Double-layer liquid crystal film and preparation method thereof

By introducing epoxy liquid crystals and chiral dopants into polyacrylate films, combined with ultraviolet cross-linking technology, the durability and adhesion of the film are solved, and the double-reflection band and composite color are realized. Film preparation improves the durability and optical properties of the film.

CN116656204BActive Publication Date: 2024-11-22SUZHOU SUKAI ROAD CHEM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310413979.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-11-22
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Polyacrylate films have poor processing performance and poor cold resistance, and are not resistant to water, water vapor, acid and alkali, salt solutions and organic polar solvents. The elasticity and wear resistance at room temperature are also poor, resulting in the adhesion of the preparation of the double-layer film. Poor.

Method used

Using a preparation method of a double-layer liquid crystal film, the mixed solution includes epoxy liquid crystal molecules, acrylic liquid crystal molecules, chiral dopants, photoinitiators and free radical photoinitiators, and the ultraviolet cross-linking polymerization technology is used to form A double-layer liquid crystal film with double reflection band and composite color adjusts the chiral dopant ratio to adjust the position of the reflection band, improves the polymerization rate and reduces haze.

Benefits of technology

Through one coating and two photocrosslinking polymerization, a double-layer liquid crystal film with double reflection band and composite color is achieved, which improves the durability and optical transparency of the film, enables the preparation of patterned films, and obtains a wider Reflection band.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116656204B_ABST
    Figure CN116656204B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of liquid crystals, and specifically relates to a double-layer liquid crystal film and a preparation method thereof. The present invention utilizes acrylate liquid crystals and epoxy liquid crystals and uses chiral dopants with different terminal groups, adds free radical photoinitiators and cationic photoinitiators, and prepares a double-layer liquid crystal film separated by an acrylate system and an epoxy liquid crystal system by one coating and two photocrosslinking polymerizations, utilizing polymerization-induced phase separation and the polymerization rate difference of two reactive terminal group mixtures, and obtains a double-layer liquid crystal film with double reflection bands and composite colors, and the relative positions of the two reflection bands can be adjusted by adjusting the relative content and overall content of the two chiral dopants, thereby obtaining a double-layer film with band-tunable composite structural colors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of liquid crystals, and in particular relates to a double-layer liquid crystal film and a preparation method thereof. Background Art

[0002] The helical structure of cholesteric liquid crystal (CLC) can produce selective Bragg reflection. The wavelength of the Bragg reflection band (λ) depends on the length of the helical pitch (P) and the average refractive index (n) of the material. Since CLC can be adjusted by changing the concentration of chiral additives and external conditions, CLC has become a hot research area for polycarbonate (PC) materials. So far, various polymer-stabilized CLC (PSCLC) films have been prepared based on acrylates, which can be used for filters and gratings. However, free radical polymerization is inhibited by oxygen. Therefore, polyacrylate films are usually prepared in cells or under N2. Epoxy resin liquid crystals themselves have the advantages of good adhesion, high cross-linking density and low volume shrinkage, and are not affected by oxygen inhibition. Doping chiral dopants into nematic epoxy liquid crystals to induce the formation of cholesteric liquid crystals can well solve the shortcomings of acrylate liquid crystals.

[0003] Reactive liquid crystals self-assemble under certain external conditions to form a specific structure and then UV-cured to obtain a liquid crystal polymer film. Compared with ordinary polymer materials, this liquid crystal polymer not only fixes the optical properties and orderliness of the liquid crystal molecules themselves, but also has the advantages of polymers, including mechanical properties, dimensional stability, heat resistance and low thermal expansion coefficient. It is also possible to obtain a system with specific functions by doping other functional components, so that the liquid crystal polymer has different properties. Therefore, liquid crystal polymers are widely used in sensors, laser protection, photochromism, photoisomerism and liquid crystal displays. Double-layer liquid crystal films can be obtained by adjusting the proportion of the components and the preparation conditions to obtain liquid crystal films with wide reflection bands. Summary of the invention

[0004] The problems existing in the prior art are that the polyacrylate film has poor processing performance, slow flow rate, poor cold resistance, is not resistant to water, water vapor, acid and alkali, salt solution and organic polar solvents, has poor elasticity and wear resistance at room temperature, and has poor electrical properties. Since the epoxy layer in the prepared double-layer film is on the upper layer, the adhesion of the prepared film is poor.

[0005] In order to solve the above-mentioned technical problems, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a double-layer liquid crystal film, comprising the following steps:

[0007] S11: preparing a mixed solution, heating it at 90-120° C. for volatilization, and then irradiating it with a high-pressure mercury lamp for 10-20 seconds to obtain a polymer film material;

[0008] The solute of the mixed solution includes epoxy liquid crystal molecules, acrylic liquid crystal molecules, chiral dopants, photoinitiators, photoinitiator aids and free radical photoinitiators;

[0009] The epoxy liquid crystal molecules are selected from one or more of liquid crystal compound 1, liquid crystal compound 2, liquid crystal compound 3 and liquid crystal compound 4;

[0010] The general structural formula of the liquid crystal compound 1 is as follows:

[0011]

[0012] The general structural formula of the liquid crystal compound 2 is as follows:

[0013]

[0014] The general structural formula of the liquid crystal compound 3 is as follows:

[0015]

[0016] The general structural formula of the liquid crystal compound 4 is as follows:

[0017]

[0018] Wherein R is COOCH2CH3, OCH3 or COOCH3;

[0019] In the liquid crystal compound 1, the liquid crystal compound 2, the liquid crystal compound 3 and the liquid crystal compound 4, m=4-8; A represents the central group of the liquid crystal compound 1 or the liquid crystal compound 2, and the general structural formula thereof is shown in Formula I:

[0020]

[0021] Wherein, R1 is H, Cl, F, CH3, CH2CH3, OCH3 or COOCH3;

[0022] The general structural formula of the acrylic liquid crystal molecule is as follows:

[0023]

[0024] In the acrylic liquid crystal molecule, t=4-8, B represents the central group of the acrylic liquid crystal molecule, and its general structural formula is shown in Formula II:

[0025]

[0026] Wherein, R2 is H, Cl, F, CH3, CH2CH3, OCH3 or COOCH3;

[0027] S12: Under the condition of 80-130° C., the polymer film material is irradiated with 365 nm ultraviolet light (LED lamp) to obtain the double-layer liquid crystal film.

[0028] Preferably, the chiral dopant is selected from any two of chiral dopant 1, chiral dopant 2, chiral dopant 3 and chiral dopant 4;

[0029] The general structural formula of the chiral dopant 1 is as follows:

[0030] Among them, p = 4-8;

[0031] The general structural formula of the chiral dopant 2 is as follows:

[0032]

[0033] Wherein, x=4-8;

[0034] The general structural formula of the chiral dopant 3 is as follows:

[0035] Wherein, n = 3-12;

[0036] The general structural formula of the chiral dopant 4 is as follows:

[0037] Wherein, q = 3-12;

[0038] In the chiral dopant, M represents a group of the chiral center of the chiral dopant, and its general structural formula is shown in Formula III, Formula IV, Formula V or Formula VI:

[0039]

[0040] Preferably, in the solute of the mixed solution, the mass fraction of chiral dopant 1, chiral dopant 2, chiral dopant 3 or chiral dopant 4 is not higher than 4.5%.

[0041] Preferably, in the solute of the mixed solution, the mass ratio of epoxy liquid crystal molecules to acrylic liquid crystal molecules is 27-54:36-63.

[0042] Preferably, in the solute of the mixed solution, the mass ratio of epoxy liquid crystal molecules, photoinitiator, photoinitiator auxiliary and free radical photoinitiator is 27-54:2.7-5.4:1-2:1.8-3.2.

[0043] Preferably, the photoinitiator is a triarylsulfonium salt.

[0044] Preferably, the photoinitiator auxiliary is 2-isopropylthioxanthone (ITX) or 2-hydroxy-2-methyl-1-phenyl-1-propanone, and its structural formula is as follows:

[0045]

[0046] Preferably, the free radical photoinitiator is 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, and its structural formula is as follows:

[0047]

[0048] Preferably, the solvent of the mixed solution is cyclopentanone and cyclohexanone.

[0049] Furthermore, the mass ratio of cyclopentanone to cyclohexanone is 4:1.

[0050] Preferably, the solvent of the mixed solution is cyclohexanone and ethyl acetate.

[0051] Furthermore, the mass ratio of cyclohexanone to ethyl acetate is 4:1.

[0052] Preferably, the solid content of the mixed solution is 5-40wt%.

[0053] Preferably, the solute of the mixed solution further includes a leveling agent (EFKA-3600 leveling agent).

[0054] Furthermore, the mass ratio of the epoxy liquid crystal molecules to the leveling agent is 27-54:0.1-0.2.

[0055] The present invention also provides a double-layer liquid crystal film prepared by the above preparation method.

[0056] The technical solution of the present invention has the following advantages over the prior art:

[0057] 1. The present invention uses one coating and two photo-crosslinking polymerizations to prepare a double-layer liquid crystal film separated by an acrylate system and an epoxy liquid crystal system by utilizing polymerization-induced phase separation and the difference in polymerization rates of two reactive end group mixtures, thereby obtaining a double-layer liquid crystal film with double reflection bands and composite colors.

[0058] 2. By adjusting the relative content and overall content of the two chiral dopants, the relative positions of the two reflection bands are adjusted, thereby obtaining a double-layer film with a band-tunable composite structural color and a double-layer film with a wider reflection band.

[0059] 3. Photoinitiator additives are introduced into the system to increase the polymerization rate and reduce the haze.

[0060] 4. The double reflection band characteristics of the double-layer film can be used to prepare patterning. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 is a schematic diagram of preparing a double-layer film 1.

[0062] Figure 2 These are FESEM images of double-layer films prepared at different ratios of liquid crystal and chiral dopant.

[0063] Figure 3 is a photograph of the prepared double-layer film.

[0064] Figure 4 is the UV-visible spectrum of the prepared double-layer film.

[0065] Figure 5 It is the UV-visible spectrum of a double-layer film with a wider reflection band prepared by changing the ratio of liquid crystal and chiral dopant.

[0066] Figure 6 is a photograph of the prepared patterned film. DETAILED DESCRIPTION

[0067] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0068] Example 1

[0069] A material 1 comprising the following structure is prepared:

[0070]

[0071]

[0072] Epoxy liquid crystal molecules 1 (45 wt%), acrylic liquid crystal molecules 1 (45 wt%), chiral dopant A (0.9 wt%), chiral dopant B (3.6 wt%), photoinitiator (2.7 wt%) (triarylsulfonium salt), photoinitiator auxiliary X (1 wt%) (ITX), free radical photoinitiator (1.8 wt%) and leveling agent 3600 (0.1 wt%) were weighed and dissolved in a solvent with a mixing ratio of 4:1 of cyclopentanone and cyclohexanone, and the solvent volatilization rate was controlled by blending in different proportions to prepare a mixed solution with a solid content of 20 wt%. The solution was coated on a flexible PET base film by a wire rod, the solvent was volatilized at 105°C, irradiated under a high-pressure mercury lamp, and then placed on a hot stage at 110°C and irradiated with a 365 nm ultraviolet lamp to obtain a stable double-layer liquid crystal polymer film.

[0073] By mixing chiral dopants of different mass ratios using the above method, liquid crystal materials of different composite colors can be obtained. And the relative positions of the two reflection bands can be adjusted by adjusting the relative ratio of the two chiral dopants. The prepared film photos and UV-visible spectra are shown in Figure 1 and Figure 2 As shown, Figure 3 This is a photo of a patterned film prepared using a double-layer film.

[0074] Example 2

[0075] A material 2 comprising the following structure is prepared:

[0076]

[0077]

[0078] Epoxy liquid crystal molecules 2 (27 wt%), epoxy liquid crystal molecules 3 (18 wt%), acrylic liquid crystal molecules 2 (45 wt%), chiral dopant A (2.0 wt%), chiral dopant B (2.5 wt%), photoinitiator (2.7 wt%) (triarylsulfonium salt), photoinitiator auxiliary X (1 wt%) (ITX), free radical photoinitiator (1.8 wt%) and leveling agent 3600 (0.1 wt%) were weighed and dissolved in a solvent with a mixing ratio of 4:1 of cyclopentanone and cyclohexanone, and the solvent volatilization rate was controlled by blending in different proportions to prepare a mixed solution with a solid content of 20 wt%. The solution was coated on a flexible PET base film by a wire rod, the solvent was volatilized at 120°C, irradiated under a high-pressure mercury lamp, and then placed on a hot stage at 110°C and irradiated with a 365 nm ultraviolet lamp to obtain a stable double-layer liquid crystal polymer film.

[0079] Example 3

[0080] A material 3 comprising the following structure is prepared:

[0081]

[0082] Epoxy liquid crystal molecules 1 (45 wt%) and acrylic liquid crystal molecules 1 (45 wt%), chiral dopant A (3.6 wt%), chiral dopant C (0.9 wt%), photoinitiator (2.7 wt%) (triarylsulfonium salt), photoinitiator auxiliary X (1 wt%) (ITX), free radical photoinitiator (1.8 wt%) and leveling agent 3600 (0.1 wt%) were weighed and dissolved in a solvent with a mixing ratio of 4:1 of cyclopentanone and cyclohexanone, and the solvent volatilization rate was controlled by blending in different proportions to prepare a mixed solution with a solid content of 20 wt%. The solution was coated on a flexible PET base film by a wire rod, the solvent was volatilized at 120°C, irradiated under a high-pressure mercury lamp, and then placed on a hot stage at 110°C and irradiated with a 365 nm ultraviolet lamp to obtain a stable double-layer liquid crystal polymer film.

[0083] Example 4

[0084] A material 4 comprising the following structure was prepared:

[0085]

[0086] Epoxy liquid crystal molecules 1 (45 wt%) and acrylic liquid crystal molecules 2 (45 wt%), chiral dopant A (0.9 wt%), chiral dopant B (3.6 wt%), photoinitiator (2.7 wt%) (triarylsulfonium salt), photoinitiator auxiliary Y (1 wt%) (1173), free radical photoinitiator (1.8 wt%) and leveling agent 3600 (0.1 wt%) were weighed and dissolved in a solvent with a mixing ratio of 4:1 of cyclopentanone and cyclohexanone, and the solvent volatilization rate was controlled by blending in different proportions to prepare a mixed solution with a solid content of 20 wt%. The solution was coated on a flexible PET base film by a wire rod, the solvent was volatilized at 120°C, irradiated under a high-pressure mercury lamp, and then placed on a hot stage at 110°C and irradiated with a 365 nm ultraviolet lamp to obtain a stable double-layer liquid crystal polymer film.

[0087] Example 5

[0088] A material 5 comprising the following structure was prepared:

[0089]

[0090] Epoxy liquid crystal molecules 1A (45 wt%) and acrylic liquid crystal molecules 1 (45 wt%), chiral dopant A (1.5 wt%), chiral dopant E (3.0 wt%), photoinitiator (2.7 wt%) (triarylsulfonium salt), photoinitiator auxiliary X (1 wt%) (1173), free radical photoinitiator (1.8 wt%) and leveling agent 3600 (0.1 wt%) were weighed and dissolved in a solvent with a mixing ratio of cyclopentanone and cyclohexanone of 4:1, and the solvent volatilization rate was controlled by blending in different proportions to prepare a mixed solution with a solid content of 20 wt%. The solution was coated on a flexible PET base film by a wire rod, the solvent was volatilized at 120°C, irradiated under a high-pressure mercury lamp, and then placed on a hot stage at 120°C and irradiated with a 365 nm ultraviolet lamp to obtain a stable double-layer liquid crystal polymer film.

[0091] Example 6

[0092] A material 6 comprising the following structure was prepared:

[0093]

[0094]

[0095] Epoxy liquid crystal molecules 1A (45 wt%) and acrylic liquid crystal molecules 1 (45 wt%), chiral dopant A (1.5 wt%), chiral dopant B (3.0 wt%), photoinitiator (2.7 wt%) (triarylsulfonium salt), photoinitiator auxiliary X (1 wt%) (1173), free radical photoinitiator (1.8 wt%) and leveling agent 3600 (0.1 wt%) were weighed and dissolved in a solvent with a mixing ratio of 4:1 of cyclopentanone and cyclohexanone, and the solvent volatilization rate was controlled by blending in different proportions to prepare a mixed solution with a solid content of 20 wt%. The solution was coated on a flexible PET base film by a wire rod, the solvent was volatilized at 120°C, irradiated under a high-pressure mercury lamp, and then placed on a hot stage at 110°C and irradiated with a 365 nm ultraviolet lamp to obtain a stable double-layer liquid crystal polymer film.

[0096] Example 7

[0097] A material 7 comprising the following structure was prepared:

[0098]

[0099]

[0100] Epoxy liquid crystal molecules 2A (27 wt%), epoxy liquid crystal molecules 3A (18 wt%), acrylic liquid crystal molecules 3 (45 wt%), chiral dopant D (2.5 wt%), chiral dopant E (2 wt%), photoinitiator (2.7 wt%) (triarylsulfonium salt), photoinitiator auxiliary X (1 wt%) (1173), free radical photoinitiator (1.8 wt%) and leveling agent 3600 (0.1 wt%) were weighed and dissolved in a solvent with a mixing ratio of 4:1 of cyclopentanone and cyclohexanone, and the solvent volatilization rate was controlled by blending in different proportions to prepare a mixed solution with a solid content of 20 wt%. The solution was coated on a flexible PET base film by a wire rod, the solvent was volatilized at 100°C, irradiated under a high-pressure mercury lamp, and then placed on a hot stage at 100°C and irradiated with a 365 nm ultraviolet lamp to obtain a stable double-layer liquid crystal polymer film.

[0101] Effect evaluation

[0102] Figure 2 The FE-SEM images shown indicate that the prepared film is controllable in terms of the relative reflection wavelength and thickness of the upper and lower layers; Figure 3 Actual photos of double-layer films prepared with different ratios of chiral dopants show that the prepared films have good optical transparency and aesthetics. Figure 4 The tunability of the dual reflection bands of the prepared double-layer film is further demonstrated. Figure 5 The films prepared by adjusting the ratio of liquid crystal and chiral dopant show that a film with a wider spectrum can be obtained by adjusting the ratio; Figure 6 It is a patterned film prepared using a double-layer film.

[0103] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing a double-layer liquid crystal film, It is characterized in that The steps include: S11: heating the mixed solution at 90-120° C. for volatilization and then irradiating it with a high pressure mercury lamp for 10-20 s to obtain a polymer film material; The solute of the mixed solution includes epoxy liquid crystal molecules, acrylic liquid crystal molecules, chiral dopants, photoinitiators, photoinitiator aids and free radical photoinitiators; in the solute of the mixed solution, the mass ratio of epoxy liquid crystal molecules, photoinitiators, photoinitiator aids and free radical photoinitiators is 27-54:2.7-5.4:1-2:1.8-3.2; in the solute of the mixed solution, the mass ratio of epoxy liquid crystal molecules and acrylic liquid crystal molecules is 27-54:36-63; The epoxy liquid crystal molecules are selected from one or more of liquid crystal compound 1, liquid crystal compound 2, liquid crystal compound 3 and liquid crystal compound 4; The general structural formula of the liquid crystal compound 1 is as follows: ; The general structural formula of the liquid crystal compound 2 is as follows: ; The general structural formula of the liquid crystal compound 3 is as follows: ; The general structural formula of the liquid crystal compound 4 is as follows: ; Wherein, R is selected from COOCH 2 CH 3 、OCH 3 or COOCH 3 , m=4-8; A represents the central group of the liquid crystal compound 1 or the liquid crystal compound 2, and its general structural formula is shown in Formula I: ; Among them, R 1 Selected from H, Cl, F, CH 3 , CH 2 CH 3 、OCH 3 or COOCH 3 ; The general structural formula of the acrylic liquid crystal molecule is as follows: ; In the acrylic liquid crystal molecule, t=4-8, B represents the central group of the acrylic liquid crystal molecule, and its general structural formula is shown in Formula II: ; Among them, R 2 Selected from H, Cl, F, CH 3 , CH 2 CH 3 、OCH 3 or COOCH 3 ; The free radical photoinitiator is 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone; the photoinitiator is a triarylsulfonium salt; the chiral dopant is selected from any two of chiral dopant 1, chiral dopant 2, chiral dopant 3 and chiral dopant 4; in the solute of the mixed solution, the mass fraction of chiral dopant 1, chiral dopant 2, chiral dopant 3 or chiral dopant 4 is not higher than 4.5%; The general structural formula of the chiral dopant 1 is as follows: ; Among them, p = 4-8; The general structural formula of the chiral dopant 2 is as follows: ; Where x=4-8; The general structural formula of the chiral dopant 3 is as follows: ; Among them, n=3-12; The general structural formula of the chiral dopant 4 is as follows: ; Among them, q=3-12; In the chiral dopant, M represents a group of the chiral center of the chiral dopant, and its general structural formula is shown in Formula III, Formula IV, Formula V or Formula VI: 、 、 、 ; S12: irradiating the polymer film material with 365 nm ultraviolet light at 80-130° C. to obtain the double-layer liquid crystal film.

2. The method for preparing a double-layer liquid crystal film according to claim 1, It is characterized in that The photoinitiator auxiliary agent is 2-isopropylthioxanthone or 2-hydroxy-2-methyl-1-phenyl-1-propanone.

3. The method for preparing a double-layer liquid crystal film according to claim 1, It is characterized in that The solvents of the mixed solution are cyclopentanone and cyclohexanone.

4. The method for preparing a double-layer liquid crystal film according to claim 1, It is characterized in that The solvents of the mixed solution are cyclohexanone and ethyl acetate.

5. The method for preparing a double-layer liquid crystal film according to claim 1, It is characterized in that The solute of the mixed solution also includes a leveling agent.

6. A double-layer liquid crystal film prepared by the preparation method according to any one of claims 1 to 5.