A main chain spirocyclic ammonium polybenzimidazole and its anion exchange membrane, preparation method and application of ionomer solution
By using polybenzimidazole containing an aliphatic cyclohexane structure in the polymer anion exchange membrane for main chain spirocyclic ammonization reaction, the problem of insufficient stability of the polymer anion exchange membrane is solved, and its chemical and antioxidant properties are significantly improved. Stability promotes the application process in alkaline fuel cells and other fields.
Patent Information
- Application Number
- CN202210117997.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-02-08
AI Technical Summary
Polymer anion exchange membranes and their ionomers have poor chemical stability and antioxidant stability, which limits their commercial application in alkaline fuel cells, water electrolysis, flow batteries and other fields.
Polybenzimidazole containing an aliphatic cyclohexane structure is used to perform a main chain spirocyclic ammonization reaction to prepare anion exchange membranes and ionomers with higher chemical stability and improved solubility, which are further processed through condensation polymerization and cross-linking reactions. Improve its performance.
The chemical stability of the polymer anion exchange membrane is improved, and the antioxidant stability reaches 3.75 times, which extends the service life of the membrane and significantly improves its application potential in the fields of fuel cells, water electrolysis, and flow batteries.
Smart Images

Figure CN116606438B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer ion exchange membranes and ionomers, and particularly relates to a main chain spirocyclic ammonium polybenzimidazole and a preparation method and application of an anion exchange membrane and an ionomer solution thereof. Background Art
[0002] Due to the global energy crisis, it is urgent to develop efficient and clean hydrogen energy technology. Alkaline fuel cells, water electrolysis, flow batteries and other related electrochemical devices are low-cost green and clean energy with broad application prospects. Among them, polymer anion exchange membranes and ionomers have an important influence on the performance of batteries and devices. At present, the chemical stability, especially the anti-oxidation stability, of polymer anion exchange membranes and ionomers is poor, which seriously limits their commercial applications in the fields of alkaline fuel cells, water electrolysis and flow batteries. Therefore, it is extremely important to develop polymer anion exchange membranes and ionomers with high durability, especially anti-oxidation stability.
[0003] As an excellent special engineering plastic, polybenzimidazole has excellent mechanical stability, heat resistance and alkali resistance. At present, there have been some reports on the application of polybenzimidazole in alkaline anion exchange membranes in recent years. Patents [Zhu Xiuling et al., patent publication numbers: CN110527087A and CN110527088A] disclose a polybenzimidazole anion exchange membrane with monocyclic ammonium ions and dicyclic ammonium ions and a preparation method. Patent [Zhu Xiuling et al., patent number: 202111335775.0] discloses a long side chain ammonium polybenzimidazole anion exchange membrane with high chemical stability and oxidation resistance. Patent [Cui Mengbing et al., patent publication number: CN 108373545A] discloses a cycloolefin-polybenzimidazole cross-linked composite membrane and its application in fuel cells. However, in order to meet the application requirements of fuel cells, water electrolysis and energy storage battery ion membranes, the chemical stability of polybenzimidazole anion exchange membranes is in urgent need of further improvement. The literature [EnergyEnviron.Sci., 2021, 14, 3393] shows that the benzene ring structure in the polymer anion exchange membrane or ionomer is easily electrochemically oxidized and degraded, thereby reducing the life of the device. The large steric hindrance of the benzene ring structure will also affect the solubility of the polymer. Therefore, reducing the benzene ring structure in the polymer is beneficial to improving durability and solubility. Summary of the invention
[0004] According to the problems existing in polymer anion exchange membranes and ionomers thereof, the present invention discloses for the first time a main chain spiroaminated polymer synthesized based on polybenzimidazole containing a fatty cyclohexane structure, and further prepares anion exchange membranes and ionomers. The main chain of the polybenzimidazole of the present invention uses a cyclohexane structure to replace the traditional benzene ring structure, which overcomes the electrochemical oxidation problem of the benzene ring structure. The chemical stability of the polymer anion exchange membrane and ionomer prepared by the main chain spiroaminated reaction is 3.75 times higher than that of the non-main chain spiroaminated polybenzimidazole anion membrane, and the solubility is significantly improved. The double bond of the norbornene structure in the polymer facilitates the subsequent cross-linking reaction, further improving the chemical stability. So far, the main chain spiroaminated polybenzimidazole containing a fatty cyclohexane structure, the anion membrane and the ionomer thereof have not been reported in the literature.
[0005] The present invention is achieved by adopting the following technical solutions:
[0006] A main chain spirocyclic ammonium polybenzimidazole, which is obtained by polycondensation of aromatic tetraamine monomers and dicarboxylic acid monomers, and contains structural units represented by general formula (1), (1-1), (2) or (2-2):
[0007]
[0008] Wherein, n is a positive integer greater than or equal to 1, and k and l are positive integers greater than or equal to 0.
[0009] Z is Cl - Br - ,I - 、HCO3 - or OH - ;
[0010] A is a methylene group -CH2-, an ether bond -O- or a carbonyl group -CO-, and each A in the structural unit may be the same or different;
[0011] X is one of the following chemical structures:
[0012]
[0013] Y is any one of the following chemical structures:
[0014]
[0015] Wherein 2≤q≤12, preferably 2≤q≤10;
[0016] Preferably Y is structure (a), (d), (e), (h) or (i);
[0017] The preparation method of the main chain spirocyclic ammonium polybenzimidazole comprises the following steps:
[0018] Step 1: Synthesis of polybenzimidazole
[0019] Polybenzimidazole is synthesized by solution polycondensation reaction of aromatic tetraamine monomer (II) and dicarboxylic acid monomer (III), as follows:
[0020] Add polyphosphoric acid to a stirred reactor, and under the protection of N2, add aromatic tetraamine monomer (II) or (II-1) and dicarboxylic acid monomer (III) in an equal molar ratio to the aromatic tetraamine monomer (II) or (II-1), heat and stir to dissolve so that the total concentration of the monomers is 1-20wt%; heat to 90-140°C and stir to react for 0.5-10h, then heat to 140-160°C and stir to react for 0.5-10h, then heat to 160-210°C and react for 3-30h; terminate the polymerization reaction when the reaction liquid becomes very viscous and climbs the pole; pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight; filter, wash the polymer with deionized water until it is neutral; dry to obtain a light brown polybenzimidazole.
[0021] The structure of the aromatic tetraamine monomer (II) or (II-1) is as follows:
[0022]
[0023] Wherein, A is a methylene group -CH2-, an ether bond -O- or a carbonyl group -CO-, and each A in the structural unit may be the same or different;
[0024] The polybenzimidazole (1') is obtained by polymerizing the aromatic tetraamine monomer (II) and the dicarboxylic acid monomer (III);
[0025] The polybenzimidazole (1-1') is obtained by polymerizing the aromatic tetraamine monomer (II-1) and the dicarboxylic acid monomer (III);
[0026] The dicarboxylic acid monomer (III) includes HOOC-X-COOH, HOOC-Y-COOH and norbornene dicarboxylic acid, wherein HOOC-Y-COOH and norbornene dicarboxylic acid may be added or not, and HOOC-X-COOH is 1,4-cyclohexane dicarboxylic acid or 1,3-cyclohexane dicarboxylic acid, that is, X is an alicyclic structure as shown below:
[0027]
[0028] In HOOC-Y-COOH, Y has any of the following structures:
[0029]
[0030] Wherein 2≤q≤12, preferably 2≤q≤10;
[0031] Preferably Y is (a), (d), (e), (h) or (i);
[0032] When the dicarboxylic acid monomer (III) is HOOC-X-COOH, step 1 obtains a polybenzimidazole homopolymer containing a cyclohexane structure;
[0033] When the dicarboxylic acid monomer (III) is HOOC-X-COOH and HOOC-Y-COOH, the step 1 obtains a polybenzimidazole copolymer containing a cyclohexane structure; and the molar ratio of HOOC-X-COOH to HOOC-Y-COOH is any value greater than zero.
[0034] When the dicarboxylic acid monomer (III) is HOOC-X-COOH, HOOC-Y-COOH and norbornene dicarboxylic acid, the polybenzimidazole containing a cyclohexane structure obtained in step 1 has a double bond functional group, which can be subsequently subjected to a cross-linking reaction; wherein the molar content of norbornene dicarboxylic acid in the dicarboxylic acid monomer (III) is less than 30%.
[0035] Step 2: Synthesis of main chain spiroammonium polybenzimidazole
[0036] (2.1) Synthesis of main chain spirocyclic ammonium-modified polybenzimidazole (1) or (1-1):
[0037] The polybenzimidazole (1') is heated and dissolved in solvent A to obtain a 0.5-10 wt% solution, and reagent IV and catalyst A are slowly added and stirred evenly, and the mixture is reacted at 30-150° C. for 8-100 hours. After the reaction is completed, a precipitant A is poured in to precipitate, and the mixture is filtered. The filter cake is washed with deionized water until it is neutral, and the filter cake is dried to obtain the main chain spirocyclic ammonium polybenzimidazole (1).
[0038] Substituting polybenzimidazole (1-1') for (1'), the main chain spirocyclic ammonium polybenzimidazole (1-1) is obtained by the same reaction;
[0039] The reagent IV is 1,5-dibromopentane, and the molar ratio of 1,5-dibromopentane to polybenzimidazole is (0.5-10):1, and the molar ratio of catalyst A to polybenzimidazole is (0.5-10):1.
[0040] (2.2) Synthesis of main chain spirocyclic ammonium-modified polybenzimidazole (2) or (2-2):
[0041] Add piperidine to dibromoalkane Br-(CH2) m -Br is prepared into a 0.5-10wt% solution in solvent B, heated to 30-90°C and stirred for reaction for 6-72h; after the reaction is completed, filtered and dried to obtain a bromide salt M';
[0042] The polybenzimidazole (1') is heated and dissolved in a solvent A to obtain a 0.5-10 wt% solution, and a bromide salt M' is added and reacted at 30-150° C. for 8-100 hours. After the reaction is completed, a precipitant A is poured in, filtered, and the filter cake is washed with deionized water until it is neutral. The product is dried to obtain a main chain spiroammonium polybenzimidazole (2); wherein 2≤m≤6 is an integer.
[0043] Substituting polybenzimidazole (1-1') for (1'), the main chain spirocyclic ammonium polybenzimidazole (2-2) was obtained by the same reaction;
[0044] The piperidine and dibromoalkane Br-(CH2) m The molar ratio of -Br is 0.05 to 1:1; the molar ratio of polybenzimidazole to bromide salt M' is 0.1 to 1.2:1.
[0045] The solvent A is one or a mixture of two or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dichloromethane, tetrahydrofuran, formic acid, and methanesulfonic acid;
[0046] The solvent B is one or a mixture of two or more of methanol, ethanol, N,N-dimethylformamide, tetrahydrofuran, acetonitrile, ethyl acetate, acetone, dimethyl sulfoxide, N,N-dimethylacetamide, and N-methylpyrrolidone.
[0047] The solvent C is one or a mixture of two or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, methanol, ethanol, isopropanol, formic acid, acetic acid, and methanesulfonic acid.
[0048] The precipitant A is one or a mixture of two or more of methyl tert-butyl ether, ethyl ether, methanol, ethanol, ethyl acetate, dichloromethane, tetrahydrofuran, acetone, and water;
[0049] The catalyst A is one or a mixture of two or more of anhydrous sodium carbonate, anhydrous potassium carbonate, anhydrous sodium hydride, anhydrous sodium hydroxide, anhydrous potassium hydroxide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diisopropylethylamine, N,N-dimethylpropylamine, and N,N-dipropylethylamine.
[0050] The main chain spirocyclic ammonium polybenzimidazole is used to prepare anion exchange membrane, and the specific steps are as follows:
[0051] The dried main chain spirocyclic ammonium polybenzimidazole (1), (1-1), (2) or (2-2) is added to solvent C, heated to 30-150° C., stirred and dissolved to prepare a 1-20 wt % solution, filtered, degassed, poured onto a clean plate, and dried to obtain Br –The membrane is immersed in 1M or 2M NaOH solution for 24-48 hours, after ion exchange, it is washed with deionized water until neutral, and dried to obtain OH - Type polymer anion exchange membrane.
[0052] The main chain spirocyclic ammonium polybenzimidazole is used to prepare an ionomer solution, and the specific steps are as follows:
[0053] The dried main chain spirocyclic ammonium polybenzimidazole (1), (1-1), (2) or (2-2) is heated to 30-150° C. in solvent C and stirred to dissolve to prepare a 1-10 wt % solution, which is filtered and degassed to obtain a transparent ionomer solution.
[0054] The intrinsic viscosity of the main chain spirocyclic ammonium polybenzimidazole is 1.5-4.5 dL / g (the solvent is concentrated sulfuric acid), or the viscosity average molecular weight of the polybenzimidazole is 30000-500000 g / mol, and the degree of polymerization n is 20-1200;
[0055] The anion exchange membrane is used in the fields of fuel cells, water electrolysis, carbon dioxide conversion, liquid flow batteries and other electrochemical devices.
[0056] The ionomer solution is used in fuel cells, water electrolysis, flow batteries, carbon dioxide conversion and other polyelectrolyte related fields.
[0057] In the main chain spirocyclic ammonium polybenzimidazole structure (1), (1-1), (2) or (2-2), when l≠0, the double bond in the norbornene structure can be used for cross-linking reaction to obtain a cross-linked main chain spirocyclic ammonium polybenzimidazole and its anion membrane and ionomer.
[0058] Compared with the prior art, the present invention has the following advantages:
[0059] At present, the chemical stability of polymer anion exchange membranes and their ionomers is poor, especially the poor anti-oxidation stability, which is one of the bottleneck problems restricting the promotion and application of technologies such as alkaline fuel cells, alkaline water electrolysis or flow batteries. It is urgent to develop polymer ion membranes with high durability, especially outstanding anti-oxidation properties. In polymer proton exchange membrane fuel cells, it is generally adopted to immerse the proton membrane in Fenton's reagent and observe the time when the membrane begins to rupture to evaluate the oxidation stability of the proton exchange membrane. At present, the evaluation method of proton exchange membrane is generally adopted to evaluate the anti-oxidation property of polymer anion exchange membranes. It should be noted that in order to ensure the strong oxidizing property of Fenton's reagent, the test oxidizability method disclosed in the present invention requires the replacement of freshly prepared Fenton's reagent every 12 hours during the test process. Using this test method, the present invention discloses a spirocyclic ammonium polybenzimidazole anion exchange membrane, and the time for the membrane to start to break is 96 hours; the patent [Zhu Xiuling et al., patent number: 202111335775.0] discloses a long side chain ammonium polybenzimidazole alkaline ion exchange membrane. Under the same test conditions, the time for the ion membrane to start to break is 24 hours (such as Figure 3 The spirocyclic ammonium polybenzimidazole anion exchange membrane disclosed in the present invention has an anti-oxidation time increased by 375% (3.75 times) compared with the long side chain ammonium polybenzimidazole anion exchange membrane in the prior art. This may be due to the higher chemical stability of cyclic ammonium ions than linear ammonium ions. Therefore, the technology of the present invention has the beneficial effect of outstanding durability and will strongly promote the application process of alkaline fuel cells, alkaline water electrolysis or liquid flow batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 The main chain of Example 1 is spirocyclic ammonium PBI 1 H-NMR spectrum;
[0061] Figure 2 The OH of the main chain spirocyclic ammonium PBI anion exchange membrane of Example 1 - Conductivity versus temperature curve;
[0062] Figure 3 The oxidative stability of the anion exchange membranes of the main chain spirocyclic ammonium-modified PBI and the long side chain ammonium-modified PBI in Example 1. DETAILED DESCRIPTION
[0063] The following examples further illustrate the preparation method and application of the main chain spirocyclic ammonium polybenzimidazole anion exchange membrane and its ionomer solution in detail, but are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the methods involved are all conventional methods.
[0064] The test method involved in the embodiment:
[0065] IEC test: Take three portions of main chain spirocyclic ammonium polybenzimidazole (about 0.1 g), soak them in 100 mL 1 mol / L NaCl for 24 hours, and then soak them in 500 mL deionized water for 24 hours to wash away the residual NaCl on the surface. Dry them in a vacuum oven at 75°C and weigh and record the mass, then soak them in 25 mL 0.2M NaNO3 solution for 24 hours. Finally, add the indicator potassium chromate solution to the solution and titrate it with 0.1M AgNO3 solution. When a brick-red precipitate appears and does not change color within 30 seconds, the titration is complete. Record the volume of AgNO3 solution consumed. The product of the concentration and volume of the AgNO3 solution divided by the mass of the dried film is the IEC.
[0066] Evaluation of alkali resistance stability: The membrane samples were immersed in 2M NaOH aqueous solution at 80°C. The samples were taken out at regular intervals and washed with deionized water several times until neutral. The anionic conductivity of the membrane was then measured. The stability of the membrane in alkaline solution was evaluated by comparing the changes in anionic conductivity, and the retention rate of ionic conductivity was calculated.
[0067] Oxidative stability evaluation: The ion membrane is immersed in freshly prepared Fenton reagent and evaluated by testing the retention rate of the ion membrane mass before and after immersion. Accurately weigh the mass of the dry membrane and record it as Weight intinal The membrane was immersed in 80℃, 4ppm FeSO4+3%H2O2Fenton reagent, and the membrane sample was taken out after a certain period of time, and the residual reagent on the surface was rinsed with deionized water and dried. The mass of the dry membrane at this time was weighed and recorded as Weight test It should be noted that during the test, the Fenton reagent needs to be replaced every 12 hours to maintain its strong oxidizing property. The oxidative stability of the ion membrane is evaluated by the mass retention rate of formula 1:
[0068]
[0069] Fuel cell test: The test was performed using the 850e fuel cell test system produced by Scribner Associates Inc. The anion exchange membrane prepared by the present invention was used as the battery diaphragm, and the ion liquid was a homemade ionomer solution. The test was performed at 60°C and 80°C, and the test mode was a constant current mode.
[0070] Water electrolysis test: The test was conducted by LANHE CT3001D battery test station of Wuhan Lanhe Company using constant voltage and current measurement. The anion exchange membrane prepared by the present invention was used as a diaphragm, and the ionic liquid was a homemade ionomer solution.
[0071] The equipment involved in the embodiment:
[0072] Conductivity test: The electrochemical workstation used was produced by Shanghai Chenhua Instrument Co., Ltd., model CHI660C.
[0073] Nuclear magnetic resonance test: The instrument used was produced by Bruker Corporation of the United States, model BrukerAVANCEⅢ500, with DMSO-d6 as solvent and tetramethylsilane as internal standard.
[0074] Table 1 Chemical structures of polybenzimidazoles with spirocyclic ammonium backbone in the examples
[0075]
[0076] Example 1
[0077] Add 85% polyphosphoric acid to a stirred reactor, pass N2 protection, add 3,3'-diaminobenzidine, (III) 1,4-cyclohexanedicarboxylic acid and isophthalic acid in equal molar ratios to 3,3'-diaminobenzidine, heat and stir to dissolve so that the total concentration of the monomer is 15wt%. Heat to 130℃ for reaction for 5h, then heat to 160℃ for reaction for 5h, and then heat to 200℃ for reaction for 6h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain light brown polybenzimidazole. Among them, the molar ratio of 1,4-cyclohexanedicarboxylic acid to isophthalic acid is 6:4.
[0078] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain an 8wt% solution, 1,5-dibromopentane and anhydrous sodium hydride were slowly added and stirred evenly, and the mixture was reacted at 100°C for 15h. After the reaction was completed, the mixture was poured into methanol for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and the filter cake was dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 5:1; the molar ratio of anhydrous sodium hydride to polybenzimidazole was 5:1.
[0079] The prepared dry main chain spirocyclic ammonium polybenzimidazole (1-1) was stirred and dissolved in dimethyl sulfoxide at 100° C. to prepare a 5 wt % solution, which was filtered and degassed to obtain a transparent ionomer solution.
[0080] The prepared dried main chain spirocyclic ammonium polybenzimidazole (1-1) was added to dimethyl sulfoxide and heated to 70°C and stirred to dissolve to prepare an 8 wt% solution. The solution was filtered and degassed. The solution was poured onto a clean plate and dried in an oven to obtain a light yellow transparent Br – The membrane was immersed in 2M NaOH solution for 24 h for ion exchange, washed with deionized water until neutral, and dried to obtain OH -Type main chain spirocyclic ammonium polymer anion exchange membrane.
[0081] analyze:
[0082] Figure 1 The main chain spirocyclic ammonium PBI anion exchange membrane in this embodiment was subjected to nuclear magnetic resonance hydrogen spectrum ( 1 H-NMR) characterization results. First, the chemical shift at 7.65-9.17ppm corresponds to the characteristic peak of the proton on the benzene ring, and the characteristic peak of the alkane in the cyclohexane structure appears at 2.26ppm, 1.85ppm and 1.96ppm. At the same time, the characteristic peak of the proton connected to the N atom on the imidazole structural unit at 13.3ppm disappeared, and the characteristic peak of the methylene proton connected to the N atom appeared at 4.05ppm. The other two characteristic peaks on the ring appeared at 2.01ppm and 1.48ppm, respectively, indicating that the main chain spirocyclic amination reaction of the PBI polymer was successfully carried out.
[0083] Figure 2 The OH-conductivity of the PBI anion exchange membrane with spirocyclic ammonium in the main chain in this embodiment varies with temperature. Hydroxyl ion conductivity is an important indicator for evaluating anion exchange membranes. - The curve of conductivity changing with temperature is shown in the figure. As the temperature increases from 20℃ to 80℃, the conductivity increases from 21.38mScm -1 Increased to 59.83mScm -1 , indicating that the main chain spirocyclic ammonium PBI anion exchange membrane has a high anion conductivity and can meet the requirements of fuel cells.
[0084] Figure 3 During the operation of the fuel cell, due to the incomplete oxygen reduction reaction on the cathode side, free radicals such as OH· and HOO· may be generated. These free radicals will attack and accelerate the degradation of the ion membrane AEMs. The oxidation stability test of the membrane is evaluated by testing the change in mass before and after the membrane is immersed in 80℃ Fenton reagent (4ppm FeSO4+3% H2O2) for a period of time. Figure 3As shown, under the same test conditions, the long side chain ammonium PBI anion membrane disclosed in the patent [Zhu Xiuling et al., patent number: 202111335775.0] began to break after being immersed in Fenton reagent for 24 hours, and its mass retention rate was 90.3%, and the mass loss was close to 10%, while the main chain spirocyclic ammonium PBI anion membrane disclosed in the present invention began to break after being immersed in Fenton reagent for 96 hours, and its mass retention rate was 93.6%, and the mass loss after immersion for 24 hours did not exceed 2%. This result is also better than the results of other polymer anion exchange membranes reported in the literature, indicating that the main chain spirocyclic ammonium PBI anion exchange membrane disclosed in the present invention has ultra-high oxidation resistance and stability, and the technology of the present invention plays an extremely important role in promoting the commercial application of alkaline hydrogen and oxygen fuel cells, water electrolysis, flow batteries, and carbon dioxide conversion.
[0085] Example 2
[0086] Add 85% polyphosphoric acid to a stirred reactor, and under N2 protection, add 3,3'-diaminobenzidine and (III)1,4-cyclohexanedicarboxylic acid in equal molar ratios, heat and stir to dissolve the monomers to a total concentration of 10wt%. Heat to 130℃ for 2h, then heat to 150℃ for 5h, and then heat to 170℃ for 20h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain a polybenzimidazole homopolymer containing a cyclohexane structure.
[0087] Polybenzimidazole was heated and dissolved in N-methylpyrrolidone to obtain a 5wt% solution, 1,5-dibromopentane and anhydrous potassium carbonate were slowly added and stirred evenly, and the mixture was reacted at 30°C for 60h. After the reaction was completed, the mixture was poured into methyl tert-butyl ether for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and the filter cake was dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 1:1; the molar ratio of anhydrous potassium carbonate to polybenzimidazole was 1:1.
[0088] The prepared dry main chain spirocyclic ammonium polybenzimidazole (1-1) was added to N,N-dimethylformamide and heated to 100°C and stirred to dissolve to prepare a 10 wt% solution. After filtering and degassing, the solution was poured onto a clean plate and dried in an oven to obtain a light yellow transparent Br – The membrane was immersed in 2M NaOH solution for 24 h for ion exchange, washed with deionized water until neutral, and dried to obtain OH - Type main chain spirocyclic ammonium polymer anion exchange membrane.
[0089] Example 3
[0090] Add 85% polyphosphoric acid to a stirred reactor, pass N2 protection, add 3,3'-diaminobenzidine, and (III) 1,4-cyclohexanedicarboxylic acid and isophthalic acid in equal molar ratios, heat and stir to dissolve the monomers to a total concentration of 15wt%. Heat to 120℃ for 5h, then heat to 150℃ for 2h, and then heat to 180℃ for 28h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain a light brown polybenzimidazole. Among them, the molar ratio of 1,4-cyclohexanedicarboxylic acid to isophthalic acid is 1:1.
[0091] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain a 10wt% solution, 1,5-dibromopentane and anhydrous sodium hydroxide were slowly added and stirred evenly, and the mixture was reacted at 90°C for 20h. After the reaction was completed, the mixture was poured into ether for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and the filter cake was dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 5:1; the molar ratio of anhydrous sodium hydroxide to polybenzimidazole was 4:1.
[0092] The prepared dried main chain spirocyclic ammonium polybenzimidazole (1-1) was added to N-methylpyrrolidone and heated to 60°C and stirred to dissolve to prepare a 3 wt% solution. After filtering and degassing, the solution was poured onto a clean plate and dried in an oven to obtain a light yellow transparent Br – The membrane was immersed in 1M NaOH solution for 48h for ion exchange, washed with deionized water until neutral, and dried to obtain OH - Type main chain spirocyclic ammonium polymer anion exchange membrane.
[0093] Example 4
[0094] Add 85% polyphosphoric acid to a stirred reactor, pass N2 protection, add 3,3'-diaminobenzidine, and 3,3'-diaminobenzidine with equal molar ratios of (III) 1,4-cyclohexanedicarboxylic acid, isophthalic acid and norbornene dicarboxylic acid, heat and stir to dissolve the monomers to a total concentration of 5wt%. Heat to 110℃ for reaction for 3h, then heat to 150℃ for reaction for 6h, and then heat to 210℃ for reaction for 6h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain a light brown polybenzimidazole. Among them, the molar ratio of 1,4-cyclohexanedicarboxylic acid: isophthalic acid: norbornene dicarboxylic acid is 6:2.5:1.5.
[0095] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain a 10wt% solution, 1,5-dibromopentane and N,N-dipropylethylamine were slowly added and stirred evenly, and the mixture was reacted at 50°C for 35h. After the reaction was completed, the mixture was poured into methanol for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 1.5:1; the molar ratio of N,N-dipropylethylamine to polybenzimidazole was 1:1.
[0096] The prepared dry main chain spirocyclic ammonium polybenzimidazole (1-1) was dissolved in N-methylpyrrolidone at 70° C. by stirring to prepare an 8 wt % solution, which was filtered and degassed to obtain a transparent ionomer solution.
[0097] The prepared dried main chain spirocyclic ammonium polybenzimidazole (1-1) was added to dimethyl sulfoxide, heated to 90°C, stirred and dissolved to prepare an 8 wt% solution. The other processes were the same as in Example 1 to obtain OH - Type main chain spirocyclic ammonium polymer anion exchange membrane.
[0098] Example 5
[0099] Add 85% polyphosphoric acid to a stirred reactor, pass N2 protection, add aromatic tetraamine (Ⅱ, A is -CH2-), (Ⅲ) 1,4-cyclohexanedicarboxylic acid and isophthalic acid in equal molar ratios to (Ⅱ), heat and stir to dissolve so that the total concentration of the monomer is 2wt%. Heat to 130℃ for reaction for 3h, then heat to 160℃ for reaction for 3h, and then heat to 180℃ for reaction for 14h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain light brown polybenzimidazole. Among them, the molar ratio of 1,4-cyclohexanedicarboxylic acid to isophthalic acid is 1:1.
[0100] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain a 5wt% solution, 1,5-dibromopentane and N,N-dimethylformamide were slowly added and stirred evenly, and the mixture was reacted at 40°C for 40h. After the reaction was completed, the mixture was poured into tetrahydrofuran for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and dried to obtain a main chain spiroammonium polybenzimidazole (1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 5:1; the molar ratio of N,N-dimethylformamide to polybenzimidazole was 5:1.
[0101] The prepared dried main chain spirocyclic ammonium polybenzimidazole (1) was added to a 1:1 methanol-dimethyl sulfoxide mixture, heated to 60°C and stirred to dissolve, to prepare a 5 wt% solution. The other processes were the same as in Example 2 to obtain OH -Type main chain spirocyclic ammonium polymer anion exchange membrane.
[0102] Example 6
[0103] Add 85% polyphosphoric acid to a stirred reactor, pass N2 protection, add 3,3'-diaminobenzidine, (III) 1,4-cyclohexanedicarboxylic acid and 1,4-naphthalene dicarboxylic acid in equal molar ratios to 3,3'-diaminobenzidine, heat and stir to dissolve the monomers to a total concentration of 12wt%. Heat to 130℃ for 6h, then heat to 140℃ for 3h, and then heat to 175℃ for 15h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain a light brown polybenzimidazole. Among them, the molar ratio of 1,4-cyclohexanedicarboxylic acid to 1,4-naphthalene dicarboxylic acid is 8:2.
[0104] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain a 12 wt% solution, 1,5-dibromopentane and anhydrous sodium carbonate were slowly added and stirred evenly, and the mixture was reacted at 85°C for 30 hours. After the reaction was completed, the mixture was poured into water for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and the filter cake was dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 4:1; the molar ratio of anhydrous sodium carbonate to polybenzimidazole was 10:1.
[0105] The prepared dried main chain spirocyclic ammonium polybenzimidazole (1-1) was added to N,N-dimethylacetamide and heated to 70°C and stirred to dissolve to prepare a 3 wt% solution. The other processes were the same as in Example 2 to obtain OH - Type main chain spirocyclic ammonium polymer anion exchange membrane.
[0106] Example 7
[0107] Add 85% polyphosphoric acid to a stirred reactor, pass N2 protection, add 3,3'-diaminobenzidine, (III) 1,4-cyclohexanedicarboxylic acid and isophthalic acid in equal molar ratios, heat and stir to dissolve the monomers to a total concentration of 7wt%. Heat to 140℃ for reaction for 0.5h, then heat to 160℃ for reaction for 1h, and then heat to 200℃ for reaction for 7h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain a polybenzimidazole copolymer containing a cyclohexane structure. Among them, the molar ratio of 1,4-cyclohexanedicarboxylic acid to isophthalic acid is 7:3.
[0108] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain a 1wt% solution, 1,5-dibromopentane and N,N-diisopropylethylamine were slowly added and stirred evenly, and the mixture was reacted at 70°C for 48h. After the reaction was completed, ethyl acetate was poured into the mixture to precipitate, the mixture was filtered, the filter cake was washed with deionized water until it was neutral, and the filter cake was dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 2:1; the molar ratio of N,N-diisopropylethylamine to polybenzimidazole was 3:1.
[0109] The film making process is the same as that in Example 3.
[0110] Example 8
[0111] Add 85% polyphosphoric acid to a stirred reactor, pass N2 protection, add 3,3'-diaminobenzidine, (III) 1,4-cyclohexanedicarboxylic acid, isophthalic acid and norbornene dicarboxylic acid in equal molar ratios with 3,3'-diaminobenzidine, heat and stir to dissolve so that the total concentration of the monomer is 10wt%. Heat to 130℃ for reaction for 0.5h, then heat to 145℃ for reaction for 5h, and then heat to 205℃ for reaction for 12h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain light brown polybenzimidazole. Among them, the molar ratio of 1,4-cyclohexanedicarboxylic acid: isophthalic acid: norbornene dicarboxylic acid is 7:2:1.
[0112] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain a 12 wt% solution, 1,5-dibromopentane and anhydrous sodium carbonate were slowly added and stirred evenly, and the mixture was reacted at 50°C for 72 hours. After the reaction was completed, the mixture was poured into dichloromethane for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and the filter cake was dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 0.5:1; the molar ratio of anhydrous sodium carbonate to polybenzimidazole was 1.5:1.
[0113] The film making process is the same as that in Example 1.
[0114] Example 9
[0115] Add 85% polyphosphoric acid to a stirred reactor, pass N2 protection, add 3,3'-diaminobenzidine, (III) 1,4-cyclohexanedicarboxylic acid and 1,7-heptanedicarboxylic acid in equal molar ratios to 3,3'-diaminobenzidine, heat and stir to dissolve the monomers to a total concentration of 3wt%. Heat to 130℃ for 10h, then heat to 150℃ for 10h, and then heat to 200℃ for 10h. The polymerization reaction ends when the reaction liquid becomes very viscous and climbs the pole. Pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight. Filter and wash the polymer with deionized water until it is neutral. Dry to obtain a light brown polybenzimidazole. Among them, the molar ratio of 1,4-cyclohexanedicarboxylic acid to 1,7-heptanedicarboxylic acid is 1:1.
[0116] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain an 8wt% solution, 1,5-dibromopentane and anhydrous potassium carbonate were slowly added and stirred evenly, and the mixture was reacted at 45°C for 48h. After the reaction was completed, the mixture was poured into ether for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and the filter cake was dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 5:1; the molar ratio of anhydrous potassium carbonate to polybenzimidazole was 2:1.
[0117] The film making process is the same as that in Example 2.
[0118] Example 10
[0119] The synthesis of polybenzimidazole was the same as in Example 4, and the molar ratio of 1,4-cyclohexanedicarboxylic acid:isophthalic acid:norbornene dicarboxylic acid was 5:4:1.
[0120] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain a 5wt% solution, 1,5-dibromopentane and anhydrous sodium hydroxide were slowly added and stirred evenly, and the mixture was reacted at 60°C for 50h. After the reaction was completed, the mixture was poured into tetrahydrofuran for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and the filter cake was dried to obtain a main chain spiroammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 1.5:1; the molar ratio of anhydrous sodium hydroxide to polybenzimidazole was 1.5:1.
[0121] The film making process is the same as that in Example 2.
[0122] Embodiment 11
[0123] The synthesis of polybenzimidazole is the same as that in Example 4.
[0124] Piperidine is added to dimethyl sulfoxide of dibromopropane Br-(CH2)3-Br to prepare a 5wt% solution, and the temperature is raised to 60°C and stirred for reaction for 15 hours; after the reaction is completed, the solution is filtered and dried to obtain M'; a certain amount of polybenzimidazole is heated and dissolved in dimethyl sulfoxide to prepare a 5wt% solution, and M' is added and reacted at 60°C for 32 hours; after the reaction is completed, the solution is poured into ether for sedimentation, filtered, and the filter cake is washed with deionized water until it is neutral, and the product is dried to obtain a main chain bispirocyclic ammonium polybenzimidazole (2-2); wherein the molar ratio of piperidine to dibromopropane is 0.5:1, and the molar ratio of polybenzimidazole to M' is 0.5:1.
[0125] The film making process is the same as that in Example 1.
[0126] Example 12
[0127] The synthesis of polybenzimidazole was the same as in Example 4, and the molar ratio of 1,4-cyclohexanedicarboxylic acid:isophthalic acid:norbornene dicarboxylic acid was 3:6.5:0.5.
[0128] Polybenzimidazole was heated and dissolved in dimethyl sulfoxide to obtain an 8wt% solution, 1,5-dibromopentane and anhydrous potassium hydroxide were slowly added and stirred evenly, and the mixture was reacted at 90°C for 24h. After the reaction was completed, the mixture was poured into ethanol for precipitation, filtered, and the filter cake was washed with deionized water until neutral, and the filter cake was dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1-1). The molar ratio of 1,5-dibromopentane to polybenzimidazole was 6:1; the molar ratio of anhydrous potassium hydroxide to polybenzimidazole was 5:1.
[0129] The film making process is the same as that in Example 1.
[0130] Table 2 Performance of ion membrane and its assembled fuel cell or water electrolyzer in the examples
[0131]
[0132] As can be seen from Table 2, the main chain spirocyclic ammonium polybenzimidazole anion exchange membrane prepared according to the present invention has a high OH - Ion conductivity, excellent mechanical properties, the time for the ion membrane to begin to rupture in Fenton's reagent at 80°C is up to 96 hours, which is better than the polymer anion exchange membrane reported in the literature. The anion membrane of the present invention has outstanding durability advantages. The main chain spirocyclic ammonium polybenzimidazole anion exchange membrane and its ionomer of the present invention have excellent performance in alkaline fuel cells and alkaline water electrolysis.
Claims
1. A polybenzimidazole with spirocyclic ammoniumization of the main chain, characterized in that: The main chain spirocyclic ammonium polybenzimidazole is obtained by polycondensation of aromatic tetraamine monomers and dicarboxylic acid monomers, and contains structural units as shown in general formula (1), (1-1), (2) or (2-2): Wherein, n is a positive integer greater than or equal to 1, k is an integer greater than or equal to 0, and l is a positive integer greater than 0; Z is Cl - Br - ,I - 、HCO3 - or OH - ; A is a methylene group -CH2-, an ether bond -O- or a carbonyl group -CO-, and each A in the structural unit may be the same or different; X is one of the following chemical structures: Y is any one of the following chemical structures: Where 2≤q≤12; The main chain spirocyclic ammonium polybenzimidazole has an intrinsic viscosity of 1.5-4.5 dL / g, or a viscosity average molecular weight of 30000-500000 g / mol, or a polymerization degree n of 20-1200.
2. The polybenzimidazole with spirocyclic ammoniumization of the main chain according to claim 1, characterized in that: 2≤q≤10; Y is structure (a), (d), (e), (h) or (i).
3. The method for preparing the main chain spirocyclic ammonium polybenzimidazole according to claim 1, characterized in that: The following steps are involved: Step 1: Synthesis of polybenzimidazole Polybenzimidazole is synthesized by solution polycondensation reaction of aromatic tetraamine monomer (II) or (II-1) and dicarboxylic acid monomer (III), as follows: Add polyphosphoric acid to a stirred reactor, and under the protection of N2, add aromatic tetraamine monomer (II) or (II-1) and dicarboxylic acid monomer (III) in an equal molar ratio to the aromatic tetraamine monomer (II) or (II-1), heat and stir to dissolve so that the total concentration of the monomers is 1-20wt%; heat to 90-140°C and stir to react for 0.5-10h, then heat to 140-160°C and stir to react for 0.5-10h, then heat to 160-210°C and react for 3-30h; terminate the polymerization reaction when the reaction liquid becomes very viscous and climbs the pole; pour the reaction liquid into a large amount of deionized water, add excess NaHCO3, and stir overnight; filter, wash the polymer with deionized water until it is neutral; dry to obtain a light brown polybenzimidazole; The structure of the aromatic tetraamine monomer (II) or (II-1) is as follows: Wherein, A is a methylene group -CH2-, an ether bond -O- or a carbonyl group -CO-, and each A in the structural unit may be the same or different; The polybenzimidazole (1') is obtained by polymerizing the aromatic tetraamine monomer (II) and the dicarboxylic acid monomer (III); The polybenzimidazole (1-1') is obtained by polymerizing the aromatic tetraamine monomer (II-1) and the dicarboxylic acid monomer (III); The dicarboxylic acid monomer (III) includes HOOC-X-COOH, HOOC-Y-COOH and norbornene dicarboxylic acid, wherein HOOC-Y-COOH may be added or not, and HOOC-X-COOH is 1,4-cyclohexane dicarboxylic acid or 1,3-cyclohexane dicarboxylic acid, that is, X is an alicyclic structure as shown below: In HOOC-Y-COOH, Y has any of the following structures: Where 2≤q≤12; When the dicarboxylic acid monomer (III) is HOOC-X-COOH, HOOC-Y-COOH and norbornene dicarboxylic acid, the polybenzimidazole containing a cyclohexane structure obtained in step 1 has a double bond functional group, which can be subsequently subjected to a cross-linking reaction; wherein the molar content of norbornene dicarboxylic acid in the dicarboxylic acid monomer (III) is less than 30%; Step 2: Synthesis of main chain spiroammonium polybenzimidazole (2.1) Synthesis of main chain spirocyclic ammonium-modified polybenzimidazole (1) or (1-1): The polybenzimidazole (1') is heated and dissolved in solvent A to obtain a 0.5-10 wt% solution, and reagent IV and catalyst A are slowly added and stirred evenly, and the mixture is reacted at 30-150° C. for 8-100 hours. After the reaction is completed, a precipitant A is poured in to precipitate, and the filter cake is filtered. The filter cake is washed with deionized water until it is neutral, and the filter cake is dried to obtain a main chain spirocyclic ammonium polybenzimidazole (1); Substituting polybenzimidazole (1-1') for (1'), the main chain spirocyclic ammonium polybenzimidazole (1-1) is obtained by the same reaction; The reagent IV is 1,5-dibromopentane, and the molar ratio of 1,5-dibromopentane to polybenzimidazole is (0.5-10):1, and the molar ratio of catalyst A to polybenzimidazole is (0.5-10):1; (2.2) Synthesis of main chain spirocyclic ammonium polybenzimidazole (2) or (2-2): Add piperidine to dibromoalkane Br-(CH2) m -Br is prepared into a 0.5-10wt% solution in solvent B, heated to 30-90°C and stirred for reaction for 6-72h; after the reaction is completed, filtered and dried to obtain a bromide salt M'; The polybenzimidazole (1') is heated and dissolved in a solvent A to obtain a 0.5-10 wt% solution, and a bromide salt M' is added and reacted at 30-150° C. for 8-100 hours. After the reaction is completed, a precipitant A is poured in, filtered, and the filter cake is washed with deionized water until it is neutral. The product is dried to obtain a main chain spiroammonium polybenzimidazole (2); wherein 2≤m≤6 is an integer; Substituting polybenzimidazole (1-1') for (1'), the main chain spirocyclic ammonium polybenzimidazole (2-2) was obtained by the same reaction; The piperidine and dibromoalkane Br-(CH2) m The molar ratio of -Br is 0.05 to 1:1; the molar ratio of polybenzimidazole to bromide salt M' is 0.1 to 1.2:
1.
4. The method for preparing the main chain spiroammonium polybenzimidazole according to claim 3, characterized in that: The solvent A is one or a mixture of two or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dichloromethane, tetrahydrofuran, formic acid, and methanesulfonic acid; The solvent B is one or a mixture of two or more of methanol, ethanol, N,N-dimethylformamide, tetrahydrofuran, acetonitrile, ethyl acetate, acetone, dimethyl sulfoxide, N,N-dimethylacetamide, and N-methylpyrrolidone; The precipitant A is one or a mixture of two or more of methyl tert-butyl ether, ethyl ether, methanol, ethanol, ethyl acetate, dichloromethane, tetrahydrofuran, acetone, and water; The catalyst A is one or a mixture of two or more of anhydrous sodium carbonate, anhydrous potassium carbonate, anhydrous sodium hydride, anhydrous sodium hydroxide, anhydrous potassium hydroxide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diisopropylethylamine, N,N-dimethylpropylamine, and N,N-dipropylethylamine.
5. A method for preparing anion exchange membrane using polybenzimidazole with spirocyclic ammonium in the main chain, the polybenzimidazole with spirocyclic ammonium in the main chain prepared by claim 3 or 4, characterized in that: The specific steps are as follows: The dried main chain spirocyclic ammonium polybenzimidazole (1), (1-1), (2) or (2-2) is added to solvent C, heated to 30-150° C., stirred and dissolved to prepare a 1-20 wt % solution, filtered, degassed, poured onto a clean plate, and dried to obtain Br – The membrane is immersed in 1M or 2M NaOH solution for 24-48 hours, after ion exchange, it is washed with deionized water until neutral, and dried to obtain OH - Type polymer anion exchange membrane.
6. A method for preparing an ionomer solution using a polybenzimidazole with a main chain spirocyclic ammonium ring, wherein the polybenzimidazole with a main chain spirocyclic ammonium ring is prepared according to claim 3 or 4, characterized in that: The specific steps are as follows: The dried main chain spirocyclic ammonium polybenzimidazole (1), (1-1), (2) or (2-2) is heated to 30-150° C. in solvent C and stirred to dissolve to prepare a 1-10 wt % solution, which is filtered and degassed to obtain a transparent ionomer solution.
7. The method for preparing anion exchange membrane using a main chain spirocyclic ammonium polybenzimidazole according to claim 5, wherein the solvent C is one or a mixture of two or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, methanol, ethanol, isopropanol, formic acid, acetic acid, and methanesulfonic acid.
8. Use of an anion exchange membrane prepared from a main chain spirocyclic ammonium polybenzimidazole according to claim 5, characterized in that: The prepared anion exchange membrane is used in fuel cells, water electrolysis, carbon dioxide conversion, and liquid flow batteries.
9. Use of the ionomer solution prepared from the main chain spiroammonium polybenzimidazole according to claim 6, characterized in that: The prepared ionomer solution is used in fuel cells, water electrolysis, flow batteries, and carbon dioxide conversion.