A release agent for lead-acid battery grid casting and preparation method thereof

By using mold release agent formulas with cork powder, diatomaceous earth and other components in lead-acid battery grid casting, the problems of unsmooth mold release and the influence of lead liquid surface tension are solved, forming a thermal insulation film layer, and improving the complete grid formation is improved The consistency of performance and battery performance extends the service life of the mold release agent and improves production efficiency.

CN116673432BActive Publication Date: 2024-11-26JIANGSU LEOCH BATTERY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310624433.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-11-26
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

The mold release in traditional lead-acid battery panel grid casting is not smooth, the lead liquid surface tension affects molding integrity and battery performance, and insufficient mold insulation leads to large crystals, low mechanical strength, and poor corrosion resistance.

Method used

Using a mold release agent formula including pure water, soft wood powder, diatomaceous earth, magnesium stearate, male resin and baking soda, a thermal insulation film layer is formed through soft wood powder and diatomaceous earth, destroying the surface tension of the lead liquid and promoting the lead liquid. Flow and strengthen the film layer through male resin to improve mold release smoothness and battery performance.

Benefits of technology

It achieves smooth mold release, molding integrity and battery performance consistency of the grid, extends the service life of the mold release agent, improves production efficiency, and reduces the number of spraying times of the grid process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116673432B_ABST
    Figure CN116673432B_ABST
Patent Text Reader

Abstract

The invention provides a demoulding agent for casting a lead-acid battery grid, which comprises the following raw materials: water, cork powder, diatomaceous earth, magnesium stearate, sodium tripolyphosphate, maleic resin, ethanol and baking soda. When casting the grid, the demoulding agent of the formula is evenly sprayed on the surface of a mold cavity, and a film layer can be formed after high-temperature water loss. The cork powder and diatomaceous earth in the formula can keep the heat, and prevent the grid from cooling too fast, resulting in coarse crystal particles with pores, and causing the grid to have low mechanical strength and poor corrosion resistance. The grid is easy to demould and is not easy to deform. The baking soda in the formula promotes the dissolution of maleic rosin in an ethanol-water solution, and the maleic rosin forms a high-temperature, wear-resistant and corrosion-resistant film layer, fixes and strengthens the cork powder, and the sodium tripolyphosphate destroys the surface tension of the alloy lead liquid, which is conducive to the flow of the lead liquid. The grid is completely formed, the weight and thickness tolerance of the grid are reduced, and the battery performance consistency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mold release agent production, and in particular relates to a mold release agent for lead-acid battery grid casting and a preparation method thereof. Background Art

[0002] Today, with the rapid development of lithium batteries and hydrogen energy, lead-acid batteries still have a place in the energy field. Lead-acid batteries have low self-discharge rates and high safety, making them excellent UBS power sources. At the same time, as a starting battery, they have excellent large-current discharge characteristics, making them very suitable for vehicle starting and short-term use of high-power electrical appliances. The discharge carrier of lead-acid batteries is the plate, and the active ingredient of the plate, lead paste, is attached to the grid, and the charge and discharge current is also transmitted on the grid. Therefore, good grid quality also determines the discharge performance of the plate and the performance of the battery;

[0003] Traditional grids are made by casting. The molten lead alloy is transferred into a lead bucket, which is then tilted and poured into the mold to fill the cavity. After cooling, the grid is formed. During this period, a release agent needs to be sprayed on the surface of the mold cavity regularly to maintain the quality characteristics of the grid.

[0004] First: Ensure that the grid is demolded smoothly. After the grid is formed, the mold is opened, and after the grid falls off, the mold is closed. If demolding is not smooth, it will interfere with the subsequent grid casting. At the same time, the grid that is difficult to fall off is prone to deformation, affecting the subsequent paste coating process. The release agent will form a smooth and elastic film layer on the surface of the cavity, making the surface of the grid smooth and easy to remove from the mold;

[0005] Second: destroy the surface tension of the lead liquid. The surface tension of the lead alloy will cause the small passages inside the mold to not be filled, and the corners will not be completely formed. This will affect the weight of the paste, the charge and discharge current density will be uneven, and the battery performance will be seriously reduced. The release agent can destroy the surface tension of the lead liquid, so that the grid is completely formed and the weight and size are consistent;

[0006] Third: mold insulation. After the lead liquid is poured into the mold, it will cool down quickly, and the crystals inside the lead alloy will grow and form quickly, forming coarse crystal particles. Studies have shown that this type of crystal has poor corrosion resistance and low mechanical strength. The release agent can provide insulation, slowing down the temperature change of the lead alloy during crystal growth and forming dense and fine crystals. Summary of the invention

[0007] To achieve the above-mentioned purpose, the technical scheme of the present invention is as follows: a release agent for casting a lead-acid battery grid, the release agent comprising the following raw materials in parts by mass: 120-140 parts of pure water; 7-8 parts of cork powder; 1-2 parts of diatomaceous earth; 0.5-1 parts of magnesium stearate; 2-3 parts of sodium tripolyphosphate; 3-4 parts of maleic resin; 30-40 parts of ethanol; and 1-2 parts of baking soda.

[0008] As an improvement of the present invention, the parts by mass are 130 parts of pure water; 7 parts of cork powder; 1.5 parts of diatomaceous earth; 1 part of magnesium stearate; 2 parts of sodium tripolyphosphate; 3 parts of maleic resin; 30 parts of ethanol; and 1 part of baking soda.

[0009] As an improvement of the present invention, the conductivity of the pure water is ≤10µs / cm.

[0010] As an improvement of the present invention, the fineness of the cork powder is 300 meshes.

[0011] As an improvement of the present invention, the diatomaceous earth has a fineness of 600 meshes.

[0012] As an improvement of the present invention, the weight ratio of the cork powder to diatomaceous earth is 14:3.

[0013] When casting the grid, the release agent of this formula is evenly sprayed on the surface of the mold cavity, and a film layer can be formed after high-temperature water loss; the cork powder and diatomaceous earth in the formula can keep warm and prevent the grid from cooling too fast, resulting in coarse crystal particles with pores, resulting in low mechanical strength and poor corrosion resistance of the grid; the grid is easy to demold and not easy to deform; the baking soda in the formula promotes the dissolution of maleic rosin in the ethanol-water solution, and the maleic rosin forms a high-temperature, wear-resistant and corrosion-resistant film layer, which fixes and strengthens the cork powder, and the sodium tripolyphosphate destroys the surface tension of the alloy lead liquid, which is beneficial to the flow of the lead liquid, and the grid is completely formed, thereby reducing the weight and thickness tolerance of the grid and improving the consistency of battery performance.

[0014] By mixing the cork powder and diatomaceous earth, a fine frosted film layer is formed on the surface of the mold cavity, making it easy to demould the lead alloy grid, so the ratio of the cork powder and diatomaceous earth in this formula can be fine-tuned.

[0015] As an improvement of the present invention, a method for preparing a release agent for casting a lead-acid battery grid is provided, the method comprising the following steps:

[0016] Step 1: dry-mix diatomaceous earth and cork powder to obtain mixture 1;

[0017] Step 2: Add water to the mixture and stir to raise the temperature;

[0018] Step 3: Heat pure water, add magnesium stearate and sodium tripolyphosphate while stirring, stir evenly and let stand to obtain solution 3;

[0019] Step 4: Mix ethanol and water to prepare ethanol-water solution 4, and add baking soda;

[0020] Step 5: Crush the maleic rosin and add it into solution 4, stir at room temperature to obtain solution 5;

[0021] Step six: Stir the obtained solution five and solution three evenly to obtain the release agent.

[0022] As an improvement of the present invention, in the method, after dry mixing the formulated amount of cork powder and diatomaceous earth, 100 parts of water are added, stirred evenly, and then heated to 80°C, and after adding the formulated amount of magnesium stearate and sodium tripolyphosphate, heating is continued for 30 minutes, and the temperature is cooled to obtain an emulsion.

[0023] As an improvement of the present invention, in the method, after mixing 30 parts of ethanol in a hydration formula at room temperature, the maleic resin ground into powder is poured into the ethanol-water mixture and stirred until it is completely dissolved to obtain a resin solution.

[0024] As an improvement of the present invention, the emulsion and the resin solution are finally mixed and stirred at room temperature for 10 minutes to obtain the release agent.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: the mold release agent for casting the lead-acid battery grid of the present invention improves the traditional cork powder formula, and diatomaceous earth is added to the cork powder to form gaps in the film layer formed by the mold release agent. The cork powder and diatomaceous earth in the mold release agent can keep the mold warm, so that the film layer has a good thermal insulation effect, and the grid can be smoothly demolded. Resin is used to strengthen the film layer, and the service life of the cork powder is increased; magnesium stearate improves the resin molding effect; sodium tripolyphosphate and cork powder can both destroy the surface tension of the lead liquid, so that the lead liquid flows more smoothly in the mold, and the integrity of the grid is good after molding; the condensation speed of the lead alloy is slowed down, and small crystals inside the grid grow; magnesium stearate in the formula can improve resin molding; baking soda improves the dissolution effect of the resin, so that the resin can be evenly dispersed in the solution, and maleic resin can strengthen the strength of the film layer, so that the cork powder on the film layer is resistant to high temperature and not easy to fall off, thereby extending the service life of the mold release agent, reducing the number of times the mold release agent is sprayed in the process of casting the grid, and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a graph showing the weight change of the new and old release agent grids in this embodiment.

[0027] Figure 2 This is a graph showing the thickness change of the new and old release agent grids in this embodiment. Implementation

[0028] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0029] Embodiment: This embodiment is a release agent for casting a lead-acid battery grid, and the release agent comprises the following raw materials in parts by mass: 120-140 parts of pure water; 7-8 parts of cork powder; 1-2 parts of diatomaceous earth; 0.5-1 parts of magnesium stearate; 2-3 parts of sodium tripolyphosphate; 3-4 parts of maleic resin; 30-40 parts of ethanol; and 1-2 parts of baking soda.

[0030] Furthermore, the parts by mass are 130 parts of pure water; 7 parts of cork powder; 1.5 parts of diatomaceous earth; 1 part of magnesium stearate; 2 parts of sodium tripolyphosphate; 3 parts of maleic resin; 30 parts of ethanol; and 1 part of baking soda. The conductivity of the pure water is ≤10µs / cm, the fineness of the cork powder is 300 mesh, the fineness of the diatomaceous earth is 600 mesh, and the weight ratio of the cork powder to the diatomaceous earth is 14:3. By mixing the cork powder and the diatomaceous earth, a fine frosted film layer is formed on the surface of the mold cavity, which makes it easy to demold the lead alloy grid. Therefore, the ratio of the cork powder and the diatomaceous earth in this formula can be fine-tuned.

[0031] Furthermore, a method for preparing a release agent for casting a lead-acid battery grid is provided, the method comprising the following steps: step 1: dry-mixing diatomaceous earth and cork powder to obtain mixture 1; step 2: adding water to mixture 1 and stirring to increase the temperature; step 3: heating pure water, adding magnesium stearate and sodium tripolyphosphate while stirring, stirring and standing to obtain solution 3; step 4: mixing ethanol and water to form ethanol-water solution 4, and adding baking soda; step 5: breaking maleic rosin and adding it to solution 4, stirring at room temperature to obtain solution 5; step 6 : The obtained solution five and solution three are stirred evenly to obtain the release agent. In the method, after dry mixing the formula amount of cork powder and diatomaceous earth, 100 parts of water are added and stirred evenly, and then heated to 80°C, and the formula amount of magnesium stearate and sodium tripolyphosphate are added and continued to be heated for 30 minutes, and the temperature is cooled to obtain an emulsion. In the method, after mixing 30 parts of hydration formula amount of ethanol at room temperature, the maleic resin ground into powder is poured into the ethanol-water mixture and stirred until it is completely dissolved to obtain a resin solution. Finally, the emulsion and the resin solution are mixed and stirred at room temperature for 10 minutes to obtain the release agent.

[0032] like Figure 1 As shown (the horizontal axis represents the serial number of the grid sample, and the vertical axis represents the weight value corresponding to the weight of the grid sample), when the grid is cast, the weight of the grid changes when using the new and old release agents. The standard deviation of the grid weight when using the ordinary release agent is σ=2.75, and the standard deviation of the grid weight with the release agent of this formula is σ=1.03, where "σ" stands for sigma, which refers to the standard deviation. The larger the value, the more dispersed the data. Conversely, the smaller the value, the more concentrated the data. In addition to ensuring the quality of grid casting, this formula of release agent also ensures the consistency of grid weight and thickness. The better the consistency, the better the battery's charging and discharging capacity and the consistency of resistance, voltage, etc.

[0033] like Figure 2 As shown (the horizontal axis represents the serial number of the grid sample, and the vertical axis represents the thickness value corresponding to the weight of the grid sample), when the grid is cast, the thickness of the grid changes when using the new and old release agents. The standard deviation of the thickness of the grid using the ordinary release agent is σ=0.04, and the standard deviation of the thickness of the grid with the release agent of this formula is σ=0.026. Therefore, it is shown that when the grid is cast, the weight and thickness change values ​​of the grid are improved, and the performance consistency of the grid is effectively improved. When verifying the formula of the new and old release agents, the process parameters during casting are consistent (lead spoon temperature 480℃-520℃, grinding temperature 100℃-140℃, mold bottom 110℃-150℃). The old release agent formula: 120~140 parts of pure water; 7~8 parts of cork powder; 2-3 parts of bone glue; 1-2 parts of polyvinyl alcohol.

[0034] It should be noted that the above content only illustrates the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.

Claims

1. A lead-acid battery grid casting release agent, characterized in that: The release agent comprises the following raw materials in parts by mass: 120-140 parts of pure water; 7-8 parts of cork powder; 1-2 parts of diatomaceous earth; 0.5-1 parts of magnesium stearate; 2-3 parts of sodium tripolyphosphate; 3-4 parts of maleic resin; 30-40 parts of ethanol; and 1-2 parts of baking soda. The conductivity of the pure water is ≤10µs / cm, the fineness of the cork powder is 300 mesh, the fineness of the diatomaceous earth is 600 mesh, and the weight ratio of the cork powder to the diatomaceous earth is 14:

3.

2. The lead-acid battery grid casting release agent according to claim 1, characterized in that: The parts by mass are 130 parts of pure water, 7 parts of cork powder, 1.5 parts of diatomaceous earth, 1 part of magnesium stearate, 2 parts of sodium tripolyphosphate, 3 parts of maleic resin, 30 parts of ethanol and 1 part of baking soda.

3. A method for preparing a release agent for lead-acid battery grid casting according to claim 1, characterized in that: The method comprises the following steps: Step 1: dry-mix diatomaceous earth and cork powder to obtain mixture 1; Step 2: Add water to the mixture and stir to raise the temperature; Step 3: Heat pure water, add magnesium stearate and sodium tripolyphosphate while stirring, stir evenly and let stand to obtain solution 3; Step 4: Mix ethanol and water to prepare ethanol-water solution 4, and add baking soda; Step 5: Crush the maleic rosin and add it into solution 4, stir at room temperature to obtain solution 5; Step six: Stir the obtained solution five and solution three evenly to obtain the release agent.

4. The method for preparing a release agent for lead-acid battery grid casting according to claim 3, characterized in that: In the method, after dry mixing the formulated amount of cork powder and diatomaceous earth, 100 parts of water are added, stirred evenly, and then heated to 80° C., magnesium stearate and sodium tripolyphosphate are added, and then heated for 30 minutes, and cooled to obtain an emulsion.

5. The method for preparing a release agent for lead-acid battery grid casting according to claim 4, characterized in that: In the method, 30 parts of water and a formulated amount of ethanol are mixed at room temperature, and then maleic resin ground into powder is poured into the ethanol-water mixture and stirred until it is completely dissolved to obtain a resin solution.

6. The method for preparing a release agent for lead-acid battery grid casting according to claim 5, characterized in that: Finally, the emulsion and the resin solution were mixed and stirred at room temperature for 10 minutes to obtain the release agent.