A nanofiber composite proton exchange membrane and its preparation method

The nanofiber composite proton exchange membrane prepared by electrospinning solves the problem of poor hydrophobicity of existing proton exchange membrane materials, improves the hydrophilicity and mechanical properties of the membrane, reduces energy consumption, and achieves efficient proton transfer and thermal stability, making it suitable for hydrogen production by water electrolysis.

CN116607323BActive Publication Date: 2026-11-10SHANGHAI JUNA NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310447898.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2026-11-10
Estimated Expiration
2043-04-24

AI Technical Summary

Technical Problem

Existing proton exchange membrane materials have poor hydrophobicity, resulting in high energy consumption, severe membrane fouling, poor mechanical properties, low proton transfer efficiency, and high cost.

Method used

A polysulfone-hydroxypropyl cellulose casting solution was prepared by electrospinning. A nanofiber composite membrane was obtained by electrospinning and then immersed in a perfluorosulfonic acid polymer solution to prepare a nanofiber composite proton exchange membrane.

Benefits of technology

It improves the hydrophilicity, mechanical properties and proton conductivity of the membrane, reduces energy consumption, and enhances the thermal stability and durability of the membrane, making it suitable for hydrogen production by water electrolysis.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention belongs to the field of proton exchange membrane preparation technology, specifically disclosing a nanofiber composite proton exchange membrane and its preparation method. The method includes adding hydroxypropyl cellulose powder to an N,N-dimethylacetamide solvent and ultrasonically treating it to obtain a dispersion; adding a pore-forming agent to the dispersion, dissolving it, adding dried polysulfone, heating, and stirring to obtain a polysulfone-hydroxypropyl cellulose casting solution; electrospinning the casting solution to obtain a nanofiber composite membrane; and impregnating the nanofiber composite membrane in a perfluorosulfonic acid polymer solution to prepare the nanofiber composite proton exchange membrane. The nanofiber proton exchange membrane of this invention exhibits high proton conductivity, hydrophilicity, mechanical properties, thermal stability, and durability. The preparation method of this invention is simple and has low energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of proton exchange membrane preparation technology, and particularly to a nanofiber composite proton exchange membrane and its preparation method. Background Technology

[0002] Hydrogen energy, as a green and environmentally friendly energy carrier, can achieve efficient conversion between hydrogen and electricity through water electrolysis technology. Currently, there are three main technical routes for hydrogen production via water electrolysis: alkaline electrolysis (AWE), proton exchange membrane (PEM) electrolysis, and solid oxide electrolysis (SOEC).

[0003] Currently, proton exchange membranes mainly include perfluorosulfonic acid type proton exchange membranes, non-fluoropolymer proton exchange membranes, and composite proton exchange membranes. The durability of PEM determines the durability of PEMWE (proton exchange membrane electrolyzer).

[0004] Polysulfone (PSF) is a common material for proton exchange membranes, possessing excellent properties such as outstanding oxidation, thermal, and hydrolytic stability, as well as good mechanical and film-forming properties due to its diarylsulfonyl groups. However, PSF is a highly hydrophobic material with very poor hydrophilicity, which leads to two serious problems during membrane use: First, due to the material's hydrophobicity, a larger pressure difference needs to be formed across the membrane during filtration, resulting in greater energy consumption. Second, the hydrophobicity easily leads to the adhesion of organic molecules such as proteins and bacteria to the membrane surface and inside the pores, causing problems such as decreased flux, pore blockage, shortened lifespan, and severe membrane fouling. Therefore, it is often necessary to improve the hydrophilicity of the membrane.

[0005] Existing methods provide a class of composite membranes whose matrix is ​​made of a stable inert polymer and is typically filled and supported by a hydrophilic inorganic material, such as polysulfone incorporating hydrophilic zirconia particles. However, due to the poor surface compatibility between polysulfone and hydrophilic zirconia particles, the interaction between the organic polymer and the inorganic filler is weak, resulting in high membrane brittleness and poor mechanical properties.

[0006] Existing methods also provide a method for modifying the hydrophilicity of polysulfone membranes through blending. This involves adding polymers with hydrophilic or other properties during the preparation of the casting solution, offering high controllability and making it easier to industrialize compared to other modification methods. For example, a polysulfone (PSF) membrane is impregnated in a deionized solution of hydroxypropyl cellulose (HPC) for 16 hours, followed by washing with deionized water for 16 hours. However, this method lacks an insoluble treatment to ensure HPC adheres to the hydrophobic membrane surface and a preferred thermal modification, resulting in the HPC dissolving during washing as it cannot remain on the membrane surface.

[0007] On the other hand, electrospinning is a simple and effective method for preparing large-scale polymer nanofibers. It primarily utilizes electrostatic forces generated by high voltage to prepare electrostatic nanofibers from polymer solutions or melts. Electrospun nanofibers possess advantages such as large specific surface area, high porosity, and good fiber continuity. They have already demonstrated excellent performance in many fields, including air filtration, adsorption and removal of heavy metal ions and / or multi-component pollutants, and the development of modified multi-component nanocomposites, and will gradually replace traditional nanofiber materials in a wider range of applications. Electrospun nanofiber membranes are novel nanoscale support materials. Typical electrospun nanofiber membranes have high porosity (e.g., 80-95%) and large specific surface area (approximately 10-40 m²). 2 Electrospun nanofiber membranes, with their advantages of low mass transfer resistance and easy surface modification, are widely used as carriers for various membrane materials. In proton exchange membranes, their application mainly involves combining with proton exchange materials as a three-dimensional nanonetwork support material; simultaneously, their high porosity and high specific surface area are utilized to improve proton conduction efficiency.

[0008] Perfluorosulfonic acid membranes (Nafion membranes) have advantages such as high mechanical strength, long service life, high proton conductivity, and good chemical stability. However, these membranes are expensive, and their ionic conductivity is strongly dependent on the water content of the membrane. The conductivity decreases significantly when the water content is low or the temperature is high, especially above 100°C.

[0009] Therefore, if a proton exchange membrane can be provided that has a simple preparation process, low cost, good hydrophilicity, good mechanical properties, good thermal, chemical and structural stability, and high proton transfer efficiency, it will be more conducive to the development of hydrogen production by water electrolysis. Summary of the Invention

[0010] In view of this, the purpose of this invention is to provide a nanofiber composite proton exchange membrane and its preparation method, so as to solve the problems of poor hydrophilicity, low proton transfer efficiency, and poor mechanical properties of polysulfone proton exchange membranes in the prior art.

[0011] To achieve the above and related objectives, the first aspect of the present invention provides a method for preparing a nanofiber composite proton exchange membrane, the method comprising the following steps:

[0012] (1) Preparation of polysulfone-hydroxypropyl cellulose casting solution: Hydroxypropyl cellulose powder was added to N,N-dimethylacetamide solvent and ultrasonically treated to obtain a dispersion; a pore-forming agent was added to the dispersion, dissolved, and then dry polysulfone was added, heated and stirred to obtain polysulfone-hydroxypropyl cellulose casting solution.

[0013] (2) Obtain a nanofiber composite membrane by electrospinning the casting solution in step (1);

[0014] (3) The nanofiber composite membrane from step (2) is immersed in a perfluorosulfonic acid polymer solution to prepare a nanofiber composite proton exchange membrane.

[0015] In one embodiment of this application, the mass fraction of hydroxypropyl cellulose in step (1) is 0.5% to 2%.

[0016] In one embodiment of this application, the mass fraction of the pore-forming agent in step (1) is 5% to 15%.

[0017] In one embodiment of this application, the mass fraction of polysulfone in step (1) is 10% to 25%.

[0018] In one embodiment of this application, the ultrasonic treatment time in step (1) is 20 to 60 minutes.

[0019] In one embodiment of this application, the heating temperature in step (1) is 70-90°C.

[0020] In one embodiment of this application, the pore-forming agent is any one of polyethylene glycol, povidone, polyurethane, urea, and polyvinylpyrrolidone.

[0021] In one embodiment of this application, the voltage for electrospinning in step (2) is 10-25kV.

[0022] In one embodiment of this application, the electrospinning temperature in step (2) is 20–70°C.

[0023] In one embodiment of this application, the electrospinning time in step (2) is 1 to 60 hours.

[0024] In one embodiment of this application, the nanofiber composite membrane in step (2) is cold-rolled for 1 to 5 minutes.

[0025] In one embodiment of this application, the cold-rolled nanofiber composite membrane is spread in a container containing a perfluorosulfonic acid polymer solution, then the perfluorosulfonic acid polymer solution is added, the membrane is left to stand, and then the nanofiber composite membrane is removed and dried.

[0026] In one embodiment of this application, the dried nanofiber composite membrane is immersed in a sulfuric acid solution, and washed after immersion to obtain a nanofiber composite proton exchange membrane. The immersion time is 6 to 24 hours, and the volume concentration of the sulfuric acid solution is 1 to 2.5 mol / L.

[0027] In one embodiment of this application, the drying temperature is 20–80°C.

[0028] A second aspect of this invention also provides a nanofiber composite proton exchange membrane prepared according to the above-described preparation method. The nanofiber composite proton exchange membrane prepared by this invention is suitable for hydrogen production via water electrolysis, exhibiting high hydrogen production efficiency, good durability, and the ability to produce hydrogen through long-term water electrolysis.

[0029] The beneficial technical effects of this invention are as follows:

[0030] This invention uses hydroxypropyl cellulose, a polymer material with high hydrophilicity, to blend and modify hydrophobic polysulfone. The modification process is simple to operate and highly controllable.

[0031] Existing technologies propose methods for immobilizing hydroxyalkyl cellulose in hydrophobic membranes. These methods involve immersing a proton exchange membrane composed of a sulfone polymer in an alcoholic solution containing hydroxyalkyl cellulose, followed by high-pressure reactor treatment in the presence of steam or water, and immersion in boiling water. However, this method may reduce the hydrophilicity by excessively promoting the thermal modification of hydroxyalkyl cellulose at high temperatures, thus failing to fully express the inherent hydrophilic properties of hydroxyalkyl cellulose. Therefore, this invention maintains a relatively low temperature throughout the preparation of the polysulfone-hydroxypropyl cellulose casting solution to avoid excessively promoting the thermal modification of hydroxypropyl cellulose.

[0032] Furthermore, the present invention prepares a polysulfone-hydroxypropyl cellulose casting solution to obtain a nanofiber composite membrane in one step, avoiding the problem that the hydroxypropyl cellulose cannot adhere to the polysulfone surface and is easily dissolved during cleaning when the polysulfone membrane is first prepared and then immersed in the hydroxypropyl cellulose solution.

[0033] In this invention, the polysulfone-hydroxypropyl cellulose casting solution is prepared at a uniform temperature of approximately 70°C, which promotes the adhesion between hydroxypropyl cellulose and polysulfone. This results in good adhesion of hydroxypropyl cellulose on the electrospun nanofiber composite membrane, preventing detachment during subsequent processing and ensuring the nanofiber composite membrane maintains good hydrophilicity. Furthermore, the electrospun nanofiber composite membrane possesses advantages such as large specific surface area, high porosity, good fiber continuity, and high mass transfer efficiency.

[0034] This invention involves cold-rolling the nanofiber composite membrane to make it denser and more uniform. After immersing the nanofiber composite membrane in a perfluorosulfonic acid polymer solution (Nafion solution), the membrane undergoes complete protonation treatment, resulting in a nanofiber composite proton exchange membrane with higher thermal stability, proton conductivity, swelling degree, and selectivity.

[0035] In summary, the hydrophilic modified polysulfone proton exchange membrane prepared by electrospinning in this invention, after treatment with Nafion solution, exhibits high proton conductivity, hydrophilicity, mechanical properties, and thermal stability, and the nanofiber composite proton exchange membrane demonstrates good durability. Furthermore, the preparation method of this invention is simple, the entire preparation process is conducted at relatively low temperatures, and energy consumption is low. Detailed Implementation

[0036] Unless otherwise defined, all technical and / or scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. It should be understood that certain features of the invention (described in the context of separate embodiments for clarity) may also be provided in combination in a single embodiment. Conversely, multiple features of the invention (described in the context of a single embodiment for brevity) may also be provided separately or in any suitable combination or, where appropriate, in any other described embodiment of the invention. Certain features described in the context of various embodiments will not be considered essential features of those embodiments unless the embodiment is inoperable without those elements. The invention is further illustrated below by specific examples; however, it should be noted that the specific preparation methods, conditions, and results described in the embodiments of the invention are merely illustrative and should not be construed as limiting the scope of protection of the invention. All equivalent changes or modifications made in accordance with the spirit and essence of the invention should be covered within the scope of protection of the invention.

[0037] It's important to note that proton conductivity is a crucial performance indicator for proton exchange membranes used in water electrolysis for hydrogen production. The proton conductivity of a proton exchange membrane primarily depends on the interaction between water and acidic groups within the hydrophilic region. At lower water contents, the hydrogen bonds formed between water and acidic groups are shorter and more tightly bound, making their formation and breakage more difficult. This results in a higher activation energy for proton transport and a lower proton transport capacity. Conversely, as the water content increases, extended hydrogen bonds are more easily formed between water molecules, thus facilitating proton transport. Temperature is also a significant factor affecting proton conductivity; higher temperatures increase the speed of proton and water molecule movement, thereby improving proton conductivity.

[0038] Hygroscopicity is an important property of proton exchange membranes, closely related to ion exchange capacity and proton conductivity. Most proton exchange membrane materials follow the transport mechanism within the proton transport mechanism, in which protons bind to surrounding water molecules through hydrogen bonding, transforming into hydrated hydrogen ions (H+). + (H2O) x The conduction of protons relies on electroosmotic resistance. Water molecules play an important role in the transfer of protons, so a certain water absorption rate is necessary for the transport of protons.

[0039] This invention provides a method for preparing a nanofiber composite proton exchange membrane, the method comprising the following steps:

[0040] (1) Preparation of polysulfone-hydroxypropyl cellulose casting solution: Hydroxypropyl cellulose powder was added to N,N-dimethylacetamide solvent and ultrasonically treated to obtain a dispersion; a pore-forming agent was added to the dispersion, dissolved, and then dry polysulfone was added, heated and stirred to obtain polysulfone-hydroxypropyl cellulose casting solution.

[0041] (2) Obtain a nanofiber composite membrane by electrospinning the casting solution in step (1);

[0042] (3) The nanofiber composite membrane from step (2) is immersed in a perfluorosulfonic acid polymer solution to prepare a nanofiber composite proton exchange membrane.

[0043] The present invention also provides a nanofiber composite proton exchange membrane prepared according to the above preparation method.

[0044] Example 1

[0045] (1) Preparation of polysulfone-hydroxypropyl cellulose casting solution: 0.5% by mass of hydroxypropyl cellulose (HPC) powder was added to a three-necked flask containing N,N-dimethylacetamide (DMAc) solvent and ultrasonically treated for 30 min to obtain HPC-DMAc dispersion; 5% by mass of polyvinylpyrrolidone was added to HPC-DMAc dispersion under a constant temperature water bath at 70℃. After complete dissolution, polysulfone with a mass fraction of 10% was added and dried in a vacuum environment at 60℃ for 24 h. The mixture was stirred until it was completely dissolved to obtain a uniform polysulfone-hydroxypropyl cellulose casting solution, which was then allowed to stand at room temperature for 12 h.

[0046] (2) The polysulfone-hydroxypropyl cellulose casting solution in step (1) was electrospun to obtain a nanofiber composite membrane. The electrospinning parameters were: voltage 2kV, flow rate 50 μL / min, spinning distance 15cm, temperature 50℃, relative humidity 40%, collection speed 100rpm, and spinning time 6h.

[0047] (3) The nanofiber composite membrane obtained in step (2) is subjected to cold rolling at room temperature with a pressure of 6 MPa and a time of 3 min; a small amount of perfluorosulfonic acid polymer solution (Nafion solution) is poured into a clean container, and then the nanofiber composite membrane is spread flat on the Nafion solution. A certain amount of Nafion solution is added and left to stand for a while. The prepared nanofiber composite membrane is placed in a vacuum oven and placed under low vacuum for 10 h. The temperature of the vacuum oven is then adjusted to 60 °C and heated for 10 h. The temperature is then adjusted to 80 °C and kept at that temperature for 10 h. The nanofiber composite membrane is then removed.

[0048] The dried nanofiber composite membrane was immersed in a sulfuric acid solution with a volume concentration of 1.5 mol / L for 20 h to completely protonate the nanofiber composite membrane. Then, the nanofiber composite membrane was washed repeatedly with deionized water and soaked in deionized water until the water was neutral. The nanofiber composite membrane was then removed, dried, and the nanofiber composite proton exchange membrane was obtained.

[0049] Example 2

[0050] The difference between this embodiment and Embodiment 1 is that:

[0051] (1) Preparation of polysulfone-hydroxypropyl cellulose casting solution: 1.0% by mass of hydroxypropyl cellulose (HPC) powder was added to a three-necked flask containing N,N-dimethylacetamide (DMAc) solvent and ultrasonically treated for 30 min to obtain HPC-DMAc dispersion; 8% by mass of polyvinylpyrrolidone was added to HPC-DMAc dispersion under a constant temperature water bath at 70℃. After complete dissolution, polysulfone with a mass fraction of 14% was added and dried in a vacuum environment at 60℃ for 24 h. The mixture was stirred until it was completely dissolved to obtain a uniform polysulfone-hydroxypropyl cellulose casting solution, which was then allowed to stand at room temperature for 12 h.

[0052] Example 3

[0053] The difference between this embodiment and Embodiment 1 is that:

[0054] (1) Preparation of polysulfone-hydroxypropyl cellulose casting solution: 1.5% by mass of hydroxypropyl cellulose (HPC) powder was added to a three-necked flask containing N,N-dimethylacetamide (DMAc) solvent and ultrasonically treated for 30 min to obtain HPC-DMAc dispersion; 10% by mass of polyvinylpyrrolidone was added to HPC-DMAc dispersion under a constant temperature water bath at 70℃. After complete dissolution, polysulfone with a mass fraction of 18% was added and dried in a vacuum environment at 60℃ for 24 h. The mixture was stirred until it was completely dissolved to obtain a uniform polysulfone-hydroxypropyl cellulose casting solution, which was then allowed to stand at room temperature for 12 h.

[0055] Example 4

[0056] The difference between this embodiment and Embodiment 1 is that:

[0057] (1) Preparation of polysulfone-hydroxypropyl cellulose casting solution: 2.0% by mass of hydroxypropyl cellulose (HPC) powder was added to a three-necked flask containing N,N-dimethylacetamide (DMAc) solvent and ultrasonically treated for 30 min to obtain HPC-DMAc dispersion; 15% by mass of polyvinylpyrrolidone was added to HPC-DMAc dispersion under a constant temperature water bath at 70℃. After complete dissolution, polysulfone with a mass fraction of 22% was added and dried in a vacuum environment at 60℃ for 24 h. The mixture was stirred until it was completely dissolved to obtain a uniform polysulfone-hydroxypropyl cellulose casting solution, which was then allowed to stand at room temperature for 12 h.

[0058] Example 5

[0059] The difference between this embodiment and embodiment 3 is as follows:

[0060] (3) The prepared nanofiber composite membrane was cold-rolled at room temperature at a pressure of 6 MPa for 5 min. A small amount of perfluorosulfonic acid polymer solution (Nafion solution) was poured into a clean container, and then the nanofiber composite membrane was spread flat on the Nafion solution. A certain amount of Nafion solution was added and the membrane was left to stand for a while. The prepared nanofiber composite membrane was placed in a vacuum oven and placed under low vacuum for 10 h. The temperature of the vacuum oven was then adjusted to 60 °C and heated for 10 h. The temperature was then adjusted to 80 °C and kept at that temperature for 10 h. The nanofiber composite membrane was then removed.

[0061] The dried nanofiber composite membrane was immersed in a sulfuric acid solution with a volume concentration of 2.5 mol / L for 15 hours to completely protonate the nanofiber composite membrane. Then, the nanofiber composite membrane was washed repeatedly with deionized water and soaked in deionized water until the water was neutral. The nanofiber composite membrane was then removed, dried, and the nanofiber composite proton exchange membrane was obtained.

[0062] Comparative Example 1

[0063] Preparation of sulfonated polysulfone proton exchange membrane: 20.0g of polysulfone was placed in sufficient dichloroethane and stirred until dissolved. Fuming sulfuric acid was added dropwise. After the reaction was completed, the dichloroethane and excess acid were poured off. Then, the membrane was washed with distilled water until neutral and dried in a vacuum drying oven at 50℃ to obtain the sulfonated polysulfone product.

[0064] The sulfonated polysulfone product was placed in a 250 mL round-bottom beaker, an organic solvent was added, and the mixture was reacted in a water bath at a certain temperature for 3 hours. After the reaction was completed, the film-forming solution was allowed to stand at room temperature for more than 24 hours to degas. A certain amount of sulfonated polymer solution was poured evenly onto a glass plate covered with a polysulfone film. The glass plate wrapped with fine copper wire was moved at a uniform speed to allow the film-forming solution to flow onto the glass plate. The glass plate was then placed stably in a constant-temperature gel water bath and allowed to stand for 30 minutes. Finally, the peeled polymer sheet film was stored in a deionized water solution.

[0065] Comparative Example 2

[0066] Preparation of HPC-PSF proton exchange membrane: The polysulfone (PSF) membrane was immersed in a deionized solution of hydroxypropyl cellulose (HPC) for 16 hours, and then washed with deionized water for 16 hours to obtain the HPC-PSF proton exchange membrane.

[0067] Comparative Example 3

[0068] DuPont Nafion 117 membrane.

[0069] Performance testing

[0070] Example 3 and Comparative Examples 1-3 were used as test samples, and the following performance tests were performed respectively:

[0071] Mechanical property testing: Mechanical properties were characterized by tensile testing using a universal tensile testing machine (Instron 3369 USA) at room temperature and in a completely dry state, with a tensile rate of 20 mm / min. The test samples were cut into 10 mm × 40 mm strips, with three strips tested per group, and the average value was calculated as the final result. The mechanical property test results are shown in Table 1.

[0072] Proton conductivity performance testing: A CH1660D electrochemical workstation (frequency range 1-10) manufactured by Beijing Huake Putian Technology Co., Ltd. was used. 5 Using two electrodes and a proton conductivity measuring device, an AC impedance diagram was obtained. The intercept of the spectral line on the X-axis at the high-frequency end of the AC impedance diagram is the membrane resistance R. The proton conductivity of the membrane is calculated using the following formula:

[0073] σ=I / (twR)

[0074] Where σ(S / cm) represents the proton conductivity of the membrane, I(cm) represents the distance between the two electrodes, t(cm) and w(cm) represent the thickness and width of the sample membrane, respectively, and R(Ω) represents the measured resistance of the membrane. The proton conductivity results are shown in Table 2.

[0075] Water absorption test: Water absorption rate (WU) is the ratio of the mass difference of the membrane in the wet and dry states to the dry membrane mass. The test membrane is dried at 60°C and then weighed, and the weight is recorded as W. d Then soak it in distilled water for 24 hours, remove it and quickly wipe off the water droplets on the surface with filter paper, weigh it, and record it as W. w The water absorption rate of the membrane can be calculated using the following formula:

[0076] WU(%)=[(W w -W d ) / W d ]×100

[0077] The results of the water absorption test are shown in Table 3.

[0078] Table 1. Mechanical performance test results of Example 3 and Comparative Examples 1-3

[0079] Tensile stress (MPa) Example 3 35 Comparative Example 1 31 Comparative Example 2 30 Comparative Example 3 27

[0080] High mechanical strength of proton exchange membranes is a prerequisite for expanding their practicality. The mechanical properties of the nanofiber composite proton exchange membrane of Example 3 and the membranes of Comparative Examples 1 to 3 were tested, and the results are shown in Table 1. The tensile stress of the Nafion 117 membrane was 27 MPa, while the HPC-PSF / Nafion composite proton exchange membrane of Example 3 increased the mechanical properties of the Nafion membrane to a certain extent, and its mechanical strength was significantly improved compared with the sulfonated polysulfone membrane and HPC-PSF membrane that had not undergone electrospinning.

[0081] Table 2. Proton conductivity test results of Example 3 and Comparative Examples 1-3

[0082] σ(S / cm)20℃ σ(S / cm)40℃ σ(S / cm)60℃ σ(S / cm)80℃ Example 3 0.091 0.118 0.131 0.152 Comparative Example 1 0.085 0.094 0.115 0.138 Comparative Example 2 0.088 0.105 0.121 0.101 Comparative Example 3 0.082 0.088 0.116 0.132

[0083] This invention calculates the proton conductivity of Examples 3 and Comparative Examples 1-3 by measuring the AC impedance between two electrodes. The samples to be tested were cut into 2×1.5cm pieces. 2 The samples were then tested using a proton conductivity measuring device. The samples were placed on two copper plates, the membrane was fixed vertically, and completely immersed in distilled water. The positive and negative electrodes were connected, and the electrochemical workstation was turned on to measure the proton conductivity. Following the above testing method, four samples were placed in water baths at different temperatures: 20℃, 40℃, 60℃, and 80℃. The proton conductivity of different sample membranes at different temperatures was measured, and the results are shown in Table 2.

[0084] As shown in Table 2, under 100% relative humidity, the proton conductivity of Example 3, Comparative Example 1, and Comparative Example 3 all increased with increasing temperature. Furthermore, the proton conductivity of the composite proton exchange membrane of Example 3, containing nanofibers, was higher than that of Comparative Examples 1-3 at all temperatures. However, the proton conductivity of the HPC-PSF proton exchange membrane in Comparative Example 2 initially increased and then decreased with increasing temperature. This is because the hydroxypropyl cellulose in the HPC-PSF proton exchange membrane of Comparative Example 2 dissolved from the polysulfone membrane with increasing temperature and failed to adhere firmly to the polysulfone membrane. The preparation method of this invention modifies hydrophilic hydroxypropyl cellulose by blending it with polysulfone. The aqueous solution of hydroxypropyl cellulose has high viscosity, which further improves the hydrophobicity of polysulfone and increases its proton conductivity. At the same time, the temperature is maintained at about 70°C during the preparation of the casting solution and electrospinning process, which can effectively bind hydroxypropyl cellulose and polysulfone together. As a result, the nanofiber composite proton exchange membrane of Example 3 of this invention can still maintain good proton conductivity under continuously increasing temperature environment.

[0085] Table 3. Results of water absorption tests for Example 3 and Comparative Examples 1-3

[0086] WU (%) 20℃ WU (%) 40℃ WU (%) 60℃ WU (%) 80℃ Example 3 28.2 30.6 33.7 38.5 Comparative Example 1 20.2 22.3 28.6 33.4 Comparative Example 2 20.7 22.5 28.9 27.3 Comparative Example 3 19.1 21.8 25.7 32.1

[0087] In this invention, the test samples from Example 3 and Comparative Examples 1-3 were cut into 20mm × 10mm strips. The samples were dried in a 60℃ oven for 3 hours, and their mass was measured. Then, the samples were immersed in distilled water at room temperature for 24 hours. After removal, the surface moisture was quickly wiped dry with filter paper, and the weight of the samples was measured. Following the above method, the samples were then placed in distilled water and heated for 24 hours in water baths at 20℃ and 40℃, and in water-oil baths at 60℃ and 80℃, respectively. The dry and wet masses of all samples were recorded using the above measurement method. The test results are shown in Table 3.

[0088] As shown in Table 3, the water absorption rates of Example 3, Comparative Examples 1 and 3 all increased with increasing temperature. Furthermore, the water absorption rate of Example 3 was higher than that of Comparative Examples 1-3 at any temperature. This indicates that the nanofiber composite proton exchange membrane prepared by electrospinning in this invention has good hydrophilicity, low mass transfer resistance, and good water absorption. In contrast, the water absorption rate of Comparative Example 2 decreased with increasing temperature. This suggests that the hydroxypropyl cellulose in Comparative Example 2 was not subjected to a bonding treatment and dissolved from the polysulfone membrane at high temperatures, resulting in poor water absorption and mass transfer at high temperatures.

[0089] In summary, the nanofiber composite proton exchange membrane prepared by the method of the present invention has good water absorption, mechanical properties and proton conductivity, as well as good thermal stability and durability.

[0090] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A method for preparing a nanofiber composite proton exchange membrane, characterized in that, The method includes the following steps: (1) Preparation of polysulfone-hydroxypropyl cellulose casting solution: 1.5% by mass of hydroxypropyl cellulose HPC powder was added to a three-necked flask containing N,N-dimethylacetamide DMAc solvent and ultrasonically treated for 30 min to obtain HPC-DMAc dispersion; 10% by mass of polyvinylpyrrolidone was added to HPC-DMAc dispersion under a constant temperature water bath at 70℃. After complete dissolution, polysulfone with a mass fraction of 18% was added and dried in a vacuum environment at 60℃ for 24 h. The mixture was stirred until it was completely dissolved to obtain a uniform polysulfone-hydroxypropyl cellulose casting solution. The solution was allowed to stand at room temperature for 12 h. (2) The polysulfone-hydroxypropyl cellulose casting solution in step (1) was electrospun to obtain a nanofiber composite membrane. The electrospinning parameters were: voltage of 2kV, flow rate of 50 μL / min, spinning distance of 15cm, temperature of 50℃, relative humidity of 40%, collection speed of 100rpm, and spinning time of 6h. (3) The nanofiber composite membrane obtained in step (2) is subjected to cold rolling at room temperature with a pressure of 6 MPa and a time of 3 min; a small amount of perfluorosulfonic acid polymer solution Nafion solution is poured into a clean container, and then the nanofiber composite membrane is spread flat on the Nafion solution, a certain amount of Nafion solution is added, and it is left to stand for a while; the prepared nanofiber composite membrane is placed in a vacuum oven and placed under low vacuum for 10 h, then the temperature of the vacuum oven is adjusted to 60℃ and heated for 10 h, then the temperature is adjusted to 80℃ and kept for 10 h, and the nanofiber composite membrane is taken out. The dried nanofiber composite membrane was immersed in a sulfuric acid solution with a volume concentration of 1.5 mol / L for 20 h to completely protonate the nanofiber composite membrane. Then, the nanofiber composite membrane was washed repeatedly with deionized water and soaked in deionized water until the water was neutral. The nanofiber composite membrane was then removed, dried, and the nanofiber composite proton exchange membrane was obtained.

2. The nanofiber composite proton exchange membrane prepared by the preparation method according to claim 1.

Citation Information

Patent Citations

  • Fuel cell proton exchange membrane based on solution jet spinning technology

    CN105037770A

  • Preparation method of nanocellulose composite polysulfone hollow fiber membrane

    CN105664740A