Polyethylene film for heat sealing

By using a polyethylene film with a specific composition, the problems of high energy consumption and insufficient heat adhesion strength caused by high-temperature heat sealing are solved, achieving low-temperature high-strength sealing and improving packaging efficiency and the quality of contents.

CN116635459BActive Publication Date: 2026-11-17SABIC GLOBAL TECHNOLOGIES BV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180088111.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-29
Filing Date
2021-11-30
Publication Date
2026-11-17
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

Existing polyethylene films require high temperatures to form a high-strength seal during the heat-sealing process, resulting in high energy consumption and adverse effects on the quality of the packaged contents. Furthermore, insufficient heat adhesion strength affects packaging efficiency.

Method used

A polyethylene film with a specific composition, including sealing layer A, has a density of 870-920 kg/m3 and specific α-TREF fraction, shear storage modulus and melt flow rate. It forms a seal with high strength and high thermal adhesion strength by heat sealing at low temperature.

Benefits of technology

This technology enables the formation of seals with high strength and high thermal adhesion at reduced temperatures, improving the efficiency of the packaging process, preserving the quality of the contents, and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

This invention relates to a membrane comprising at least one sealing layer, wherein at least one layer A of the sealing layer comprises polyethylene containing a structural portion derived from ethylene and a structural portion derived from an α-olefin comprising 4 to 10 carbon atoms, said polyethylene having a strength of ≥870 and ≤920 kg / m³ as determined according to ASTM D792 (2013). 3 The density of the polyethylene, wherein the polyethylene has: • a material fraction eluted at a temperature ≤30.0°C in analytical temperature rise elution fractionation (a-TREF) of ≤14.0 wt%, preferably ≥5.0 wt% and ≤14.0 wt%, more preferably ≥5.0 wt% and ≤12.5 wt%, relative to the total weight of the polyethylene; • a shear storage modulus G', G', and G" of <500 Pa, determined according to ISO 6721-10 (2015) at 190°C; • a melt mass flow rate ≥4.00 and ≤8.00 g / 10 min, determined according to ASTM D1238 (2013) at 190°C and a load of 2.16 kg; and • a chemical composition distribution width (CCDB) ≥10.0, preferably ≥15.0. This membrane allows for sealing at reduced temperatures while still providing the desired sealing strength and desired thermal adhesion strength.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention relates to polyethylene films for heat sealing, and multilayer structures comprising such films. The invention also relates to articles comprising such films, and methods for producing sealing articles comprising such films.

[0002] Films containing or composed of polyethylene materials are widely used in various applications. A specific example of the application of such polyethylene films is food packaging. The use of polyethylene allows for the packaging of food in a very hygienic manner, helps preserve packaged products for extended periods, and can be done in a very economical way. Furthermore, polyethylene films can be produced with a very attractive appearance.

[0003] Suitable polyethylene materials for membrane production include low-density polyethylene (LDPE), high-density polyethylene (HDPE), and linear low-density polyethylene (LLDPE). Linear low-density polyethylene is particularly suitable for a variety of membrane applications.

[0004] Linear low-density polyethylene may be, for example, comprising structural moieties derived from ethylene and structural moieties derived from α-olefins containing 4 to 10 carbon atoms, having a strength of ≥870 and ≤920 kg / m³ as determined by ASTM D792 (2013). 3 The polyethylene has a density of ≥880 and ≤915 kg / m³. 3 More preferably ≥890 and ≤910 kg / m 3 The density.

[0005] LLDPE can, for example, have a melt mass flow rate (MFR2) of ≥4.00 and ≤8.00 g / 10 min, preferably ≥4.50 and ≤7.50 g / 10 min, more preferably ≥5.00 and ≤7.50 g / 10 min, and even more preferably ≥5.00 and ≤7.00 g / 10 min, as determined according to ASTM D1238 (2013) at 190°C and a load of 2.16 kg. Such LLDPE allows for the manufacture of films with appropriate melt stability and processability.

[0006] In the application of polyethylene film in packaging, a specific aspect involves the sealing of such packaging.

[0007] In commercial use, polyethylene film can be used, for example, for packaging products such as food, where the package is filled with the desired product and sealed by contacting two layers of film, such as a film obtained by extrusion from a cast film, and applying heat to at least a portion of the areas where the films are in contact. The applied heat causes localized softening of the polyethylene materials in the two contacting layers. This results in adhesion between the two layers and, upon cooling, a closure seal, thus forming a package that contains the desired contents and is isolated from the surrounding atmosphere.

[0008] This type of packaging is familiar in everyday use and allows for a significant increase in, for example, the preservation of the contained product.

[0009] In this type of packaging solution, the seal produced using the heat-sealing technology described above needs to have a certain strength. This is necessary to create packaging that can withstand a certain amount of force (forces that the packaging should be considered capable of withstanding) during production, transportation, and consumer use. Therefore, the seal strength should be above a certain threshold.

[0010] Furthermore, given the efficiency of the packaging process and the energy consumption involved, it is important to achieve a seal with the desired high strength at a low desired sealing temperature. The lower the temperature at which the seal is formed, the less energy is required. Another benefit of a lower required temperature for seal formation is that the contents of the package are subjected to less heat, which is beneficial for maintaining the quality of the packaged contents, for example, in the case of food packaging.

[0011] Another important property of this type of packaging solution based on polyethylene materials is the so-called heat-adhesive strength. In the context of this invention, heat-adhesive strength should be understood as the strength of a seal formed by heat sealing in a polyethylene film immediately after sealing and before the seal cools. Heat-adhesive strength affects the efficiency of packaging processes using polyethylene film materials, such as the speed at which a packaging line can operate. Higher heat-adhesive strength results in a shorter cooling time required after seal formation and before further packaging processing; that is, the earlier the seal possesses this level of strength to withstand applied forces without damage, the shorter the cycle time in, for example, a continuous packaging machine.

[0012] For these reasons, the packaging industry continues to require polyethylene films that exhibit temperature reductions that produce a seal with a defined strength, particularly high thermal adhesive strength.

[0013] This membrane, according to the present invention, is provided as a membrane comprising at least one sealing layer, wherein at least one layer A of the sealing layer comprises polyethylene containing a structural portion derived from ethylene and a structural portion derived from an α-olefin comprising 4 to 10 carbon atoms, the polyethylene having a strength of ≥870 and ≤920 kg / m³ as determined according to ASTM D792 (2013). 3 density,

[0014] Polyethylene has the following characteristics:

[0015] • Material fraction eluted at a temperature of ≤30.0°C in analytical temperature rise elution fractionation (a-TREF) of ≤14.0% by weight relative to the total weight of polyethylene, preferably ≥5.0% by weight and ≤14.0% by weight, more preferably ≥5.0% by weight and ≤12.5% ​​by weight;

[0016] • The shear storage modulus G', G' and G” <500Pa, measured at 190℃, is determined according to ISO 6721-10 (2015) under the condition that the shear loss modulus G” = 5000Pa.

[0017] • Melt mass flow rate ≥4.00 and ≤8.00 g / 10 min, determined according to ASTM D1238 (2013) at 190°C and 2.16 kg load; and

[0018] • Chemical composition distribution width (CCDB) ≥10.0, preferably ≥15.0

[0019] CCDB is determined according to formula I:

[0020]

[0021] in

[0022] ·T n-2 The moment is calculated according to Equation II:

[0023]

[0024] and

[0025] ·T z+2 The moment is calculated according to Equation III:

[0026]

[0027] in

[0028] • w(i) is the sample weight fraction relative to the total sample weight in the a-TREF analysis of sample (i) taken at temperature T(i), expressed as % by weight. Where T(i) > 30℃, the area under the a-TREF curve is normalized to a surface area of ​​1 for T(i) > 30℃; and

[0029] •T(i) is the temperature at which sample (i) is taken in the a-TREF analysis, in °C.

[0030] This type of membrane allows for sealing at reduced temperatures while still providing the desired sealing strength and the desired thermal adhesion strength.

[0031] The polyethylene used in layer A of the membrane according to the invention has a strength of ≥870 and ≤920 kg / m³. 3 Preferred weight is ≥880 and ≤915 kg / m³. 3 More preferably ≥890 and ≤910 kg / m 3 Even more preferred is ≥895 and ≤905 kg / m 3The density of polyethylene. Using polyethylene with this density in layer A of the membrane according to the invention helps to improve the seal.

[0032] Preferably, the polyethylene used in layer A of the membrane according to the invention has a material fraction of ≥86.0% by weight and ≤90.0% by weight relative to the total weight of polyethylene, eluted in α-TREF at a temperature of ≥30.0°C and ≤90.0°C. Preferably, the polyethylene used in layer A of the membrane according to the invention has a material fraction of ≥0.5% by weight and ≤1.0% by weight relative to the total weight of polyethylene, eluted in α-TREF at a temperature of ≥90.0°C. Using such polyethylene in layer A of the membrane according to the invention helps to reduce the sealing initiation temperature.

[0033] The polyethylene used in layer A of the membrane according to the invention has a shear storage modulus G' of ≤500 Pa, preferably ≥300 and ≤500 Pa, more preferably ≥400 Pa and ≤500 Pa, as measured at a shear loss modulus G” = 5000 Pa. Using polyethylene with such a shear storage modulus G' at a shear loss modulus of 5000 Pa in layer A of the membrane according to the invention helps to improve the processability of the membrane.

[0034] According to the present invention, analytical temperature rise elution fractionation (also known as α-TREF) can be performed using a Polymer Char Crystaf-TREF 300 equipped with a stainless steel column with a length of 15 cm and an inner diameter of 7.8 mm, using a solution containing 4 mg / ml of sample prepared in 1,2-dichlorobenzene, stabilized at 150 °C for 1 hour with 1 g / L Topanol CA (1,1,3-tris(3-tert-butyl-4-hydroxy-6-methylphenyl)butane) and 1 g / L Irgafos 168 (tris(2,4-di-tert-butylphenyl)phosphite). The solution can be further stabilized for 45 minutes with continuous stirring at 200 rpm at 95 °C before analysis. For analysis, the solution is crystallized from 95 °C to 30 °C using a cooling rate of 0.1 °C / min. Elution can be performed from 30 °C to 140 °C using a heating rate of 1 °C / min. The apparatus can be cleaned at 150 °C. The injection volume can be 300 μl, and the pump flow rate during elution is 0.5 ml / min. The volume between the column and the detector can be 313 μl. In the context of this invention, the fraction eluted at temperatures ≤30.0 °C can be calculated by subtracting the sum of the fractions eluted at >30.0 °C from 100%, thus the total fractions eluted at ≤30.0 °C and >30.0 °C reach 100.0% by weight.

[0035] Specifically, α-TREF can be performed using a Polymer Char Crystaf-TREF 300 with a solution containing 4 mg / ml of polymer in 1,2-dichlorobenzene. The solution is stabilized at 150°C for 1 hour with 1 g / L 1,1,3-tris(3-tert-butyl-4-hydroxy-6-methylphenyl)butane and 1 g / L tris(2,4-di-tert-butylphenyl)phosphite, and then stabilized for an additional 45 minutes at 95°C with continuous stirring at 200 rpm. The solution is then crystallized from 95°C to 30°C at a cooling rate of 0.1°C / min before analysis, and eluted from 30°C to 140°C at a heating rate of 1°C / min. The equipment has been cleaned at 150°C.

[0036] For the determination of shear storage modulus G' and shear loss modulus G”, a sample prepared according to ISO 17855-2 (2016) can be used. DMS measurements are performed at 190 °C according to ISO 6721-10 (2015). The determination of G' at G” = 5000 Pa can be performed by preparing a double log-log Cole-Cole plot of G' and G”, where two data points are selected for values ​​greater than and less than G” = 5000 Pa, for a total of four data points, and a first-order line can be determined from which G' at G” = 5000 Pa is determined.

[0037] The polyethylene used in layer A of the membrane according to the invention has a CCDB of ≥10.0, preferably ≥15.0, more preferably ≥16.0. For example, the polyethylene has a CCDB of ≥15.0 and ≤30.0, preferably ≥16.0 and ≤25.0, more preferably ≥16.0 and ≤20.0. Using polyethylene with such a CCDB in layer A of the membrane according to the invention helps to improve the sealing strength.

[0038] The polyethylene used in layer A of the membrane according to the invention has a melt mass flow rate (MFR2) of ≥4.00 and ≤8.00 g / 10 min, preferably ≥4.50 and ≤7.50 g / 10 min, more preferably ≥5.00 and ≤7.50 g / 10 min, and even more preferably ≥5.00 and ≤7.00 g / 10 min, as determined according to ASTM D1238 (2013) at 190°C and a load of 2.16 kg. Such polyethylene allows for the manufacture of membranes with suitable melt stability and processability.

[0039] Preferably, the polyethylene comprises ≥70.0% by weight, more preferably ≥75.0% by weight, and more preferably ≥80.0% by weight of ethylene-derived structural portions relative to the total weight of the polyethylene. More preferably, the polyethylene comprises ≥70.0% and ≤98.0% by weight, more preferably ≥75.0% and ≤95.0% by weight, and even more preferably ≥80.0% and ≤90.0% by weight of ethylene-derived structural portions relative to the total weight of the polyethylene.

[0040] More preferably, the polyethylene comprises ≤30.0% by weight, preferably ≤25.0% by weight, and more preferably ≤20.0% by weight, of a structural portion derived from an α-olefin comprising 4-10 carbon atoms, relative to the total weight of the polyethylene. The polyethylene may, for example, comprise ≥5.0% by weight, preferably ≥10.0% by weight, and more preferably ≥15.0% by weight, of a structural portion derived from an α-olefin comprising 4-10 carbon atoms, relative to the total weight of the polyethylene. For example, the polyethylene may comprise ≥5.0% and ≤30.0% by weight, preferably ≥10.0% by weight and ≤25.0% by weight, and more preferably ≥15.0% and ≤20.0% by weight, of a structural portion derived from an α-olefin comprising 4-10 carbon atoms, relative to the total weight of the polyethylene.

[0041] The α-olefin may contain 4-10 carbon atoms, for example selected from 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene, such as those selected from 1-butene, 1-hexene, and 1-octene. For example, the α-olefin containing 4-10 carbon atoms may be selected from 1-hexene and 1-octene. The structural moiety derived from the α-olefin containing 4-10 carbon atoms may be, for example, a structural moiety derived from 1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene, or combinations thereof, preferably a structural moiety derived from 1-hexene or 1-octene.

[0042] The polyethylene used in layer A of the membrane according to the invention may, for example, comprise ≤30.0 wt%, preferably ≤25.0 wt%, more preferably ≤20.0 wt% of a structural portion derived from an α-olefin comprising 4-10 carbon atoms relative to the total weight of the polyethylene, wherein the α-olefin comprising 4-10 carbon atoms is selected from 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene, such as those selected from 1-butene, 1-hexene, and 1-octene. The polyethylene may, for example, comprise ≥5.0 wt%, preferably ≥10.0 wt%, more preferably ≥15.0 wt% of a structural portion derived from an α-olefin comprising 4-10 carbon atoms relative to the total weight of the polyethylene, wherein the α-olefin comprising 4-10 carbon atoms is selected from 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene, such as those selected from 1-butene, 1-hexene, and 1-octene. For example, polyethylene may contain ≥5.0 and ≤30.0% by weight, preferably ≥10.0% by weight and ≤25.0% by weight, more preferably ≥15.0% by weight and ≤20.0% by weight, relative to the total weight of polyethylene, a structural moiety derived from an α-olefin comprising 4-10 carbon atoms, wherein the α-olefin comprising 4-10 carbon atoms is selected from 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene, such as those selected from 1-butene, 1-hexene, and 1-octene.

[0043] Layer A of the membrane according to the invention may, for example, comprise >10.0 wt%, or >20.0 wt%, or >30.0 wt%, or >40.0 wt%, or >50.0 wt%, or >60.0 wt%, or >70.0 wt%, or >80.0 wt%, or >90.0 wt% of polyethylene relative to the total weight of the membrane. Alternatively, the membrane may be composed of polyethylene or primarily composed of polyethylene.

[0044] In the context of this invention, embodiments in which layer A of the membrane is primarily composed of polyethylene should be understood to consist of polyethylene and additives known in the field of polyethylene films, such as additives accounting for up to 1.0% by weight relative to the total weight of the membrane. Suitable additives may include, for example, UV stabilizers, antioxidants, and processing aids.

[0045] Layer A of the membrane according to the invention may, for example, comprise <90.0% by weight, or <80.0% by weight, or <70.0% by weight, or <60.0% by weight, or <50.0% by weight, or <40.0% by weight, or <30.0% by weight, or <20.0% by weight relative to the total weight of the membrane. Layer A of the membrane may comprise, for example, >20.0% and <50.0% by weight, or >40.0% by weight and <70.0% by weight, or >60.0% by weight and <90.0% by weight, or >70.0% and <90.0% by weight of polyethylene.

[0046] Layer A may have a thickness of, for example, 1-100 μm, preferably 5-75 μm, more preferably 10-50 μm, and even more preferably 20-40 μm.

[0047] In one embodiment, the membrane consists of layer A.

[0048] Polyethylene can be produced, for example, by solution polymerization, preferably by polymerization of ethylene with 1-hexene and / or 1-octene. Polyethylene can also be produced, for example, using a metallocene catalyst, preferably by polymerization of ethylene with 1-hexene and / or 1-octene.

[0049] In some embodiments, the present invention also relates to certain multilayer membrane structures comprising the membrane according to the invention. For example, the present invention also relates to a multilayer membrane structure comprising the membrane according to the invention, wherein the membrane is arranged in an arrangement of the multilayer membrane structure such that at least one of the outer surfaces of the multilayer membrane structure is composed of layer A. Alternatively, the present invention also relates to a multilayer membrane structure comprising the membrane according to the invention, wherein the membrane is arranged in an arrangement of the multilayer membrane structure such that both outer surfaces of the multilayer membrane structure are composed of layer A.

[0050] In another embodiment, the present invention relates to a multilayer film structure comprising two outer layers and at least one inner layer located between the two outer layers, wherein one of the outer layers is composed of layer A, or wherein each of the two outer layers is composed of layer A.

[0051] The multilayer membrane structure may include, for example, 3-15 layers, preferably 3-11 layers, more preferably 3-7 layers. The multilayer membrane structure may include, for example, 3 layers, 5 layers, or 7 layers.

[0052] The multilayer film structure may have a thickness of, for example, 2-150 μm, preferably 20-100 μm, more preferably 25-75 μm.

[0053] In a specific embodiment, the present invention also relates to a method for preparing an article comprising a sealing film, the method comprising the following steps in sequence:

[0054] • Provides a membrane or multilayer membrane structure according to the present invention;

[0055] • Provide objects including surfaces for sealing with membrane or multilayer membrane structures;

[0056] • Arrange membrane or multilayer membrane structures and objects such that layer A of the membrane or multilayer membrane structure and the sealing surface of the object can contact each other;

[0057] • At a temperature ≥60 and ≤80°C, when applying ≥0.3 N / mm 2 Under pressure, the membrane is brought into contact with the surface used for sealing within 1-5 seconds.

[0058] To obtain heat-sealed products.

[0059] The present invention also relates to an article comprising a membrane sealed to a surface, wherein the article comprises a membrane or multilayer membrane structure according to the invention, or wherein the article is manufactured according to a method according to the invention. For example, such an article may be packaging for containing food, or packaging containing food.

[0060] The present invention further relates to the use of the film according to the invention or the multilayer film structure according to the invention for reducing the sealing temperature of packaging.

[0061] The present invention will now be described through the following non-limiting embodiments.

[0062] The following polyethylene material was used in the experiments conducted during this invention.

[0063]

[0064] Analysis of these materials revealed the following product properties:

[0065] PE1 PE2 MFR2 (g / 10min) 6.0 6.0 <![CDATA[Density (kg / m 3 )]]> 900 900 G'(Pa) at G” = 5000Pa 490 524 <30℃ α-TREF fraction (wt%) 10.7 14.0 CCDB(-) 16.5 15.3 PSP1 19.34 16.10

[0066] Using these materials, films are produced via cast film extrusion using a single-screw extruder with a screw diameter of 40 mm. The films are produced at a die temperature of 220°C. The films have a thickness of 40 μm and a width of 350 mm.

[0067] The membranes produced using each of PE 1 to 2 according to the above method underwent the analysis and testing described below.

[0068] membrane F1 F2 Polyethylene type PE1 PE2 SIT (°C) with heat adhesion at 0.4N 78.6 82.5 At 75°C, thermal adhesion strength 0.24 0.16 At 80℃, thermal adhesion strength 0.46 0.27 At 85℃, thermal adhesion strength 0.59 0.52 SIT (°C) at 0.4N heat seal 86.8 93.2 At 86℃, sealing strength 335 30 At 90℃, sealing strength 576 89 At 94℃, sealing strength 787 551

[0069] in:

[0070] • The thermal tack strength at a given temperature is the thermal tack strength of a 25 mm wide seal, as determined according to ASTM F1921 (2012) for seals produced at given temperatures of 75°C, 80°C and 85°C, and is expressed in N / cm.

[0071] • The seal strength at a given temperature is measured for a 25 mm wide seal, according to ASTM F88 (2015), for seals produced at given temperatures of 86 °C, 90 °C, and 94 °C, and is expressed in g.

[0072] • The SIT (sealing initiation temperature) of thermal adhesion at 0.4N is the temperature at which a thermal adhesion strength of 0.4N is achieved, in °C, where the thermal adhesion strength is determined according to the above measurements.

[0073] • The SIT at which a heat seal of 0.4N is achieved is the temperature at which a sealing strength of 0.4N is achieved, in °C, where the sealing strength is determined according to the above measurements.

[0074] As can be observed from the above results, the membrane of the present invention, as reflected by F1, allows for the production of a seal with a certain strength by heat sealing at particularly low sealing temperatures.

Claims

1. A membrane comprising at least one sealing layer, wherein at least one layer A of the sealing layer comprises polyethylene containing a structural portion derived from ethylene and a structural portion derived from an α-olefin comprising 4 to 10 carbon atoms, said polyethylene having a strength ≥ 870 and ≤ 920 kg / m³ as determined according to ASTM D792 (2013). 3 density, The polyethylene thereon has: The material fraction eluted at a temperature ≤ 30.0°C in the analytical temperature rise elution fraction is ≤ 14.0% by weight relative to the total weight of the polyethylene. The shear storage modulus G' < 500 Pa was determined at a shear loss modulus G'' = 5000 Pa. G' and G'' were determined at 190 °C according to ISO 6721-10 (2015). The melt mass flow rate is ≥ 4.50 and ≤ 8.00 g / 10 min, as determined by ASTM D1238 (2013) at 190°C and 2.16 kg load. Chemical composition distribution width ≥ 10.0 The chemical composition distribution width is determined according to Formula I: Formula I in T n-2 The moment is calculated according to Equation II: Formula II and T z+2 The moment is calculated according to Equation III: Formula III in w(i) is the fraction of sample (i) taken at temperature T(i) relative to the total sample weight in the temperature rise elution fractionation analysis, expressed as % by weight. For T(i) > 30℃, the area under the temperature rise elution fractionation curve is normalized to a surface area of ​​1 for T(i) > 30℃. T(i) is the temperature at which sample (i) is taken in the temperature rise elution fractionation analysis, in °C.

2. The membrane according to claim 1, wherein the polyethylene has a material fraction eluted at a temperature of ≤ 30.0°C in an analytical temperature rise elution fraction, comprising ≥ 5.0% by weight and ≤ 14.0% by weight relative to the total weight of the polyethylene.

3. The membrane according to claim 1, wherein the polyethylene has a material fraction eluted at a temperature ≤ 30.0°C in an analytical temperature rise elution fraction, comprising ≥ 5.0% by weight and ≤ 12.5% ​​by weight relative to the total weight of the polyethylene.

4. The membrane according to claim 1, wherein the polyethylene has a chemical composition distribution width of ≥ 15.

0.

5. The membrane according to claim 1, wherein the polyethylene has a principal structural parameter 1 of ≥ 17.0, i.e., PSP1, wherein PSP1 is determined according to Formula IV: Formula IV in M i The molecular weight of fraction i is determined by SEC-IR analysis; W i It has the molecular weight M i The weight fraction; and SCB i It is in the presence of the molecular weight M i The number of short chain branches per 1000 carbon atoms in the fraction.

6. The membrane according to claim 1, wherein the polyethylene has a PSP1 of ≥ 18.

0.

7. The membrane according to claim 1, wherein the polyethylene has a PSP1 of ≥ 19.

0.

8. The membrane according to any one of claims 1-7, wherein the polyethylene comprises: Material fractions eluted at temperatures ≥ 30.0°C and ≤ 90.0°C in analytical temperature rise elution fractionation, comprising ≥ 86.0% by weight and ≤ 90.0% by weight relative to the total weight of the polyethylene; and / or Material fractions eluted at temperatures ≥ 90.0°C in analytical temperature rise elution fractionation, comprising ≥ 0.5% by weight and ≤ 1.0% by weight relative to the total weight of the polyethylene.

9. The membrane according to any one of claims 1-7, wherein the polyethylene comprises ≥ 70.0% by weight of ethylene-derived structural portions relative to the total weight of the polyethylene.

10. The membrane according to any one of claims 1-7, wherein the polyethylene comprises ≤ 30.0% by weight of a structural portion derived from an α-olefin comprising 4 to 10 carbon atoms relative to the total weight of the polyethylene.

11. The membrane according to claim 10, wherein the α-olefin comprising 4 to 10 carbon atoms is selected from 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene.

12. The membrane according to any one of claims 1-7, wherein the layer A comprises > 50.0% by weight of the polyethylene relative to the total weight of the layer A.

13. The membrane according to any one of claims 1-7, wherein the polyethylene is produced by solution polymerization, and / or wherein the polyethylene is produced using a metallocene catalyst.

14. The membrane according to any one of claims 1-7, wherein layer A has a thickness of 1-100 μm.

15. The membrane according to any one of claims 1-7, wherein the membrane comprises layer A.

16. A multilayer membrane structure comprising the membrane according to any one of claims 1-15, wherein the membrane is arranged in the multilayer membrane structure such that at least one of the outer surfaces of the multilayer membrane structure is composed of layer A.

17. The multilayer membrane structure according to claim 16, wherein the structure comprises 3-15 layers.

18. The multilayer membrane structure according to claim 16 or 17, comprising two outer layers and at least one inner layer located between the two outer layers, wherein one of the outer layers is composed of layer A, or wherein each of the two outer layers is composed of layer A.

19. The multilayer film structure according to claim 16 or 17, wherein the structure has a thickness of 2-150 μm.

20. A method for preparing an article comprising a sealing film, the method comprising steps in the following order: Provide a membrane according to any one of claims 1-15 or a multilayer membrane structure according to any one of claims 16-19; Provide an object comprising a surface sealed with a membrane according to any one of claims 1-15 or a multilayer membrane structure according to any one of claims 16-19; The membrane or multilayer membrane structure and the object are arranged such that layer A of the membrane or multilayer membrane structure and the sealing surface of the object can contact each other; At temperatures ≥ 60 and ≤ 80 °C, when applying ≥ 0.3 N / mm 2 Under pressure, the membrane and the sealing surface are brought into contact within 1-5 seconds. To obtain heat-sealed products.

21. An article comprising a membrane sealed to a surface, wherein the article comprises a membrane according to any one of claims 1-15, a multilayer membrane structure according to any one of claims 16-19, or wherein the article is manufactured according to claim 20.

22. The article of claim 21, wherein the article of claim 21 is packaging for containing food.

23. Use of the film according to any one of claims 1-15 or the multilayer film structure according to any one of claims 16-19 for reducing the sealing temperature of packaging.

Citation Information

Patent Citations

  • Multilayered film

    JP2012035630A

  • Polyethylene film for heat sealing.

    WO2020064349A1