A microporous zinc / cadmium-tin selenide ion exchanger, its preparation method and application

By preparing a three-dimensional microporous zinc/cadmium-tin selenide ion exchanger, the problems of slow exchange rate and low selectivity of existing materials were solved, and the efficient removal of Cs+, Ba2+, Co2+ and Ni2+ was achieved, which is suitable for nuclear waste liquid treatment.

CN116603576BActive Publication Date: 2026-11-17TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310601513.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2026-11-17
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

Existing inorganic ion exchange materials suffer from slow exchange rates, low selectivity, susceptibility to high salt and strong acid conditions, and high costs when treating nuclear waste liquids. They are also difficult to effectively remove radionuclides such as Cs+, Ba2+, Co2+, and Ni2+.

Method used

MSnSe-K material with a three-dimensional microporous structure was prepared by using zinc/cadmium-tin selenide ion exchanger through a stepwise method of eutectic solvothermal synthesis and K+ ion substitution. The material has a large pore size and utilizes the easy migration of K+ and the soft base properties of Se to achieve rapid exchange.

Benefits of technology

This material is stable within a pH range of 0-12 and can rapidly and efficiently adsorb Cs+, Ba2+, Co2+, and Ni2+ with a removal rate of up to 97.5%-100%. It is suitable for the treatment of highly acidic and highly radioactive nuclear waste liquids at a low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116603576B_ABST
    Figure CN116603576B_ABST
Patent Text Reader

Abstract

This invention relates to a microporous zinc / cadmium-tin selenide ion exchanger, its preparation method, and its applications. The molecular formula of this ion exchanger is: K 4‑x (CH3NH3) 0.75x (NH4) 0.25x M2Sn3Se 10 ·(4-x)H2O, where M=Zn or Cd, x=0.3-1; the structure consists of three-dimensional microporous anions [M2Sn3Se 10 ] n 4n‑ Framework and hydrated K distributed in the channels + Composed of ions, methylamine ions, and ammonium ions, with relatively large pore sizes, including hydrated K+. + The ions have a weaker binding to the framework and can bind to Cs. + Ba 2+ Co 2+ Ni 2+ The reaction involves an exchange process. This invention uses a eutectic mixture of organic amine hydrochloride and N,N'-dimethylurea as the reaction medium, promoting the dissolution of reactants, resulting in a rapid and short reaction time. The resulting material does not contain precious metals, thus reducing cost. Utilizing K... + By replacing organic amines and ammonium cations in the precursors, the resulting material has a fast exchange rate and high removal rate, making it suitable for emergency treatment of large-scale water bodies containing radioactive ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical fields:

[0001] This invention belongs to the field of water treatment involving cesium, barium, cobalt, and nickel elements, specifically relating to a method for treating Cs. + Ba 2+ Co 2+ Ni 2+ Microporous selenide ion exchangers with ion adsorption function, their preparation methods and applications. Background technology:

[0002] Properly handling and disposing of high-level radioactive waste is a crucial step in achieving a safe nuclear fuel cycle and promoting the green and efficient development of nuclear energy. It is also a key task in implementing nuclear safety and radioactive pollution prevention measures. (The waste contains fission products.) 137 Cs(t 1 / 2 =30.2 years), 133 Ba(t 1 / 2 =10.5 years) and neutron activation products 60 Co(t 1 / 2 =5.27 years), 63 Ni(t 1 / 2 =101.2 years) is a radioactive isotope with extremely high biotoxicity, usually in the form of cationic Cs + Ba 2+ Co 2+ Ni 2+ Its presence poses a significant risk of contaminating aquatic systems such as groundwater, rivers, lakes, and oceans, endangering human health. Removal from nuclear wastewater... 137 Cs、 133 Ba、 60 Co、 63 Ni is of great significance. On the one hand, the current disposal of high-level radioactive waste liquids still involves vitrification followed by deep geological landfilling, while the disposal of high-level radioactive waste liquids... 137 Cs releases a large amount of heat during decay, requiring a larger geological disposal space to ensure safety (Energies, 2019, 12, 596-618; Energies 2019, 12, 2052-2079). If... 137 Separating Cs can effectively reduce the calorific value of high-level radioactive waste, increase the effective capacity of deep geological disposal facilities, and reduce the dangers associated with long-term storage (Nuclear Chemistry and Radiochemistry, 2019, 41, 27-39). On the other hand, a sudden nuclear accident can lead to the continuous leakage of large amounts of soluble radioactive material. Once ingested by humans... 137 Cs can spread through bodily fluids and cause damage or death to cells and soft tissues (J. Environ. Chem. Eng., 2018, 6, 5845-5854), while 133Ba, like calcium, preferentially accumulates in bone, thus inducing diseases with high mortality rates such as leukemia and bone cancer (Ind. Eng. Chem. Res., 2017, 56, 13866-13873). 60 Co、 63 Ni accumulation can affect the blood system by reducing white blood cell count, increasing the risk of diseases such as aplastic anemia and even death (Appl. Surf. Sci., 2019, 466, 903-910; J. Hazard. Mater., 2019, 369, 226-235). Therefore, whether for the safe disposal of high-level radioactive waste or to improve nuclear accident emergency response mechanisms, efficient removal of radioactive isotopes from nuclear waste is crucial. 137 Cs、 133 Ba、 60 Co、 63 Ni is one of the key issues that urgently need to be addressed in the field of nuclear safety technology.

[0003] Currently, Cs is extracted from aqueous solutions. + Ba 2+ Co 2+ Ni 2+ Ion exchange methods mainly include precipitation, extraction, membrane filtration, biological treatment, adsorption, and ion exchange (Sep. Purif. Technol. 2017, 188, 523-529; Energies 2020, 13, 3284). Among these, ion exchange has received widespread attention due to its advantages such as high recovery rate, good purification effect, simple operation, and no secondary pollution. Compared with organic exchange resins, inorganic ion exchange materials have better heat resistance and radiation resistance, which is a significant advantage for treating nuclear waste liquids. They are commonly used for enriching Cs. + Ba 2+ Co 2+ Ni 2+ Inorganic exchangers for plasma exchange include clay, zeolite, titania silicate, and metal sulfides (Appl. Clay Sci. 2019, 179, 105-151; Environ. Sci. Pollut. Res. 2020, 27, 6824-6836; J. Environ. Manage. 2022, 309, 114-685). However, traditional inorganic materials suffer from slow exchange rates and low selectivity, and are susceptible to degradation, pulverization, and deactivation during use due to high salt and strong acid environments, making them unsuitable for ion exchange column operations (Chem. Sci. 2016, 7, 4804-4824; Inorg. Chem. 2019, 58, 10184-10193). Therefore, there is an urgent need to develop an ion exchange material with high adsorption activity and good acid resistance to achieve the adsorption of Cs.+ Ba 2+ Co 2+ Ni 2+ Rapid enrichment of radioactive nuclides.

[0004] Metal selenide exchangers are microporous materials composed of a selenide anionic framework and countercations. They can efficiently adsorb soft acidic ions and have strong acid corrosion resistance, making them a promising class of ion exchangers. However, research on them is still in its early stages. Chinese invention patent CN 101985106 B discloses a method for adsorbing Cs... + Microporous silver-tin selenide materials with adsorption properties. However, this material has the following three limitations: (1) This silver-tin selenide material is synthesized by the reaction of AgCl, Sn, and Se, which involves the use of the noble metal Ag, resulting in high cost; (2) The solvent used in the preparation of this silver-tin selenide is volatile N,N'-dimethylformamide, which has poor solubility for inorganic reaction raw materials and slow reaction rate; (3) This silver-tin selenide material uses organic amines as countercations. Our recent research found that the hydrogen bonding between organic amine cations and anionic frameworks is strong, resulting in poor adsorption of Cs by the material. + The exchange rate is relatively slow, requiring 6-8 hours to reach adsorption equilibrium (Inorg.Chem.2020,59,9638-9447); (4) The pore size of this silver-tin selenide crystal is small, which makes it difficult to reach the adsorption equilibrium of +2 valence metal ions with larger hydration radii, such as Ba. 2+ Co 2+ Ni 2+ It lacks adsorption activity. Therefore, this type of silver-tin selenide material has disadvantages such as high preparation cost, long reaction time, low adsorption rate, and narrow ion applicability range. Summary of the Invention:

[0005] The purpose of this invention is to address the problems existing in the above-mentioned development by providing a zinc / cadmium-tin selenide ion exchanger, its preparation method, and its application. This exchanger utilizes zinc powder (or cadmium chloride hemipentahydrate), tin powder, and selenium powder as raw materials, and a eutectic formed from trimethylamine hydrochloride (or diethylamine hydrochloride) and N,N'-dimethylurea as the reaction medium to prepare a zinc / cadmium-tin selenide precursor containing methylamine ions and ammonium ions, which is then subjected to K... + Ion substitution treatment was used to prepare a new type of three-dimensional microporous zinc / cadmium-tin selenide ion exchanger with a novel structural composition, the general structural formula being K. 4-x (CH3NH3) 0.75x (NH4) 0.25x M2Sn3Se 10 ·3,4H₂O (denoted as MSnSe⁻K; where M = Zn or Cd, x = 0.3-1). The structure consists of three-dimensional microporous anions [M₂Sn₃Se⁻]. 10 ]n 4n- Framework and hydrated K distributed in the channels + Composed of ions, methylamine ions, and ammonium ions, with relatively large pore sizes, including hydrated K+. + The ions have a weaker binding to the framework and can bind to Cs. + Ba 2+ Co 2+ Ni 2+ The reaction involves an exchange process. This invention uses a eutectic mixture of organic amine hydrochloride and N,N'-dimethylurea as the reaction medium, promoting the dissolution of reactants, resulting in a rapid and short reaction time. The resulting material does not contain precious metals, thus reducing cost. Utilizing K... + By replacing organic amines and ammonium cations in the precursors, the resulting material has a fast exchange rate and high removal rate, making it suitable for emergency treatment of large-scale water bodies containing radioactive ions.

[0006] The technical solution of the present invention is as follows:

[0007] A microporous zinc / cadmium-tin selenide ion exchanger, its preparation method, and its application. The molecular formula of the ion exchanger is: K 4-x (CH3NH3) 0.75x (NH4) 0.25x M2Sn3Se 10 ·(4-x)H2O, denoted as MSnSe-K; where M = Zn or Cd, x = 0.3-1;

[0008] All M in the aforementioned exchanger II (M = Zn or Cd), Sn IV Each atom adopts a tetrahedral coordination mode to coordinate with four Se atoms. These four {(M / Sn)Se4} tetrahedral building units further condense and aggregate through shared vertices to form {(M / Sn)4Se} with a zincblende configuration. 10 Supertetrahedral clusters, which are assembled with bridging metal atoms in an alternating 4,4-connected manner to form [M2Sn3Se] with a microporous structure. 10 ] n 4n- Framework, pore size 0.4–0.6 nm, hydrated K + As counteracting cations, they fill the pores of the framework, together forming the MSnSe-K lattice structure.

[0009] A method for preparing a zinc / cadmium-tin selenide ion exchanger, the method comprising the following steps:

[0010] (1) Substance A and N,N'-dimethylurea are stirred to form a eutectic. Then, substance B, tin powder, selenium powder, and hydrazine hydrate (98%) are added to the eutectic medium and stirred for 1-20 minutes to ensure uniform mixing. The mixture is then transferred to a reaction vessel and reacted at 120-200℃ for 1-5 days. After natural cooling to room temperature, the initial product is washed and then naturally dried to obtain the crystalline precursor (CH3NH3)3NH4M2Sn3Se. 10 M = Zn or Cd;

[0011] Substance A is trimethylamine hydrochloride or diethylamine hydrochloride, and substance B is zinc powder or cadmium chloride hemipentahydrate; wherein the molar ratios are: substance A: N,N'-dimethylurea = 1:1-3; substance B: tin powder: selenium powder = 1:1-3:3-10; substance B: substance A = 1:2-10; substance A: hydrazine hydrate = 1:0.5-2;

[0012] (2) The obtained precursor was soaked in KCl solution and stirred for 4-24 h. After filtration, washing and drying, zinc / cadmium-tin selenide ion exchanger was obtained.

[0013] The purity of hydrazine hydrate in step (1) is 98%;

[0014] In step (2), the concentration of the KCl solution is 0.1-3M.

[0015] The zinc / cadmium-tin selenide ion exchanger described above is used for the adsorption of Cs. + Ba 2+ Co 2+ and Ni 2+ ion;

[0016] Specifically, one of the following three methods:

[0017] Method 1, batch adsorption, includes the following steps:

[0018] The ion exchanger is added to the solution to be treated and stirred for 1 min to 24 h to complete the adsorption of the target ions;

[0019] The solution to be treated contains Cs + Ba 2+ Co 2+ and Ni 2+ One or more of the ions;

[0020] In the solution to be treated, Cs + Ba 2+ Co 2+ and Ni 2+ The concentration range of the ions is 0.5-8000 ppm;

[0021] In the adsorption method described above, the ratio of solution volume to exchange resin mass is 300-3000 mL / g. -1 ;

[0022] The MSnSe-K ion exchanger adsorbs Cs + Ba 2+ Co 2+ and Ni 2+ The ion temperature is 5-60℃, with 20℃ being preferred;

[0023] Alternatively, method two, ion exchange column adsorption, includes the following steps:

[0024] The ion exchanger is filled into a glass chromatography column as a stationary phase, and the solution to be treated flows through the chromatography column to complete the adsorption of the target ion.

[0025] Among them, each 1cm 3 The flow rate of the stationary phase treatment solution is 0.1-5 mL / min. -1 ;

[0026] The solution to be treated contains Cs + Ba 2+ Co 2+ and Ni 2+ One or more ions, with the concentration range of each ion being 0.5-3000 ppm;

[0027] Alternatively, method three, microporous membrane adsorption, includes the following steps:

[0028] The ion exchanger was ball-milled to prepare a powder with a particle size of 1-10 μm, and then mixed with 10-100 mg / mL of water. -1 The N-methylpyrrolidone solution of polyvinylidene fluoride is mixed and stirred for 1-60 min. The mixture is then taken out, uniformly coated on the surface of the aqueous PTFE microporous filter membrane substrate, and allowed to air dry naturally for 2-30 h to prepare the MSnSe-K / PTFE microporous filter membrane.

[0029] The mass ratio of ball-milled ion exchanger to polyvinylidene fluoride is 5-40:1.

[0030] The thickness of the aqueous PTFE microporous filter membrane substrate is 30-200 μm;

[0031] In the MSnSe-K / PTFE microporous filter membrane, the thickness of the MSnSe-K ion exchanger layer is 10-200 μm;

[0032] Under reduced pressure filtration conditions, the solution to be treated is allowed to flow through a microporous filter membrane to complete the adsorption of target ions;

[0033] per 1cm 2 The flow rate of the MSnSe-K / PTFE microporous membrane treatment solution was 0.5-2.5 mL / min. -1 ;

[0034] The solution to be treated contains Cs + Ba 2+ Co 2+ and Ni 2+ One or more ions, with the concentration range of each ion being 0.5-3000 ppm;

[0035] Methods 1, 2, and 3 are described below.

[0036] The solution to be treated also contains Na. + K + Mg 2+ Ca 2+ One or more of the ions, with a concentration range of 0-1000 mmol / L -1 .

[0037] The solution to be treated also contains Fe3+. + Al + Eu 3+ UO2 2- One or more of the ions, with a concentration range of 0-100 ppm.

[0038] The solution to be treated is deionized water, drinking water, tap water, lake water, or industrial wastewater.

[0039] Optionally, the desorption method of the ion exchanger:

[0040] In method one or method two, MSnSe-K exchanger is used to extract Cs. + Ba 2+ Co 2+ Ni 2+ After removing one or more of the ions, immerse the sample in a 0.5-3M KCl solution for 0.5-12 hours to complete the elution. Then remove the sample, wash and dry it for reuse.

[0041] In method three, Cs is extracted using an MSnSe-K / PTFE microporous membrane. + Ba 2+ Co 2+ Ni 2+ After removing one or more of the ions, under reduced pressure filtration, a 0.5-3M KCl solution is passed through the filter membrane for 0.5-12 hours to complete the elution. The membrane is then washed with deionized water, removed, dried, and reused.

[0042] The essential features of this invention are:

[0043] The preparation process of the MSnSe-K ion exchanger of this invention does not involve the use of precious metals, thus reducing costs; it utilizes a eutectic based on organic amines and N,N'-dimethylurea as the reaction medium to promote reactant dissolution and accelerate the reaction rate; the MSnSe-K ion exchanger is a microporous selenide material, and due to the formation enthalpy of H2Se (+73 kJ mol)... -1 The concentration of H2S was significantly higher than that of H2S (-20.1 kJ / mol). -1 ) and H2O (-285.6kJ mol) -1 This gives the material the ability to resist corrosion from acidic media and remain stable within a pH range of 0-12; the soft alkaline properties of Se and K... + The easy migration and substitution characteristics of MSnSe-K exchanger make it suitable for Cs + Ba 2 + Co 2+ Ni 2+ It exhibits extremely high adsorption rate, selectivity, and adsorption capacity. Under conditions of batch adsorption, column filtration, and membrane filtration (with an average solid-liquid contact time of only 1.6-8.2 s), the removal rate at adsorption equilibrium can reach 97.5%-100%.

[0044] The beneficial effects of this invention are as follows:

[0045] 1. This invention utilizes a eutectic solvothermal synthesis method to synthesize —K + The stepwise method of ion substitution is used to prepare selenide ion exchangers, which is easy to prepare and has good reproducibility.

[0046] 2. This invention uses zinc powder (or cadmium chloride hemipentahydrate), tin powder, and selenium powder as the main raw materials to synthesize metal selenides that do not contain precious metals, resulting in lower costs.

[0047] 3. The microporous selenide ion exchanger prepared by this invention has a large pore size, which is beneficial for Cs. + Ba 2+ Co 2+ Ni 2+ It exhibits good adsorption effects on various ions and has good versatility.

[0048] 4. The microporous selenide ion exchanger prepared by this invention has a rapid adsorption rate and a high removal rate, capable of removing >99.3% of 6ppm Cs within 2 minutes. + It can remove more than 97.5% of 6ppm Ba within 10-60 minutes. 2+ Co 2+ Ni 2+ It is suitable for emergency treatment of large-scale water bodies containing radioactive ions.

[0049] 5. The microporous selenide ion exchanger prepared by this invention has good stability under pH = 0-12 and 200kGy β and γ irradiation, and is suitable for the treatment and disposal of highly acidic and highly radioactive nuclear waste liquids at home and abroad.

[0050] 6. The microporous selenide ion exchanger prepared by this invention can be used for column filtration and membrane filtration, and can be used for mixing Cs in a continuous flow solution. + Ba 2+ Co 2+ Ni 2+ The ion removal rate is higher than 99%. In particular, the MSnSe-K / PTFE membrane can remove Cs ions in an extremely short solid-liquid contact time (<3.3s). + Ions are removed efficiently, with a removal rate exceeding 99.9%. Attached image description:

[0051] Figure 1 This document presents a flowchart and magnified images of the preparation process of MSnSe-K (M = Zn or Cd) ion exchanger when x = 0.6, as described in this invention. Figure 1 (a) in the diagram is a flowchart of the preparation process of ZnSnSe-K ion exchanger. Figure 1 Image (b) shows the appearance and magnified morphology of the ZnSnSe-K ion exchanger. Figure 1 (c) in the diagram is the preparation flow chart of CdSnSe-K ion exchanger. Figure 1 (d) in the image shows the appearance and magnified morphology of the CdSnSe-K ion exchanger.

[0052] Figure 2 The image shows the crystal structure of the MSnSe-K (M = Zn or Cd) ion exchanger used in this invention. Figure 2 (a) shows the connection modes between the central supertetrahedral cluster and the four surrounding metal atoms, as well as the connection modes between the central metal atom and the four surrounding supertetrahedral clusters. Figure 2 (b) in the example is [M2Sn3Se 10 ] n 4n- An open framework structure Figure 2 (c) and (d) in the diagram represent right-handed helical (R) and left-handed helical (L) channels that intersect perpendicularly along the a-axis and b-axis, respectively. For clarity, K in the channel is shown. + Ions and crystalline H2O molecules are not shown.

[0053] Figure 3 This is the energy-dispersive X-ray spectrum of the MSnSe-K (M = Zn or Cd) ion exchanger when x = 0.6 in this invention, wherein... Figure 3Image (a) is the energy-dispersive X-ray spectrum of the ZnSnSe-K ion exchanger. Figure 3 (b) is the energy-dispersive X-ray spectrum of the CdSnSe-K ion exchanger.

[0054] Figure 4 This is the thermogravimetric curve of MSnSe-K (M = Zn or Cd) ion exchanger when x = 0.6 in this invention, under argon atmosphere and heating rate of 10℃ / min. -1 ,in, Figure 4 (a) in the figure is the thermogravimetric curve of ZnSnSe-K ion exchanger. Figure 4 (b) in the figure is the thermogravimetric curve of CdSnSe-K ion exchanger.

[0055] Figure 5 The MSnSe (M = Zn or Cd) precursor (including single-crystal simulation), MSnSe-K (M = Zn or Cd, x = 0.6) ion exchanger, and their Cs are used in this invention. + Ba 2+ Co 2+ Ni 2+ XRD patterns of saturated exchange products MSnSe-Cs, MSnSe-Ba, MSnSe-Co, and MSnSe-Ni, among which... Figure 5 (a) represents ZnSnSe precursors (including single-crystal simulations), ZnSnSe-K ion exchangers, and their Cs. + Ba 2+ Co 2+ and Ni 2+ XRD patterns of saturated exchange products ZnSnSe-Cs, ZnSnSe-Ba, ZnSnSe-Co, and ZnSnSe-Ni. Figure 5 (b) represents the CdSnSe precursor (including single-crystal simulation), CdSnSe-K ion exchanger, and its Cs. + Co 2+ and Ni 2+ XRD patterns of saturated exchange products CdSnSe-Cs, CdSnSe-Co, and CdSnSe-Ni.

[0056] Figure 6 The images show the XRD patterns of the MSnSe-K (M = Zn or Cd, x = 0.3, 0.6) ion exchanger used in this invention before and after irradiation with 200 kGy β and 100 kGy γ rays. Figure 6 (a) shows the XRD patterns of ZnSnSe-K (x = 0.3, 0.6) ion exchangers before and after irradiation with 200 kGy β rays. Figure 6(b) shows the XRD patterns of ZnSnSe-K (x = 0.3, 0.6) ion exchangers before and after irradiation with 100 kGy γ rays. Figure 6 (c) shows the XRD patterns of CdSnSe-K (x = 0.3, 0.6) ion exchangers before and after irradiation with 200 kGy β rays. Figure 6 (d) in the figure represents the XRD patterns of CdSnSe-K (x = 0.3, 0.6) ion exchangers before and after irradiation with 100 kGy γ rays.

[0057] Figure 7 The ZnSnSe precursor and ZnSnSe-K (x = 0.6) ion exchanger used in this invention for Cs + Graph showing the change in ion removal rate over time and t / q t A graph showing the changes over time, where, Figure 7 In the diagram, (a) represents the ZnSnSe precursor and the ZnSnSe-K (x = 0.6) ion exchanger for Cs. + Graph showing the change in ion removal rate over time. Figure 7 (b) in the equation represents t / q. t A graph showing the change over time.

[0058] Figure 8 The ZnSnSe precursor and ZnSnSe-K (x = 0.6) ion exchanger used in this invention for Ba 2+ Graph showing the change in ion removal rate over time and t / q t A graph showing the changes over time, where, Figure 8 In the diagram, (a) represents the interaction between the ZnSnSe precursor and the ZnSnSe-K (x = 0.6) ion exchanger on Ba. 2+ Graph showing the change in ion removal rate over time. Figure 8 (b) in the equation represents t / q. t A graph showing the change over time.

[0059] Figure 9 The ZnSnSe precursor and ZnSnSe-K (x = 0.6) ion exchanger used in this invention for Co 2+ Graph showing the change in ion removal rate over time and t / q t A graph showing the changes over time, where, Figure 9 In the diagram, (a) represents the interaction between the ZnSnSe precursor and the ZnSnSe-K (x = 0.6) ion exchanger for Co. 2+ Graph showing the change in ion removal rate over time. Figure 9 (b) in the equation represents t / q. t A graph showing the change over time.

[0060] Figure 10The ZnSnSe precursor and ZnSnSe-K (x = 0.6) ion exchanger used in this invention for Ni 2+ Graph showing the change in ion removal rate over time and t / q t A graph showing the changes over time, where, Figure 10 In the diagram, (a) represents the interaction between the ZnSnSe precursor and the ZnSnSe-K (x = 0.6) ion exchanger on Ni. 2+ Graph showing the change in ion removal rate over time. Figure 10 (b) in the equation represents t / q. t A graph showing the change over time.

[0061] Figure 11 The CdSnSe precursor and CdSnSe-K (x = 0.6) ion exchanger used in this invention for Cs + Graph showing the change in ion removal rate over time and t / q t A graph showing the changes over time, where, Figure 11 In the diagram, (a) represents the CdSnSe precursor and CdSnSe-K (x = 0.6) ion exchanger for Cs. + Graph showing the change in ion removal rate over time. Figure 11 (b) in the equation represents t / q. t A graph showing the change over time.

[0062] Figure 12 The CdSnSe precursor and CdSnSe-K (x = 0.6) ion exchanger used in this invention for Co 2+ Graph showing the change in ion removal rate over time and t / q t A graph showing the changes over time, where, Figure 12 In the diagram, (a) represents the interaction between the CdSnSe precursor and the CdSnSe-K (x = 0.6) ion exchanger for Co. 2+ Graph showing the change in ion removal rate over time. Figure 12 (b) in the equation represents t / q. t A graph showing the change over time.

[0063] Figure 13 The CdSnSe precursor and CdSnSe-K (x = 0.6) ion exchanger used in this invention for Ni 2+ Graph showing the change in ion removal rate over time and t / q t A graph showing the changes over time, where, Figure 13 In the image (a), the reaction between the CdSnSe precursor and the CdSnSe-K (x=0.6) ion exchanger on Ni... 2+ Graph showing the change in ion removal rate over time. Figure 13 (b) in the equation represents t / q. t A graph showing the change over time.

[0064] Figure 14 In this invention, when x = 0.6, the ZnSnSe-K ion exchanger for Cs... + Ba 2+ Co 2+ Ni 2+ Isothermal adsorption curves of ions and fitting results, among which, Figure 14 (a) in the figure represents the ZnSnSe-K ion exchanger for Cs + Isothermal adsorption curves of ions and fitting results. Figure 14 (b) shows the effect of ZnSnSe-K ion exchanger on Ba. 2+ Isothermal adsorption curves of ions and fitting results. Figure 14 (c) represents the ZnSnSe-K ion exchanger for Co. 2+ Isothermal adsorption curves of ions and fitting results. Figure 14 (d) represents the ZnSnSe-K ion exchanger for Ni 2+ Isothermal adsorption curves of ions and fitting results.

[0065] Figure 15 In this invention, when x = 0.6, the CdSnSe-K ion exchanger for Cs... + Co 2+ Ni 2+ Isothermal adsorption curves of ions and fitting results, among which, Figure 15 (a) represents the CdSnSe-K ion exchanger for Cs + Isothermal adsorption curves of ions and fitting results. Figure 15 (b) shows the effect of CdSnSe-K ion exchanger on Co. 2+ Isothermal adsorption curves of ions and fitting results. Figure 15 (c) represents the effect of CdSnSe-K ion exchanger on Ni 2+ Isothermal adsorption curves of ions and fitting results.

[0066] Figure 16 In this invention, when x = 0.3 or 1, the ZnSnSe-K ion exchanger for Cs... + Isothermal adsorption curves of ions and fitting results, among which, Figure 16 When (a) is x = 0.3, the ZnSnSe-K ion exchanger for Cs + Isothermal adsorption curves of ions and fitting results. Figure 16 When (b) is x=1, the ZnSnSe-K ion exchanger for Cs + Isothermal adsorption curves of ions and fitting results.

[0067] Figure 17 In this invention, when x = 0.3 or 1, the CdSnSe-K ion exchanger for Cs...+ Isothermal adsorption curves of ions and fitting results, among which, Figure 17 When (a) is x = 0.3, the CdSnSe-K ion exchanger for Cs + Isothermal adsorption curves of ions and fitting results. Figure 17 When (b) is x=1, the CdSnSe-K ion exchanger for Cs + Isothermal adsorption curves of ions and fitting results.

[0068] Figure 18 The ZnSnSe-K (x=0.6) ion exchanger and Cs in this invention are... + Saturated exchange products ZnSnSe-Cs, Ba 2+ Saturated exchange products ZnSnSe-Ba, Co 2+ Saturated exchange products ZnSnSe-Co, Ni 2+ SEM images and elemental distribution diagrams of the saturated exchange products ZnSnSe-Ni.

[0069] Figure 19 The ZnSnSe-K (x=0.6) ion exchanger used in this invention is for Cs + Ba 2+ Co 2+ Ni 2+ Energy-dispersive X-ray spectra of saturated exchange products, wherein... Figure 19 (a) in the text is Cs + Energy-dispersive X-ray spectra of the saturated exchange product ZnSnSe-Cs. Figure 19 (b) in the middle is Ba 2+ Energy-dispersive X-ray spectra of the saturated exchange product ZnSnSe-Ba. Figure 19 (c) in the text represents Co. 2+ Energy-dispersive X-ray spectra of the saturated exchange product ZnSnSe-Co. Figure 19 (d) in the figure represents Ni 2+ Energy dispersive X-ray spectrum of saturated exchange product ZnSnSe-Ni.

[0070] Figure 20 The CdSnSe-K (x=0.6) ion exchanger and Cs in this invention are... + Saturated exchange products CdSnSe-Cs, Co 2+ Saturated exchange products CdSnSe-Co, Ni 2+ SEM images and elemental distribution diagrams of the saturated exchange product CdSnSe-Ni.

[0071] Figure 21 The CdSnSe-K (x=0.6) ion exchanger in this invention is used for Cs+ Co 2+ Ni 2+ Energy-dispersive X-ray spectra of saturated exchange products, wherein... Figure 21 (a) in the text is Cs + Energy-dispersive X-ray spectra of the saturated exchange product CdSnSe-Cs. Figure 21 (b) in the text is Co 2+ Energy-dispersive X-ray spectra of the saturated exchange product CdSnSe-Co. Figure 21 (c) in the text represents Ni. 2+ Energy dispersive X-ray spectrum of the saturated exchange product CdSnSe-Ni.

[0072] Figure 22 The ZnSnSe-K (x=0.6) ion exchanger in this invention is used for single Cs + Ba 2+ Co 2+ Ni 2+ The trend of the partition coefficient of ion adsorption with solution pH, among which, Figure 22 (a) in the figure represents the ZnSnSe-K (x=0.6) ion exchanger for Cs. + The trend of the partition coefficient of ion adsorption with solution pH. Figure 22 (b) in the figure represents the effect of ZnSnSe-K (x=0.6) ion exchanger on Ba. 2+ The trend of the partition coefficient of ion adsorption with solution pH. Figure 22 (c) in the figure represents the ZnSnSe-K (x=0.6) ion exchanger for Co. 2+ The trend of the partition coefficient of ion adsorption with solution pH. Figure 22 In the figure, (d) represents the ZnSnSe-K (x=0.6) ion exchanger for Ni. 2+ The trend of the partition coefficient of ion adsorption with solution pH.

[0073] Figure 23 The ZnSnSe-K (x=0.6) ion exchanger in this invention was used to treat single Cs under different pH conditions. + XRD patterns before and after ion adsorption.

[0074] Figure 24 The CdSnSe-K (x=0.6) ion exchanger in this invention is for single Cs + Co 2+ Ni 2+ The trend of the partition coefficient of ion adsorption with solution pH, among which, Figure 24 (a) in the figure represents the CdSnSe-K (x=0.6) ion exchanger for Cs +The trend of the partition coefficient of ion adsorption with solution pH. Figure 24 (b) in the figure represents the effect of CdSnSe-K (x=0.6) ion exchanger on Co. 2+ The trend of the partition coefficient of ion adsorption with solution pH. Figure 24 (c) in the figure represents the effect of CdSnSe-K (x=0.6) ion exchanger on Ni 2+ The trend of the partition coefficient of ion adsorption with solution pH.

[0075] Figure 25 The ZnSnSe-K (x=0.6) ion exchanger in this invention is used for single Cs + Ba 2+ Co 2+ Ni 2+ The removal rate of ion adsorption varies with the types and concentrations of coexisting ions in the solution. Figure 25 (a) in the figure represents the ZnSnSe-K (x=0.6) ion exchanger for a single Cs. + The trend of ion adsorption removal rate with the variation of the types and concentrations of coexisting ions in the solution. Figure 25 (b) shows the effect of ZnSnSe-K (x=0.6) ion exchanger on a single Ba group. 2+ The trend of ion adsorption removal rate with the variation of the types and concentrations of coexisting ions in the solution. Figure 25 (c) in the figure represents the ZnSnSe-K (x=0.6) ion exchanger for Co. 2+ The trend of the partition coefficient of ion adsorption with solution pH. Figure 25 In the figure, (d) represents the ZnSnSe-K (x=0.6) ion exchanger for Ni. 2+ The trend of the partition coefficient of ion adsorption with solution pH.

[0076] Figure 26 The CdSnSe-K (x=0.6) ion exchanger in this invention is for single Cs + Co 2+ Ni 2+ The removal rate of ion adsorption varies with the types and concentrations of coexisting ions in the solution. Figure 26 (a) in the figure represents the effect of CdSnSe-K (x=0.6) ion exchanger on a single Cs group. + The trend of ion adsorption removal rate with the variation of the types and concentrations of coexisting ions in the solution. Figure 26 (b) in the figure represents the effect of CdSnSe-K (x=0.6) ion exchanger on Co. 2+ The trend of the partition coefficient of ion adsorption with solution pH. Figure 26 (c) in the figure represents the effect of CdSnSe-K (x=0.6) ion exchanger on Ni2+ The trend of the partition coefficient of ion adsorption with solution pH.

[0077] Figure 27 The ZnSnSe-K (x=0.6) ion exchanger in this invention is used at 2ppm Fe 3+ Al 3+ Eu 3+ and UO2 2+ When it exists for a single Cs + Ba 2+ Co 2+ Ni 2+ (2ppm) Removal rate by ion adsorption.

[0078] Figure 28 The CdSnSe-K (x=0.6) ion exchanger used in this invention is in a 2ppm Fe... 3+ Al 3+ Eu 3+ and UO2 2+ When it exists for a single Cs + Co 2+ Ni 2+ (2ppm) Removal rate by ion adsorption.

[0079] Figure 29 The diagram shows the ion exchange column apparatus filled with ZnSnSe-K (x = 0.6) in this invention and its application to a mixture of Cs. + Ba 2+ Co 2+ Ni 2+ Color change after treatment with a solution (1 ppm for each ion).

[0080] Figure 30 The ion exchange column filled with ZnSnSe-K (x=0.6) in this invention is used to process Cs mixed in solution. + Ba 2+ Co 2+ Ni 2+ (1 ppm for each ion) Trend chart of ion removal rate as a function of bed volume.

[0081] Figure 31 The images show the ZnSnSe-K / PTFE (x=0.6) microporous filter membrane in its flat and bent states, as well as a diagram of the apparatus for applying the ZnSnSe-K / PTFE microporous filter membrane to vacuum filtration.

[0082] Figure 32 This is a SEM image of the cross-section of the ZnSnSe-K / PTFE (x=0.6) microporous filter membrane in this invention.

[0083] Figure 33 The ZnSnSe-K / PTFE (x=0.6) microporous membrane in this invention is used to filter Cs mixed in solution. + Ba 2+ Co 2+ Ni 2+ (1 ppm for each ion) Trend graph of ion removal rate as a function of the volume of the treated solution. Detailed implementation method:

[0084] The present invention will be further explained below with reference to embodiments and accompanying drawings, in order to help readers better understand the technical solutions of the present invention, but the scope of protection of the present invention is not limited thereto.

[0085] Unless otherwise specified, all raw materials used in the examples were purchased commercially and were not further purified or processed.

[0086] The testing method in the embodiments of the present invention is as follows:

[0087] The Rigaku SmartLab 9kW diffractometer is used for powder X-ray diffraction (XRD) testing, specifically Cu-Kα rays.

[0088] The FEI Quanta FEG 250 scanning electron microscope was used to collect energy dispersive X-ray spectra (EDS) and mapping elemental distribution maps.

[0089] The Vista-MPX Varian instrument is used to collect inductively coupled plasma emission spectra (ICP-OES).

[0090] ThermoFisher iCAP RQ instrument is used for inductively coupled plasma mass spectrometry (ICP-MS).

[0091] The removal rate R (%) in the embodiments of the present invention is calculated as follows;

[0092] R = (C0 – C) f ) / C0 × 100% (1)

[0093] In the embodiments of the present invention, the allocation coefficient K d (mL g -1 The calculation method for ) is as follows;

[0094] K d = V / m × (C0 – C f ) / C f × 100% (2)

[0095] The pseudo-quadratic dynamic model in the embodiments of the present invention is expressed by the following formula;

[0096] t / q t = 1 / (k2q) e 2 ) + t / q e (3)

[0097] The Langmuir-Frendlich isothermal adsorption model in the embodiments of the present invention is expressed as follows;

[0098] q e = q m (bC e ) 1 / n / (1 + (bC e ) 1 / n (4).

[0099] In formulas (1) and (2), C0 (ppm) and C f (ppm) are Cs + Ba 2+ Co 2+ Ni 2+ Initial and final concentrations of ions; V (mL) is the volume of the test solution; m (g) is the mass of the ion exchanger; K d (mL g -1 ) is the partition coefficient of ions in the solution.

[0100] In formula (3), t(min) is the adsorption time, and q t (mg g -1 ) and q e (mg g -1 ) are Cs + Ba 2+ Co 2+ Ni 2+ The amount of ion adsorbed at time t and the equilibrium adsorption amount; k2 (g mg) -1 min -1 ) is a pseudo-quadratic rate constant.

[0101] In formula (4), q e (mg g -1 ) and q m (mg g -1 ) are Cs + Ba 2+ Co 2+ Ni 2+ Equilibrium adsorption capacity and maximum adsorption capacity of ions; C e (ppm) is the Cs at adsorption equilibrium. +Ba 2+ Co 2+ Ni 2+ Ion concentration; b (L mg) -1 ) is the Langmuir constant; n is a parameter related to the degree of heterogeneity of the system.

[0102] Example 1: Preparation and product characteristics of MSnSe-K (M = Zn or Cd) ion exchanger (demonstrated through 6 specific preparation examples).

[0103] Example 1-1 Preparation of ZnSnSe-K (x=0.6) ion exchanger

[0104] like Figure 1 As shown in (a), 0.770 g (8 mmol) of trimethylamine hydrochloride and 1.410 g (16 mmol) of N,N'-dimethylurea were mixed and stirred to obtain a eutectic. Then, 0.130 g (2 mmol) of zinc powder, 0.356 g (3 mmol) of tin powder, 0.948 g (12 mmol) of selenium powder and 0.6 mL of 98% hydrazine hydrate (12.34 mmol) were added to the eutectic in sequence and stirred for 5 min to make it homogeneous. Then, it was transferred to a 20 mL reaction vessel and reacted in an oven at 170 °C for 2 days. After the reaction was completed, it was naturally cooled to room temperature. The reaction product was washed with 20 mL of deionized water 3-4 times and then dried naturally in air to obtain 0.965 g of red crystalline ZnSnSe precursor. The yield based on tin element was 69.6%. 0.2 g of ZnSnSe precursor was added to 20 mL of potassium chloride solution (2 M). After stirring at room temperature for 12 h, the solid product was filtered, washed four times with water, and then dried naturally to obtain the product shown below. Figure 1 The ZnSnSe-K (x=0.6) ion exchanger shown in (b) is shown in the figure.

[0105] Examples 1-2 are the same as those in Examples 1-1, except that the concentration of potassium chloride solution in Examples 1-1 is replaced with 0.1M instead of 2M; thus, ZnSnSe-K (x=1) ion exchanger is obtained.

[0106] Examples 1-3 follow the same steps as Examples 1-1, except that the concentration of potassium chloride solution in Examples 1-1 is replaced with 3M instead of 2M; thus, ZnSnSe-K (x=0.3) ion exchanger is obtained.

[0107] Examples 1-4: Preparation of CdSnSe-K (x = 0.6) ion exchanger

[0108] like Figure 1As shown in (c), 0.877 g (8 mmol) of diethylamine hydrochloride and 1.410 g (16 mmol) of N,N'-dimethylurea were mixed and stirred to obtain a eutectic. Then, 0.228 g (1 mmol) of cadmium chloride hemipentahydrate, 0.178 g (1.5 mmol) of tin powder, 0.474 g (6 mmol) of selenium powder, and 0.2 mL of 98% hydrazine hydrate were added to the eutectic in sequence and stirred for 5 min to make it homogeneous. The mixture was then transferred to a 20 mL reactor and reacted in an oven at 160 °C for 3 days. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The reaction product was washed 3-4 times with 20 mL of deionized water and then dried naturally in air to obtain 0.381 g of orange blocky crystalline CdSnSe precursor. The yield was 51.4% based on the tin element. 0.2 g of CdSnSe precursor was added to 20 mL of potassium chloride solution (2 M). After stirring at room temperature for 24 h, the solid product was filtered, washed four times with water, and then dried naturally to obtain the product shown below. Figure 1 The CdSnSe-K (x=0.6) ion exchanger shown in (d) is an example.

[0109] Examples 1-5 follow the same steps as Examples 1-4, except that the concentration of potassium chloride solution in Examples 1-4 is replaced with 0.1M instead of 2M; thus, CdSnSe-K (x=1) ion exchanger is obtained.

[0110] Examples 1-6 follow the same steps as Examples 1-4, except that the concentration of potassium chloride solution in Examples 1-4 is replaced with 3M instead of 2M; thus, CdSnSe-K (x=0.3) ion exchanger is obtained.

[0111] In the above embodiments, the yield = (mass of the obtained MSnSe precursor sample / molecular weight of the precursor × 3) / (moles of tin in the tin source) × 100%.

[0112] like Figure 2 As shown, in the crystal structure of MSnSe-K (M = Zn or Cd, x = 0.3-1) ion exchanger, all metal atoms are coordinated with four Se atoms to form {(M / Sn)Se4} units with a tetrahedral geometry. The four units are connected by a common vertex to form {(M / Sn)4Se4} units with a zincblende geometry. 10 Clusters, further extended into three-dimensional space through equal amounts of M / Sn atoms interacting, forming [M2Sn3Se] through 4,4-connection. 10 ] n 4n- A microporous framework. This framework contains helical channels that intersect perpendicularly and are chiral enantiomers (L and R), filled with hydrated K+. + and CH3NH3 + / NH4 + As a countercation, it, together with the framework, constitutes the complete structure of the MSnSe-K ion exchanger. Among them, hydrated K... + Can be used with Cs + Ba 2+ Co 2+ Ni 2+ Ion exchange is performed.

[0113] Table 1 lists the molecular formulas and mass percentages of each element for ZnSnSe-K and CdSnSe-K ion exchangers (x = 0.3, 0.6, 1) obtained based on ICP-OES, ICP-MS, and C, H, and N elemental analysis techniques. The measured results are in good agreement with the theoretical values. Table 1: Measured values ​​and theoretical values ​​calculated from the molecular formulas of ZnSnSe-K and CdSnSe-K ion exchangers when x = 0.3, 0.6, and 1.

[0114]

[0115] like Figure 3 As shown, the energy-dispersive X-ray spectroscopy confirms that when x = 0.6, the mass and molar percentage of each element in the ZnSnSe-K and CdSnSe-K ion exchangers conform to the molecular formula K. 3.4 (CH3NH3) 0.45 (NH4) 0.15 M2Sn3Se 10 The elemental composition of 3,4H₂O (M = Zn or Cd).

[0116] like Figure 4 As shown, when x = 0.6, the weight loss of ZnSnSe-K and CdSnSe-K ion exchangers in the temperature range of 40-150℃ is 3.84% and 3.63%, respectively, which is basically consistent with the theoretical weight loss of 4.12% and 3.87% of the water of crystallization molecules in the materials. This confirms that the molecular formulas of ZnSnSe-K and CdSnSe-K ion exchangers do indeed contain 3.4 water of crystallization molecules, i.e., K + It exists in the form of hydrated ions.

[0117] like Figure 5As shown, the XRD patterns of the ZnSnSe and CdSnSe precursors are consistent with the spectra fitted by the single crystal data, proving that the prepared ZnSnSe and CdSnSe precursors have high phase purity. The diffraction patterns of the XRD patterns of ZnSnSe-K (x = 0.6) and CdSnSe-K (x = 0.6) ion exchangers are similar to those of the corresponding ZnSnSe and CdSnSe precursors, proving that the anionic framework of the material is still maintained after substitution. Compared with the ZnSnSe and CdSnSe precursors, the (101) diffraction peak of the corresponding ZnSnSe-K (x = 0.6) and CdSnSe-K (x = 0.6) ion exchangers shifts to a higher angle, indicating that the CH3NH3 in the pores is relatively stable. + and NH4 + Cations are K + Substitution leads to a decrease in lattice spacing, i.e., framework shrinkage. Cs was saturated and adsorbed using a ZnSnSe-K (x = 0.6) exchanger. + Ba 2+ Co 2+ Ni 2+ The XRD patterns of the subsequently obtained products ZnSnSe-Cs, ZnSnSe-Ba, ZnSnSe-Co, and ZnSnSe-Ni are very similar to those of ZnSnSe-K, while the CdSnSe-K (x = 0.6) exchanger is used for saturated adsorption of Cs. + Co 2+ Ni 2+ The XRD patterns of the subsequently obtained products CdSnSe-Cs, CdSnSe-Co, and CdSnSe-Ni are very close to those of CdSnSe-K (x = 0.6), proving that K + With Cs + 、Sr 2+ Ion exchange is an isomorphic process.

[0118] like Figure 6 As shown, the XRD patterns of MSnSe-K (M = Zn or Cd; x = 0.3, 0.6) ion exchangers after being subjected to high-intensity irradiation of 200 kGyβ or 100 kGyγ are consistent with those before irradiation, which fully demonstrates that the internal framework structure of the material is well maintained and has excellent radiation resistance.

[0119] Example 2: ZnSnSe-K (x = 0.6) ion exchanger for single Cs + Ba 2+ Co 2+ Ni 2+ Adsorption kinetics of ions.

[0120] When x = 0.6, samples ZnSnSe-K were reacted with 6 ppm of a single Cs-containing solution.+ Ba 2+ Co 2+ Ni 2+ The aqueous solutions of the ions were mixed and stirred continuously at room temperature (20°C) for 1-240 min, V / m = 1000 mL g -1 pH = 6-7. Turbid solutions with different stirring times were filtered and diluted, and the Cs content was determined by ICP-MS. + Ba 2+ Co 2+ Ni 2+ Ion concentration. Adsorption tests using ZnSnSe precursors under the same conditions were used as a reference. For example... Figure 7 (a) Figure 8 (a) Figure 9 (a) Figure 10 As shown in (a), the precursor ZnSnSe is associated with Cs + Ba 2+ Co 2+ Ni 2+ The adsorption rate of ions is slow and the removal rate is low; at 240 min, Cs + Ba 2+ Co 2+ Ni 2+ The removal rates were 8.57%, 2.67%, 1.97%, and 1.38%, respectively. The ZnSnSe-K ion exchanger showed a significant improvement in adsorption rate, reaching Cs within 2 minutes. + The adsorption equilibrium was achieved, with a removal rate of 99.34%. ZnSnSe-K ion exchanger for Ba... 2+ Co 2+ Ni 2+ Kinetic equilibrium was reached at 40, 60, and 40 minutes, respectively, with removal rates of 98.57%, 97.88%, and 97.59%. Figure 7 (b) Figure 8 (b) Figure 9 (b) Figure 10 As shown in (b), ZnSnSe-K for Cs + Ba 2+ Co 2+ Ni 2+ The exchange, in t / q t The curve plotted against time t shows good linearity, conforming to the pseudo-second-order kinetic model, with a correlation coefficient Rt. 2 All values ​​are above 0.9999, indicating that ZnSnSe-K has a positive effect on Cs. + Ba 2+ Co2+ Ni 2+ The rate-determining step of adsorption is chemisorption. Calculations show that Cs... + Ba 2+ Co 2+ Ni 2+ The exchange rate constants k2 are 1.114, 0.210, 0.062, and 0.050 g mg, respectively. -1 min -1 .

[0121] Example 3: CdSnSe-K ion exchanger for single Cs + Co 2+ Ni 2+ Adsorption kinetics of ions

[0122] When x = 0.6, take a sample of CdSnSe-K and 6 ppm of a single Cs + Co 2+ Ni 2+ The aqueous solutions of the ions were mixed and stirred continuously at room temperature (20°C) for 1-240 min, V / m = 1000 mL g -1 pH = 6-7. Turbid solutions with different stirring times were filtered and diluted, and the Cs content was determined by ICP-MS. + Co 2+ Ni 2+ Ion concentration. Adsorption tests using CdSnSe precursors under the same conditions were used as a reference. For example... Figure 11 (a) Figure 12 (a) Figure 13 As shown in (a), the precursor CdSnSe is related to Cs + Co 2+ Ni 2+ The adsorption rate of ions is slow and the removal rate is low; at 240 min, Cs + Co 2+ Ni 2+ The removal rates were 40.64%, 16.29%, and 9.55%, respectively. The adsorption rate of the CdSnSe-K ion exchanger was significantly improved; the CdSnSe-K ion exchanger could reach the Cs removal rate within 2 minutes. + The adsorption equilibrium was reached, and the removal rate reached 99.27%. CdSnSe-K ion exchanger is effective for Co... 2+ Ni 2+ Kinetic equilibrium was reached at 20 and 40 minutes, respectively, with removal rates of 98.32% and 98.73%. Figure 11 (b) Figure 12 (b) Figure 13As shown in (b), CdSnSe-K for Cs + Co 2+ Ni 2+ The exchange, in t / q t The curve plotted against time t shows good linearity, conforming to the pseudo-second-order kinetic model, with a correlation coefficient Rt. 2 All values ​​are above 0.9999, indicating that CdSnSe-K is effective against Cs. + Co 2+ Ni 2+ The rate-determining step of adsorption is chemisorption. Calculations show that Cs... + Co 2+ Ni 2+ The exchange rate constants k2 are 2.474, 0.254, and 0.115 g mg, respectively. -1 min -1 .

[0123] Example 4: ZnSnSe-K (x = 0.6) ion exchanger for single Cs + Ba 2+ Co 2+ Ni 2+ Isothermal adsorption curves of ions

[0124] Take a sample of ZnSnSe-K (x=0.6) and 3-781ppm of single Cs + 3-819ppm of single Co 2+ 2-500ppm of single Co 2+ Or 5-387 ppm of single Ni 2+ The aqueous solution was mixed and stirred continuously at room temperature (20℃) for 4 hours, V / m = 1000 mL g -1 pH = 6-7. The initial solution and the post-reaction filtrate were diluted and their Cs content was determined by ICP-MS. + Ba 2+ Co 2+ Ni 2 + Ion concentration. Experimental results are as follows: Figure 14 (a) Figure 14 (b) Figure 14 (c) Figure 14 As shown in (d), the isothermal adsorption curves were fitted using the Langmuir-Frendlich model for Cs. + Ba 2+ Co 2+ Ni 2+The saturated adsorption capacities of the ions reached 253.61±9.15, 108.94±25.32, 45.76±14.19, and 38.49±2.99 mg g, respectively. -1 .

[0125] Example 5: CdSnSe-K (x = 0.6) ion exchanger for single Cs + Co 2+ Ni 2+ Isothermal adsorption curves of ions

[0126] Take samples of CdSnSe-K and 3-676 ppm of single Cs + 4-701ppm of single Co 2+ Or 3-496ppm Ni 2+ The aqueous solution was mixed and stirred continuously at room temperature (20℃) for 4 hours, V / m = 1000 mL g -1 pH = 6-7. The initial solution and the supernatant after the reaction were taken separately, diluted, and Cs were determined by ICP-MS. + Co 2+ Ni 2+ Ion concentration. Experimental results are as follows: Figure 15 (a) Figure 15 (b) Figure 15 As shown in (c), the isothermal adsorption curves were fitted using the Langmuir-Frendlich model for Cs. + Co 2+ Ni 2+ The saturated adsorption capacities of the ions reached 218.08±80.08, 43.95±16.57, and 42.53±16.501 mgg, respectively. -1 .

[0127] Example 6: ZnSnSe-K (x = 0.3, 1) ion exchanger for single Cs + Isothermal adsorption curves of ions

[0128] Samples ZnSnSe-K (x = 0.3) and ZnSnSe-K (x = 1) were respectively compared with a single Cs + The aqueous solution was mixed and stirred continuously at room temperature (20℃) for 4 hours, V / m = 1000 mL g -1 pH = 6-7. The initial solution and the post-reaction filtrate were diluted and their Cs content was determined by ICP-MS. + Ion concentration. Experimental results are as follows: Figure 16 (a) Figure 16As shown in (b), the isothermal adsorption curves were fitted using the Langmuir-Frendlich model, and the effects of ZnSnSe-K (x = 0.3) and ZnSnSe-K (x = 1) on Cs + The saturated adsorption capacities of the ions reached 244.54±12.05 and 249.01±10.52 mg g, respectively. -1 .

[0129] Example 7: CdSnSe-K (x = 0.3, 1) ion exchanger for single Cs + Isothermal adsorption curves of ions

[0130] Samples CdSnSe-K (x = 0.3) and CdSnSe-K (x = 1) were respectively compared with a single Cs + The aqueous solution was mixed and stirred continuously at room temperature (20℃) for 4 hours, V / m = 1000 mL g -1 pH = 6-7. The initial solution and the post-reaction filtrate were diluted and their Cs content was determined by ICP-MS. + Ion concentration. Experimental results are as follows: Figure 17 (a) Figure 17 As shown in (b), the isothermal adsorption curves were fitted using the Langmuir-Frendlich model. The effects of CdSnSe-K (x = 0.3) and CdSnSe-K (x = 1) on Cs... + The saturated adsorption capacities of the ions reached 193.61±12.25 and 211.63±8.44 mg g, respectively. -1 .

[0131] Example 8: ZnSnSe-K (x = 0.6) ion exchanger and Cs + Ba 2+ Co 2+ Ni 2+ Characterization of ion-saturated adsorption samples

[0132] ZnSnSe-K (x=0.6) ion exchanger was reacted with 8000ppm of single Cs. + 8000ppm of single Ba 2+ 8000ppm of single Co 2+ Or 8000ppm Ni 2+ The aqueous solution was mixed and stirred continuously at room temperature (20℃) for 4 hours, V / m = 1000 mL g -1 The pH value was 6-7. After the reaction, the solid product was filtered out, washed three times with water, and then naturally dried to obtain the saturated adsorbed products ZnSnSe-Cs, ZnSnSe-Ba, ZnSnSe-Co, and ZnSnSe-Ni. Figure 18As shown, the ZnSnSe-K (x=0.6) ion exchanger was subjected to Cs + Ba 2+ Co 2+ Ni 2+ Ion exchange was performed, and the crystal morphology remained intact without surface fragmentation or pulverization, confirming that the exchanger's framework structure was robust enough to withstand ion substitution and shuttle movement within the pores. The elemental distribution shows that K... + Cs + Ba 2+ Co 2+ Ni 2+ The ions were uniformly distributed in the ZnSnSe-K (x=0.6), ZnSnSe-Cs, ZnSnSe-Ba, ZnSnSe-Co and ZnSnSe-Ni samples, respectively.

[0133] Figure 19 (a), (b), (c), and (d) in the figure are Cs + Ba 2+ Co 2+ Ni 2+ Energy-dispersive X-ray spectra of the ion-exchange products ZnSnSe-Cs, ZnSnSe-Ba, ZnSnSe-Co, and ZnSnSe-Ni were obtained. The mass percentage and atomic percentage of each element in these spectra are consistent with the elemental composition of the substituted material in Example 1 and the Cs obtained by fitting the isothermal adsorption curve in Example 4. + Ba 2+ Co 2+ Ni 2+ Saturated adsorption capacity.

[0134] Example 9: CdSnSe-K ion exchanger (x = 0.6) and Cs + Co 2+ Ni 2+ Characterization of ion-saturated adsorption samples

[0135] CdSnSe-K (x=0.6) ion exchanger was reacted with 8000ppm of single Cs... + 8000ppm of single Co 2+ Or 8000ppm Ni 2+ The aqueous solution was mixed and stirred continuously at room temperature (20℃) for 4 hours, V / m = 1000 mL g -1 The pH value was 6-7. After the reaction, the solid product was filtered out, washed three times with water, and then naturally dried to obtain the saturated adsorbed products CdSnSe-Cs, CdSnSe-Co, and CdSnSe-Ni. Figure 20 As shown, the CdSnSe-K (x=0.6) ion exchanger was subjected to Cs +Co 2+ Ni 2+ Ion exchange products CdSnSe-Cs, CdSnSe-Co, and CdSnSe-Ni maintained good crystal morphology, with no surface fragmentation or pulverization, confirming that the exchanger's framework structure is sufficiently robust to withstand ion substitution and shuttle movement within the pores. The elemental distribution shows that K... + Cs + Co 2+ Ni 2+ The ions were uniformly distributed in the CdSnSe-K (x=0.6), CdSnSe-Cs, CdSnSe-Co and CdSnSe-Ni samples, respectively.

[0136] Figure 21 (a), (b), and (c) in the figure are Cs + Co 2+ Ni 2+ Energy-dispersive X-ray spectra of the ion-exchange products CdSnSe-Cs, CdSnSe-Co, and CdSnSe-Ni were obtained. The mass percentage and atomic percentage of each element were consistent with the elemental composition of the substituted material in Example 1 and the Cs elemental composition fitted by the isothermal adsorption curve in Example 5. + Co 2+ Ni 2+ Saturated adsorption capacity.

[0137] Example 10: ZnSnSe-K (x = 0.6) ion exchanger for single Cs at different pH values + Ba 2+ Co 2+ Ni 2+ Ion adsorption performance test

[0138] Samples ZnSnSe-K (x = 0.6) and samples containing a single Cs at pH = 0-14 were taken separately. + Ba 2+ Co 2+ Ni 2+ Aqueous solutions of the ions (each with a concentration of 6 ppm) were mixed and stirred continuously at room temperature (20°C) for 4 hours. V / m = 1000 mL g -1 The initial solution and the filtrate after reaction were diluted and the Cs content was determined by ICP-MS. + Ba 2+ Co 2+ Ni 2+ The concentration of ions. For example... Figure 22 As shown in (a), ZnSnSe-K (x = 0.6) affects Cs in the pH range of 1–12. + The ions exhibit good adsorption activity, with a partition coefficient K.d Cs Higher than 3×10 3 mL g -1 Cs at pH=6 and pH=10 + The removal rate reached 99.3%, with a corresponding allocation coefficient as high as 1.5×10⁻⁶. 5 mL g -1 That's all. (As...) Figure 22 As shown in (b), ZnSnSe-K (x = 0.6) can also effectively remove Ba in the pH range of 3-12. 2+ Distribution coefficient K d Ba Higher than 3×10 3 mL g -1 And at pH=6 and pH=9, Ba 2+ The removal rates reached 98.57% and 98.90% respectively, with a corresponding allocation coefficient of 6.9 × 10⁻⁶. 4 9.0×10 4 mL g -1 .like Figure 22 As shown in (c) and (d), ZnSnSe-K (x=0.6) is effective against Co. 2+ Ni 2+ The adsorption activity of ions is mainly in the pH range of 4-11, within which K d Co K d Ni In 2×10 3 mL g -1 Above, Co 2+ It reaches a peak value of 1.01 × 10⁻⁶ at pH 5. 5 mL g -1 Removal rate R Co It is 99.02%, Ni 2+ It reaches a peak value of 4.05 × 10⁻⁶ at pH = 6. 4 mL g -1 Removal rate R Ni It is 97.59%. At pH=12, Co 2+ Ni 2+ The ions will partially precipitate, and as the alkalinity of the solution continues to increase to pH=13 and pH=14, the exchange resin will dissolve.

[0139] like Figure 23 As shown, the ZnSnSe-K (x = 0.6) ion exchanger reacts with Cs in solutions with pH = 0-12. + After the adsorption reaction at (6 ppm), the XRD pattern did not change significantly, indicating that the ion exchanger has good resistance to acid and alkali.

[0140] Example 11: CdSnSe-K (x=0.6) ion exchanger for single Cs at different pH values + Co 2+ Ni 2+ Ion adsorption performance test

[0141] Samples of CdSnSe-K (x = 0.6) and mixed Cs at pH 0-14 were taken separately. + Co 2+ Ni 2+ Aqueous solutions of the ions (each with a concentration of 6 ppm) were mixed and stirred continuously at room temperature (20°C) for 4 hours. V / m = 1000 mL g -1 The initial solution and the filtrate after reaction were diluted and the Cs content was determined by ICP-MS. + Co 2+ Ni 2+ The concentration of ions. For example... Figure 24 As shown in (a), CdSnSe-K (x = 0.6) affects Cs in the pH range of 2–10. + The ions exhibit excellent adsorption activity, with a partition coefficient K. d Cs Higher than 4×10 4 mL g -1 It reached a peak value of 1.45 × 10⁻⁶ at pH 4 and pH 6. 5 1.36×10 5 mL g -1 The corresponding removal rate R Cs The percentages are 99.32% and 99.27%. For example... Figure 24 As shown in (b) and (c), CdSnSe-K (x=0.6) affects Co 2+ Ni 2+ The adsorption activity of ions is within the pH range of 4-11, and the partition coefficient is 10. 4 mL g -1 The Co concentration reached its peak at pH 11, at 4.43 × 10⁻⁶. 5 mL g -1 Removal rate R Co The purity was 99.77%, and Ni reached its peak value of 7.75 × 10⁻⁶ at pH 6. 4 mL g -1 Removal rate R Ni It is 98.73%. At pH=12, Co 2+ Ni 2+ The ions will partially precipitate, and as the alkalinity of the solution continues to increase to pH=13 and pH=14, the exchange resin will dissolve.

[0142] Example 12: ZnSnSe-K (x = 0.6) ion exchanger in Na + K + Mg 2+ Ca 2+ Cs under coexisting ions + Ba 2 + Co 2+ Ni 2+ Ion exchange performance test

[0143] 20 mg of ZnSnSe-K (x = 0.6) crystals were added to 20 mL of Cs solution containing 6 ppm. + Ba 2+ Co 2+ Ni 2+ Single ions of NaCl, KCl, MgCl2, and CaCl2 (0-100 mmol / L) -1 In the solution, stir for 4 hours, and fix the value V / m = 1000 mL g. -1 The initial solution and the filtrate after the reaction were diluted and the Cs content in the solution was determined by ICP-MS. + Ba 2+ Co 2+ Ni 2+ The concentration of ions. For example... Figure 25 As shown in (a) above, Na + Mg 2+ Ca 2+ For Cs + The adsorption of these three ions was almost unaffected when the concentration of these three ions increased to 100 mmol / L. -1 At that time, Cs + The removal rate can still reach over 90%. K + For Cs + The adsorption effect is relatively large when K + The concentration increased to 100 mmol / L -1 The removal rate decreased slightly, but still remained at 64%, which may be related to K. + and Cs + The hydration radius and structural radius are very similar. For example Figure 25 As shown in (b) of the diagram, Ba 2+ Adsorption ratio Cs + More susceptible to +2 valent Mg 2+ and Ca 2+ The effect of ions, at a concentration of 1 mmol / L for both ions. -1 When, Ba 2+ The removal rates were 55% and 56%. For example... Figure 25 As shown in (c) and (d), low concentrations of Na + K + Mg 2+ Ca 2+ (not higher than 1 mmol L) -1 For Co 2+ and Ni 2+ The adsorption was almost unaffected, with removal rates consistently above 90%. Even when the concentration of coexisting ions increased to 10 mmol / L, the adsorption remained largely unaffected. -1 Na + K + Mg 2+ Ca 2+ For Ni 2+ The impact remains low, and the removal rate can still be maintained above 87%. For Co... 2+ For example, divalent Mg 2+ Ca 2+ At high concentrations (not less than 10 mmol / L) -1 ) has a slightly greater impact on it, but Co 2+ The removal rate can still be maintained at 49%-74%.

[0144] Example 13: CdSnSe-K (x = 0.6) ion exchanger in Na + K + Mg 2+ Ca 2+ Cs under coexisting ions + Co 2 + Ni 2+ Ion exchange performance test

[0145] 20 mg of CdSnSe-K (x = 0.6) crystals were added to 20 mL of a solution containing 6 ppm of Cs. + Co 2+ Ni 2+ Single ions of NaCl, KCl, MgCl2, and CaCl2 (0-100 mmol / L) -1 In the solution, stir for 4 hours, and fix the value V / m = 1000 mL g. -1 The initial solution and the filtrate after the reaction were diluted and the Cs content in the solution was determined by ICP-MS. + Co 2+ Ni 2+ The concentration of ions. For example... Figure 26 As shown in (a) above, Na + K + Mg 2+ Ca 2+ For Cs +The adsorption of these four ions was almost unaffected when the concentration of these four ions increased to 10 mmol / L. -1 At that time, Cs + The removal rate can still reach 85%-95%. Even with high concentrations of Na... + or Mg 2+ Given that Cs exists + The removal rate can still reach over 90%. K + For Cs + The adsorption effect is relatively large when K + The concentration increased to 100 mmol / L -1 The removal rate decreased slightly, but still remained at 64%, which may be related to K. + and Cs + The hydration radius and structural radius are very similar. For example Figure 26 As shown in (b) above, in the range of 0-10 mmol L -1 Na + K + Mg 2+ Ca 2+ When coexisting, Co 2+ The removal rate can reach over 77%. Even when the concentration of the four ions rises to 100 mmol / L... -1 Co 2+ The removal rate can still be maintained at 53%-74%. For example... Figure 26 As shown in (c), low concentration of Na + K + Mg 2+ Ca 2+ (not higher than 1 mmol L) -1 For Ni 2+ The adsorption was almost unaffected, with removal rates consistently above 93%. Even when the concentration of coexisting ions increased to 10 mmol / L, the adsorption remained largely unaffected. -1 Na + K + Mg 2+ Ca 2+ For Ni 2+ The impact remains low, and the removal rate can still be maintained above 74%.

[0146] Example 14: ZnSnSe-K (x = 0.6) ion exchanger in Fe 3+ Al 3+ Eu 3+ UO2 2- Cs under coexisting ions + Ba 2+ Co 2+ Ni 2+ Ion exchange performance test

[0147] 20 mg of ZnSnSe-K (x = 0.6) crystals were added to 20 mL of a solution containing 2 ppm Cs. + Ba 2+ Co 2+ Ni 2+ The single ions FeCl3·6H2O, AlCl3·6H2O, EuCl3·6H2O, UO2(NO3)2·6H2O (Fe 3+ Al 3+ Eu 3+ UO2 2+ In a 2 ppm solution, stir for 4 hours, with a fixed value of V / m = 1000 mL g. -1 The initial solution and the filtrate after the reaction were diluted and the Cs content in the solution was determined by ICP-MS. + Ba 2+ Co 2+ Ni 2+ The concentration of ions. For example... Figure 27 As shown, 2 ppm Fe 3+ Al 3+ Eu 3+ UO2 2+ Coexisting ion pair 2 ppm Cs + Ba 2+ Co 2+ Ni 2+ The adsorption effect of ions is very weak, with a removal rate of 88%-99%. This indicates that the ZnSnSe-K (x=0.6) ion exchanger has a very weak effect on Cs adsorption. + Ba 2+ Co 2+ Ni 2+ Ions exhibit excellent selectivity.

[0148] Example 15: CdSnSe-K (x = 0.6) ion exchanger in Fe 3+ Al 3+ Eu 3+ UO2 2- Cs under coexisting ions + Co 2+ Ni 2+ Ion exchange performance test

[0149] 20 mg of CdSnSe-K (x = 0.6) crystals were added to 20 mL of a solution containing 3 ppm Cs. + Co 2+ Ni 2+The single ions FeCl3·6H2O, AlCl3·6H2O, EuCl3·6H2O, UO2(NO3)2·6H2O (Fe 3+ Al 3+ Eu 3+ UO2 2+ In a 3 ppm solution, stir for 4 hours, with a fixed value of V / m = 1000 mL g. -1 The initial solution and the filtrate after the reaction were diluted and the Cs content in the solution was determined by ICP-MS. + Co 2+ Ni 2+ The concentration of ions. For example... Figure 28 As shown, 3 ppm Fe 3+ Al 3+ Eu 3+ UO2 2+ Coexisting ion pair 3 ppm Cs + The adsorption of ions has a moderate effect, but the effect on 3 ppm Co is limited. 2+ and Ni 2+ The impact is minimal, Cs + Co 2+ Ni 2+ The ion removal rates were 70%-84%, 97%-99%, and 91%-98%, respectively. This indicates that the CdSnSe-K (x=0.6) ion exchanger is effective for the removal of Co. 2+ Ni 2+ Ions exhibit excellent selectivity.

[0150] Example 16: Ion exchange column treatment of mixed Cs + Ba 2+ Co 2+ Ni 2+ Ionic solutions

[0151] like Figure 29 As shown, an exchange column was prepared by packing a ZnSnSe-K (x=0.6) sample with a height of 13 mm and a mass of approximately 2.3 g into a flash chromatography column with an inner diameter of 10 mm. A constant flow pump was used to pump 5.58 × 10⁻⁶ g of ZnSnSe-K sample. 4 Mixing Cs in a fixed bed volume (1 fixed bed volume = 1 mL) + Ba 2+ Co 2+ Ni 2+ An aqueous solution (concentration of 1 ppm for each ion) was introduced into the exchange column and allowed to accelerate at a rate of 2 mL / min. -1 The exchange resin was flowed at a rate of [missing information], and samples were taken from the effluent every 200 fixed bed volumes. After dilution, the Cs content was determined by ICP-MS. + Ba 2+ Co2+ Ni 2+ Calculate the removal rate based on the ion concentration.

[0152] like Figure 30 As shown, the ZnSnSe-K (x = 0.6) packed ion exchange column was used to treat Cs in 55.8 L (equivalent to 55,800 bed volumes) of a pH 6 solution. + Ba 2+ Co 2+ Ni 2+ The ions can be adsorbed efficiently. The entire adsorption process can be divided into two stages. The first stage (denoted as Stage I) ranges from 0 to 18,400 bed volumes, during which the column exhibits adsorption activity for all four ions. Especially during the initial 10,000 bed volumes of adsorption, Cs... + Co 2+ Ni 2+ The removal rates remained above 99.7%, 98.0%, and 98.5%. In tests with the first 5000 bed volumes, Ba... 2+ The removal rate was also higher than 94.6%, and subsequently, Ba... 2+ The removal rate of ZnSnSe-K (x=0.6) decreased and deviated significantly from the removal rates of the other three ions, confirming that ZnSnSe-K (x=0.6) significantly reduced the removal rate of Cs. + Co 2+ and Ni 2+ Its affinity is stronger than Ba 2+ When the volume of the solution being processed reaches 18,400 bed volumes, Ba 2+ The removal rate decreased to 0%, indicating that the exchange column had reached adsorption saturation. At this point, Cs... + Co 2+ and Ni 2+ The removal rate remained at approximately 92%, therefore, with further increases in the effluent volume, Ba... 2+ The removal rate continued to decline into negative values, peaking at -87.53% at a bed volume of 23,000, before gradually recovering to -17.0% ± 1% at a bed volume of 39,200 and remaining there until the end of the test. 2+ A negative removal rate indicates that the adsorbed Ba 2+ Leaching from the adsorbent can be attributed to Ba. 2+ Newly adsorbed Cs + Co 2+ and Ni 2+ For ion substitution, we denote the aforementioned bed volume phase of 18400-55800 as Phase II. Throughout Phase II, Co... 2+ and Ni 2+The adsorption efficiency was much higher, with the removal rate decreasing linearly from 92% (18400 BVs) to 10-12% (55800 BV). No Co was detected in Stage II. 2+ and Ni 2+ The leaching indicates that the ZnSnSe-K (x=0.6) framework has a high binding strength with the adsorbed ions. For Cs... + In terms of the 38,600 bed volume, Cs + Removal rate and Co 2+ Ni 2+ The trend of change is similar to that of Co, but after that, its decline was greater than that of Co. 2+ Ni 2+ Larger, reaching 0% at around 44,000 bed volume. After adsorption saturation, Cs + The removal rate further decreased, reaching -47.5% at a bed volume of 55,800, indicating that Cs... + The leaching occurs in the effluent. Based on the elution order, the affinity order of the relatively fixed ions in the exchange column can be determined as follows: Co 2+ ≈Ni 2+ >Cs + >Ba 2+ .

[0153] Example 17 Microporous membrane treatment of mixed Cs + Ba 2+ Co 2+ Ni 2+ Ionic solutions

[0154] 500 mg of ZnSnSe-K (x = 0.6) was processed in a ball mill to obtain micron-sized crystal particles. Then, 95% by mass of the ball-milled ZnSnSe-K and 5% by mass of polyvinylidene fluoride (PVDF) were mixed in NMP (N-methylpyrrolidone), stirred thoroughly, and then coated onto a PTFE membrane. The mixture was then evenly coated with a doctor blade and allowed to air dry at room temperature to obtain a ZnSnSe-K / PTFE composite microporous filter membrane. Figure 31 As shown, the obtained ZnSnSe-K / PTFE microporous filter membrane is a circular filter membrane with a diameter of 5cm. No obvious damage was found after being subjected to 30-50 bends. When using it, the membrane is laid flat on the sand core funnel and fixed for vacuum filtration.

[0155] like Figure 32 As shown, the thicknesses of the ZnSnSe-K layer and the PTFE substrate in the ZnSnSe-K / PTFE microporous filter membrane are approximately 70 and 100 μm, respectively. SEM images of the membrane surface reveal that the ball-milled ZnSnSe-K particles have a diameter of less than 3 μm, resulting in an effective increase in specific surface area compared to the original single-crystal material, thereby promoting the adsorption rate.

[0156] Under reduced pressure filtration conditions, 2500 mL of the mixed Cs + Ba 2+ Co 2+ and Ni 2+ (The concentration of each ion is 1 ppm) The solution is dispensed at 25 mL / min. -1 The film flows through the membrane at a constant rate. Residual Cs are accurately measured by ICP-MS. + Ba 2+ Co 2+ and Ni 2+ The concentration was recorded, and the removal rate was recorded as a function of filtrate volume. For example... Figure 33 As shown, the ZnSnSe-K / PTFE membrane exhibits a high degree of sensitivity to Cs throughout the testing process. + It exhibits extremely high removal efficiency. In the initial 250 mL, it can remove over 99.9% of Cs. + until the filtrate volume increases to 2000 mL, Cs + The removal rate remains above 97%. For Ba... 2+ Generally speaking, its removal rate is above 99% in the range of 0 to 400 mL, while after 850 mL, Ba... 2+ The removal rate gradually decreased, reaching adsorption saturation at 2500 mL, with a removal rate of 0%. The ZnSnSe-K / PTFE microporous membrane was effective for removing Co. 2+ and Ni 2+ The adsorption properties of Ba 2+ Similar. The difference is that there is an induction period before the solution volume reaches 100 mL, during which Co 2+ and Ni 2+ The removal rate increased from 85-90% to a peak of over 99.5% and remained thereafter up to 500 mL. After that, the removal rates of both decreased continuously until they finally reached 6.8% and 8.3% at 2500 mL.

[0157] From the above examples, we can see that MSnSe-K (M = Zn or Cd) ion exchangers have advantages such as simple preparation, high yield, good acid resistance, and strong radiation tolerance, and can effectively treat Cs in aqueous solutions. + Ba 2+ Co 2+ and Ni 2+ Ions undergo rapid and highly selective adsorption.

[0158] The above-described embodiments are not intended to limit the present invention in any way. Any modifications or alterations made by those skilled in the art without departing from the scope of the present invention are equivalent to equivalent implementations and fall within the scope of the technical solution.

[0159] Matters not covered in this invention are common knowledge.

Claims

1. A method for adsorbing Cs + Ba 2+ Co 2+ Ni 2+ Microporous zinc / cadmium-tin selenide ion exchangers, characterized by: The molecular formula of this ion exchanger is: K 4-x (CH3NH3) 0.75x (NH4) 0.25x M2Sn3Se 10 ·(4- x H₂O, denoted as MSnSe⁻K; where M = Zn or Cd, x = 0.3-1; All M in the aforementioned exchanger 2+ Sn 4+ All four {(M / Sn)Se4} tetrahedral building units are coordinated with four Se atoms in a tetrahedral coordination mode. These four {(M / Sn)Se4} tetrahedral building units further condense and aggregate through shared vertex connections to form {(M / Sn)4Se4} with a zincblende configuration. 10 Supertetrahedral clusters, which are assembled with bridging metal atoms in an alternating 4,4-connected manner to form [M2Sn3Se] with a microporous structure. 10 ] n 4n- Framework, pore size 0.4~0.6 nm, hydrated K + As counteracting cations, they fill the pores of the framework and together construct the MSnSe-K lattice structure; The preparation method of the zinc / cadmium-tin selenide ion exchanger includes the following steps: (1) Substance A and N,N'-dimethylurea are stirred to form a eutectic solvent. Then, substance B, tin powder, selenium powder, and 98% (w / w) hydrazine hydrate are added to the eutectic solvent. The mixture is stirred for 1-20 min to ensure homogeneity. The mixture is then transferred to a reaction vessel and reacted at 120-200℃ for 1-5 days. After natural cooling to room temperature, the initial product is washed and then naturally dried to obtain the crystalline precursor (CH3NH3)3NH4M2Sn3Se. 10 M = Zn or Cd; Substance A is trimethylamine hydrochloride or diethylamine hydrochloride, and substance B is zinc powder or cadmium chloride hemipentahydrate; wherein the molar ratios are: substance A: N,N'-dimethylurea = 1:1-3; substance B: tin powder: selenium powder = 1:1-3:3-10; substance B: substance A = 1:2-10; substance A: hydrazine hydrate = 1:0.5-2; (2) The obtained precursor was soaked in KCl solution and stirred for 4-24 h. After filtration, washing and drying, zinc / cadmium-tin selenide ion exchanger was obtained.

2. The microporous zinc / cadmium-tin selenide ion exchanger as described in claim 1, characterized in that, In the preparation method, the concentration of KCl solution in step (2) is 0.1-3 M.

3. The application of the microporous zinc / cadmium-tin selenide ion exchanger as described in claim 1, characterized in that it is used for... Adsorption of Cs + Ba 2+ Co 2+ and Ni 2+ One or more of the following ions.

4. The application as described in claim 3, characterized in that it is specifically one of the following three methods: Method 1, batch adsorption, includes the following steps: The ion exchanger is added to the solution to be treated and stirred for 1 min-24 h to complete the adsorption of the target ions; The solution to be treated contains Cs + Ba 2+ Co 2+ and Ni 2+ One or more of the ions; In the solution to be treated, Cs + Ba 2+ Co 2+ and Ni 2+ The concentration range of the ions is 0.5-8000 ppm; In the adsorption method described above, the ratio of solution volume to exchanger mass is 300-3000 mL g. -1 ; The ion exchanger MSnSe-K adsorbs Cs + Ba 2+ Co 2+ and Ni 2+ The temperature of the ions is 5-60℃; Alternatively, method two, ion exchange column adsorption, includes the following steps: The ion exchanger is filled into a glass chromatography column as a stationary phase, and the solution to be treated flows through the chromatography column to complete the adsorption of the target ion. Among them, each 1 cm 3 The flow rate of the stationary phase treatment solution is 0.1-5 mL / min. -1 ; The solution to be treated contains Cs + Ba 2+ Co 2+ and Ni 2+ One or more ions, with the concentration range of each ion being 0.5-3000 ppm; Alternatively, method three, microporous membrane adsorption, includes the following steps: The ion exchanger was ball-milled to prepare a powder with a particle size of 1-10 μm, and then mixed with 10-100 mg / mL of water. -1 The N-methylpyrrolidone solution of polyvinylidene fluoride was mixed and stirred for 1-60 min. The mixture was then taken out and uniformly coated onto the surface of an aqueous PTFE microporous filter membrane substrate. The substrate was then allowed to air dry naturally for 2-30 h to prepare the MSnSe-K / PTFE microporous filter membrane. The mass ratio of ball-milled ion exchanger to polyvinylidene fluoride is 5-40:

1. The thickness of the aqueous PTFE microporous filter membrane substrate is 30-200 µm; In the MSnSe-K / PTFE microporous filter membrane, the thickness of the MSnSe-K ion exchanger layer is 10-200 µm; Under reduced pressure filtration conditions, the solution to be treated is passed through a microporous filter membrane to complete the adsorption of target ions; per 1 cm 2 The flow rate of the MSnSe-K / PTFE microporous membrane treatment solution was 0.5–2.5 mL / min. -1 ; The solution to be treated contains Cs + Ba 2+ Co 2+ and Ni 2+ One or more ions, with the concentration range of each ion being 0.5-3000 ppm.

5. The application as described in claim 4, characterized in that, Methods 1, 2, and 3 are described below. The solution to be treated also contains Na. + K + Mg 2+ Ca 2+ One or more of the ions, with a concentration range of 0-1000 mmol / L -1 And not equal to 0; The solution to be treated also contains Fe. 3+ Al 3+ Eu 3+ UO2 2+ One or more of the ions, with a concentration range of 0-100 ppm and not equal to 0.

6. The application as described in claim 4, characterized in that, The solution to be treated is drinking water, tap water, lake water, or industrial wastewater.

7. The application as described in claim 4, characterized in that, The desorption method of the ion exchanger: In method one or method two, MSnSe-K exchanger is used to extract Cs. + Ba 2+ Co 2+ Ni 2+ After removing one or more of the ions, immerse the sample in a 0.5-3 M KCl solution for 0.5-12 h to complete the elution. Then remove the sample, wash and dry it for reuse. In method three, Cs is extracted using an MSnSe-K / PTFE microporous membrane. + Ba 2+ Co 2+ Ni 2+ After removing one or more of the ions, under reduced pressure filtration, a 0.5-3 M KCl solution is passed through the filter membrane for 0.5-12 h to complete the elution. The membrane is then washed with deionized water, removed, dried, and reused.

Citation Information

Patent Citations

  • Preparation method and application of novel caesium-removing silver-tin selenide microporous material

    CN101985106B