in the mixed system is 0.05-10 nm, obtaining a highly active nanoparticle dispersion, and centrifugally filtering and vacuum freeze-drying the highly active nanoparticle dispersion; wherein the mass concentration of the raw acid in the mixed system is 0.01-20%, the mass concentration of the citric acid is 1-30%, and the mass concentration of the alcohol amine is 0.01-30%; the raw acid is one or more of phytic acid, aminotrimethylenephosphonic acid, hydroxyethylidene diphosphonic acid, diethylenetriamine penta-methylenephosphonic acid and hexamethylenediaminetetra-methylenephosphonic acid;

[0008] Preparation method of component B: After mixing the heteropoly acid and pure water of equal mass, stir at 30-60°C until dispersed and melted, slowly add the acrylic acid polymer under stirring and continue stirring for 5-6 hours; stop heating and cool naturally to room temperature;

[0009] The component C is a zinc salt;

[0010] The component D is a neutralizing agent.

[0011] During the preparation of component A, the phosphate monomers in the mixed system gradually polymerize under the condition of 60-90°C in a water bath. The nanoparticles generated by the polymerization of the phosphate monomers are tested using a transmission electron microscope (TEM). Rapid cooling can be performed at a cooling rate of 10±5°C to form a highly active nanoparticle dispersion. This will promote better dispersion of the formed nanoparticles and prevent them from agglomerating; in addition, it will make the nanoparticles smaller and more uniform in size. If the food is solid, a freezer can be used to quickly freeze and cool it down.

[0012] During the preparation of component B: vigorous stirring for 1-2 hours is usually required to obtain a dispersed and molten state of heteropolyacid-water.

[0013] By using the treating agent for forming a chemical film layer on the metal surface provided by the present invention to treat the metal substrate, a color film layer can be formed on the metal surface.

[0014] According to some embodiments disclosed in the present invention, the mass percentage of each component in the treating agent is: component A 1.5%, the total amount of acrylic acid polymer and heteropoly acid in component B is 10%, zinc salt 2.5%, sodium hydroxide 1.5%, and the balance is water; or, component A 2%, the total amount of acrylic acid polymer and heteropoly acid in component B is 12%, zinc salt 3%, sodium hydroxide 2%, and the balance is water; or, component A 2%, the total amount of acrylic acid polymer and heteropoly acid in component B is 14%, zinc salt 3%, sodium hydroxide 1.5%, and the balance is water.

[0015] According to some embodiments disclosed in the present invention, the raw acid can be a mixture of aminotrimethylenephosphonic acid and hydroxyethylidene diphosphonic acid in a mass ratio of 3:2, or a mixture of diethylenetriaminepenta(methylenephosphonic acid), hexamethylenediaminetetra(methylenephosphonic acid) and phytic acid in a mass ratio of 3:3:4.

[0016] The alcoholamine may be one or more of monoethanolamine, diethanolamine and triethanolamine.

[0017] The heteropolyacid, also known as polyoxometalate, is an oxygen-containing polyacid compound formed by condensation and dehydration of different types of inorganic oxygen-containing acid anions. Heteropolyacids are composed of heteroatoms (such as phosphorus, silicon, iron, cobalt, etc.) and polyatoms (such as molybdenum, tungsten, vanadium, niobium, etc.) in a certain structure. According to some embodiments disclosed in the present invention, the heteropolyacid may be one or more of phosphotungstic acid, phosphomolybdic acid, silicotungstic acid and silicomolybdic acid. Specifically, the heteropolyacid is a mixture of phosphotungstic acid and phosphomolybdic acid in a ratio of 1.5:1. According to some embodiments disclosed in the present invention, the heteropolyacid may be a mixture of phosphotungstic acid and silicotungstic acid in a ratio of 1.5:1, or a mixture of phosphotungstic acid and phosphomolybdic acid in a mass ratio of 1.5:1, or a mixture of phosphotungstic acid, phosphomolybdic acid and silicomolybdic acid in a ratio of 2:1:1.

[0018] Acrylic acid polymer is a polymer of acrylic acid and its derivatives, which can form stable compounds with metal ions such as zinc ions, calcium ions, and magnesium ions. According to some embodiments disclosed in the present invention, the acrylic acid polymer can be one or more of polyacrylic acid, polyhydrolyzed maleic acid, phosphinohydrolyzed polymaleic anhydride, acrylic acid-hydroxypropyl acrylate copolymer, maleic acid-acrylic acid copolymer, carboxylate-sulfonate-nonionic terpolymer, acrylic acid-acrylate-phosphonic acid-sulfonate tetrapolymer, polyepoxysuccinic acid and phosphonocarboxylic acid copolymer. Among them, polyacrylic acid is a water-soluble high molecular polymer, and its molecular formula is as follows:

[0019]

[0020] According to some embodiments disclosed in the present invention, the acrylic polymer can be a mixture of polyacrylic acid, polyhydrolyzed maleic acid, and phosphino-hydrolyzed polymaleic anhydride in a mass ratio of 4:1.5:2, or a mixture of acrylic acid-hydroxypropyl acrylate copolymer, maleic acid-acrylic acid copolymer, and carboxylate-sulfonate-nonionic terpolymer in a mass ratio of 4:3:2.5, or a mixture of polyacrylic acid, acrylic acid-acrylate-phosphonic acid-sulfonate tetrapolymer, and polyepoxysuccinic acid in a mass ratio of 3:2:5.

[0021] According to some embodiments disclosed in the present invention, the zinc salt may be one or more of zinc oxide, zinc nitrate and zinc sulfate. Specifically, the zinc salt may be a mixture of zinc nitrate and zinc sulfate in a mass ratio of 2:1, or a mixture of zinc nitrate and zinc sulfate in a mass ratio of 1:1.

[0022] According to some embodiments disclosed in the present invention, the neutralizing agent may be one or more of sodium hydroxide, potassium hydroxide and ammonia water.

[0023] The method for preparing the treating agent for forming a chemical film layer on the metal surface comprises the following steps:

[0024] 1) Stir water, component A and component B in a water bath at 65±5℃ until they are evenly mixed;

[0025] 2) Add component C to the mixed solution obtained in step (1), and continue stirring until the mixture is uniformly mixed;

[0026] 3) Add component D to the mixed solution obtained in step (2) and adjust the pH to 4.0±1.

[0027] According to some embodiments disclosed in the present invention, the stirring time of step (1) is 10±0.5 hours; the stirring time of step (2) is 5±0.5 hours.

[0028] The method for using the above-mentioned treatment agent for forming a chemical film layer on a metal surface comprises the following steps:

[0029] (1) Pretreatment: Degrease the surface of the metal substrate to be treated, and then rinse it with tap water after the oil on the surface of the metal substrate is completely removed;

[0030] (2) Soaking: Place the pretreated metal substrate in the treatment agent and soak for 5-10 minutes;

[0031] (3) The metal substrate after immersion is taken out, washed with water, and then air-dried or baked, so that a corrosion-resistant film is obtained on the surface of the metal substrate, and the film layer is colorful.

[0032] The beneficial effects of the present invention are:

[0033] (1) Innovatively, acrylic polymer and zinc salt are combined on the metal surface to form a polymer for protection. At the same time, a phosphate ester nanoparticle is synthesized. In addition to chelating with metal ions, the phosphate ester nanoparticle can also be evenly distributed on the metal surface, increasing the surface roughness and enhancing the ability to combine with subsequent paint films.

[0034] (2) The heteropoly acid is introduced in the field of metal surface treatment in a cutting-edge manner. As an excellent strong proton acid, it is often used in the field of catalysts. Its introduction into the system of the present invention can enhance the adsorption ability of phosphate nanoparticles on the metal surface, thereby enhancing the subsequent adhesion ability to the paint film. DETAILED DESCRIPTION

[0035] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0036] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0037] Example 1 (cold rolled steel sheet)

[0038] Preparation of phosphate nanoparticles: adding citric acid to a raw acid aqueous solution, adding alcohol amine after the citric acid is dissolved to obtain a mixed system, continuously stirring the mixed system in a water bath at 60-90°C, rapidly cooling the mixed system to 20°C at a cooling rate of 10°C / min when the aggregate size of the nanoparticles in the mixed system is 0.05-10nm, and obtaining a highly active nanoparticle dispersion liquid, and the highly active nanoparticle dispersion liquid is centrifugally filtered and vacuum freeze-dried; the mass concentration of the raw acid in the mixed system is 3%, the mass concentration of the citric acid is 5%, and the mass concentration of the alcohol amine is 8%; wherein the raw acid is phytic acid; the alcohol amine is composed of monoethanolamine and triethanolamine in a ratio of 1:1;

[0039] Preparation of acrylate and heteropoly acid composite modified material: After mixing the heteropoly acid with pure water of equal mass, stir at a temperature of 30-60°C until dispersed and melted, slowly add the acrylic polymer under stirring and continue stirring for 5-6 hours; stop heating and cool naturally to room temperature; the acrylic polymer is a mixture of polyacrylic acid, polyhydrolyzed maleic acid, and phosphino-hydrolyzed polymaleic anhydride in a mass ratio of 4:1.5:2; the heteropoly acid is a mixture of phosphotungstic acid and phosphomolybdic acid in a mass ratio of 1.5:1;

[0040] Zinc nitrate and zinc sulfate are mixed in a mass ratio of 1:1 as zinc salt; sodium hydroxide is used as a neutralizing agent;

[0041] A treatment agent for forming a chemical film layer on a metal surface is prepared by stirring water, phosphate nanoparticles and a composite modified material of acrylate and heteropoly acid in a water bath at 65±5°C until the mixture is uniform; then zinc salt is added and stirred until the mixture is uniform, and then a neutralizer is added to adjust the pH to 4.0. The mass percentage of each raw material is as follows: phosphate nanoparticles 1.5%, the total amount of acrylic acid polymer and heteropoly acid in the composite modified material of acrylate and heteropoly acid is 10%, zinc salt 2.5%, sodium hydroxide 1.5%, and the balance is water.

[0042] The surface of the cold-rolled steel sheet is degreased, washed with water, and then placed in the above treatment agent for 5 minutes; the cold-rolled steel sheet is taken out of the treatment agent, rinsed with water, and dried naturally or baked to complete the film-forming process. Subsequently, the cold-rolled steel sheet with the film formed on the surface is electrostatically sprayed with a thickness of 60±5 microns, and a corrosion resistance test is performed.

[0043] Example 2 (Galvanized steel sheet)

[0044] A treatment agent for forming a chemical film layer on a metal surface is prepared by the method of Example 1. Compared with Example 1, there are the following differences: the raw acid is a mixture of aminotrimethylenephosphonic acid and hydroxyethylidene diphosphonic acid in a mass ratio of 3:2, the acrylic polymer is a mixture of acrylic acid-hydroxypropyl acrylate copolymer, maleic acid-acrylic acid copolymer, and carboxylate-sulfonate-nonionic terpolymer in a mass ratio of 4:3:2.5, the heteropolyacid is a mixture of phosphotungstic acid and silicotungstic acid in a mass ratio of 1.5:1; the zinc salt is a mixture of zinc nitrate and zinc sulfate in a mass ratio of 2:1; the mass percentage of each raw material is: phosphate nanoparticles 2%, the total amount of acrylic polymer and heteropolyacid in the composite modified material of acrylic acid and heteropolyacid is 12%; zinc salt 3%, sodium hydroxide 2%, and the balance is water.

[0045] The galvanized steel sheet was treated with the treatment agent prepared in this example using the method of Example 1, and a corrosion resistance test was performed.

[0046] Example 3 (5052 aluminum alloy)

[0047] A treatment agent for forming a chemical film layer on a metal surface is prepared by the method of Example 1. Compared with Example 1, there are the following differences: the raw acid is a mixture of diethylenetriaminepenta(methylenephosphonic acid), hexamethylenediaminetetra(methylenephosphonic acid), and phytic acid in a mass ratio of 3:3:4; the acrylic polymer is a mixture of polyacrylic acid, acrylic acid-acrylic acid ester-phosphonic acid-sulfonate tetrapolymer, and polyepoxysuccinic acid in a mass ratio of 3:2:5; the heteropolyacid is a mixture of phosphotungstic acid, phosphomolybdic acid, and silicomolybdic acid in a mass ratio of 2:1:1; the zinc salt is a mixture of zinc nitrate and zinc sulfate in a mass ratio of 2:1; the mass percentage of each raw material is: phosphate nanoparticles 2%, the total amount of acrylic polymer and heteropolyacid in the composite modified material of acrylic ester and heteropolyacid is 14%; zinc salt 3%, sodium hydroxide 1.5%, and the balance is water.

[0048] The method of Example 1 and the treatment agent prepared in this example were used to treat 5052 aluminum alloy, and a corrosion resistance test was performed. The difference from Example 1 is that the immersion time of 5052 aluminum alloy in the treatment agent is 8 minutes.

[0049] Test results:

[0050] The steel surfaces treated in Examples 1-3 were tested for performance, and the test items and results are as follows:

[0051] Table 1: Paint film test results

[0052]

[0053] The test results of the paint film show that the conversion film of the present invention has excellent performance and has the potential for large-scale application.

[0054] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to perform equivalent replacements on parts thereof. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention. Although the above describes the specific implementation methods of the present invention, it is not intended to limit the protection scope of the present invention. Those skilled in the art should understand that, based on the technical solution of the present invention, various modifications or deformations that can be made by those skilled in the art without creative labor are still within the protection scope of the present invention.

Claims

1. A treatment agent for forming a chemical film on a metal surface, characterized in that: There are component A: 1-3%, component B: 8-15%, component C: 10-15%, component D: 2-5%, and the balance is water; the % is the mass percentage; The preparation method of component A comprises the following steps: adding citric acid to a raw acid aqueous solution, adding alcohol amine after the citric acid is dissolved to obtain a mixed system, continuously stirring the mixed system under the condition of 60-90° C. in a water bath, cooling the mixed system to 20±5° C. when the aggregate size of nanoparticles in the mixed system is 0.05-10 nm, obtaining a highly active nanoparticle dispersion, and centrifugally filtering and vacuum freeze-drying the highly active nanoparticle dispersion; wherein the mass concentration of the raw acid in the mixed system is 0.01-20%, the mass concentration of the citric acid is 1-30%, and the mass concentration of the alcohol amine is 0.01-30%; the raw acid is one or more of phytic acid, aminotrimethylenephosphonic acid, hydroxyethylidene diphosphonic acid, diethylenetriamine penta-methylenephosphonic acid and hexamethylenediaminetetra-methylenephosphonic acid; Preparation method of component B: After mixing the heteropoly acid and pure water of equal mass, stir at 30-60°C until dispersed and melted, slowly add the acrylic acid polymer under stirring and continue stirring for 5-6 hours; stop heating and cool naturally to room temperature; The component C is a zinc salt; The component D is a neutralizing agent.

2. The treating agent for forming a chemical film layer on a metal surface according to claim 1, characterized in that: The alcohol amine is one or more of monoethanolamine, diethanolamine and triethanolamine.

3. The treating agent for forming a chemical film layer on a metal surface according to claim 1, characterized in that: The heteropoly acid is one or more of phosphotungstic acid, phosphomolybdic acid, silicotungstic acid and silicomolybdic acid.

4. The treating agent for forming a chemical film layer on a metal surface according to claim 1, characterized in that: The acrylic polymer is one or more of polyacrylic acid, polyhydrolyzed maleic acid, phosphino hydrolyzed polymaleic anhydride, acrylic acid-hydroxypropyl acrylate copolymer, maleic acid-acrylic acid copolymer, carboxylate-sulfonate-nonionic terpolymer, acrylic acid-acrylate-phosphonic acid-sulfonate tetrapolymer, polyepoxysuccinic acid and phosphonocarboxylic acid copolymer.

5. The treating agent for forming a chemical film layer on a metal surface according to claim 1, characterized in that: The zinc salt is one or more of zinc oxide, zinc nitrate and zinc sulfate.

6. The treating agent for forming a chemical film layer on a metal surface according to claim 1, characterized in that: The neutralizing agent is one or more of sodium hydroxide, potassium hydroxide and ammonia water.

7. The treating agent for forming a chemical film layer on a metal surface according to claim 1, characterized in that: The film layer after being formed on the metal surface appears colorful.

8. The method for preparing a treating agent for forming a chemical film layer on a metal surface according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) Stir water, component A and component B in a water bath at 65±5℃ until they are evenly mixed; 2) Add component C to the mixed solution obtained in step (1), and continue stirring until the mixture is uniformly mixed; 3) Add component D to the mixed solution obtained in step (2) and adjust the pH to 4.0±1.

9. The preparation method according to claim 8, characterized in that: The stirring time of step (1) is 10±0.5 hours; the stirring time of step (2) is 5±0.5 hours.

10. The method for using the treating agent for forming a chemical film layer on a metal surface according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Pretreatment: Degrease the surface of the metal substrate to be treated, and then rinse it with tap water after the oil on the surface of the metal substrate is completely removed; (2) Soaking: Place the pretreated metal substrate in the treatment agent and soak for 5-10 minutes; (3) The metal substrate after immersion is taken out, washed with water, and then air-dried or baked, so that a corrosion-resistant film is obtained on the surface of the metal substrate, and the film layer is colorful.