A smoke suppressant containing tertiary carbon polymer and its preparation method
By introducing transition metal elements into the LDHs layer and regulating the metal defect structure, the problem of flue gas release during the combustion of polymers containing tertiary carbon was solved, achieving efficient smoke suppression and environmentally friendly oxidation of the polymer and reducing smoke density.
Patent Information
- Application Number
- CN202310542204.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-05-15
AI Technical Summary
Existing tertiary carbon polymers release large amounts of dense smoke and toxic gases when burned, limiting their application in daily life and production. Furthermore, existing smoke suppressants are difficult to form an effective char layer to block oxygen and heat transfer in smoldering environments.
Transition metal elements such as Co, Fe, and Ni are introduced into the LDHs layer, and metal defects are controlled by alkaline etching in an alkaline environment to prepare LDHs with metal defect structures, thereby improving their ability to oxidize tertiary carbon and promoting the oxidation of combustion decomposition products into invisible gases such as CO2.
It significantly reduces the smoke density during polymer combustion, achieving a highly efficient smoke suppression effect. Furthermore, the preparation method is simple, low-cost, and environmentally friendly with no pollution.
Smart Images

Figure CN116693935B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of smoke suppression material preparation technology, and specifically relates to a smoke suppressant containing tertiary carbon polymer and its preparation method. Background Technology
[0002] Polypropylene, polybutene, and polypentene are polymers containing tertiary carbon and are widely used in production and daily life fields that require high flame retardancy and smoke suppression properties, such as clothing and blankets. However, these polymers are flammable materials and release large amounts of dense smoke and toxic gases when exposed to open flames or heated, posing a threat and harm to human health and the environment. This limits their application in daily life and production. Therefore, research on smoke suppression of these materials has important theoretical value and practical application significance.
[0003] Most smoke suppressants achieve their effect by promoting char formation during the combustion of polymer substrates, i.e., promoting the formation of dense char residue. However, in some cases, polymers do not easily form a char layer that can block oxygen and heat transfer in smoldering environments. Therefore, the density of polymer combustion smoke can be reduced by altering the combustion product transformation process and promoting the oxidation of combustion decomposition products into invisible smoke gases such as CO2. Summary of the Invention
[0004] This method proposes introducing transition metal elements such as Co, Fe, and Ni, as well as elements such as Al and Zn that can dissolve in an alkaline environment, into the LDHs layer. Then, alkaline etching is used to control the metal defects on the LDHs surface, thus preparing LDHs with a metal defect structure. The general composition formula is Co. x Zn 1-x Fe y Al 1-y -CO3-LDH and Ni x Zn 1-x Fe y Al 1-y -CO3-LDH, including CoFeAl-LDHs, CoZnFe-LDHs, NiFeAl-LDHs, NiZnFe-LDHs, etc., significantly increases the lone pair electron content in LDHs, enhances their ability to attack and oxidize tertiary carbons in polymers, and strengthens the smoke suppression performance of polymers containing tertiary carbons.
[0005] The preparation method of the tertiary carbon polymer smoke suppressant is as follows: 1-10g of hydrotalcite is dispersed in 100-300ml of deionized water, and then 5-50ml of sodium hydroxide solution is added dropwise while stirring. The concentration of the sodium hydroxide solution is 1-5mol / L. After the addition is completed, stirring is continued for 1-24h to allow NaOH to fully react with the surface of the hydrotalcite. Finally, the hydrotalcite is washed with deionized water and ethanol until neutral. The filter cake is dried at 50-120℃ and ground to obtain hydrotalcite with defects, which is the tertiary carbon polymer smoke suppressant.
[0006] The layer metals of the hydrotalcite are cobalt-iron-aluminum, cobalt-zinc-iron, nickel-iron-aluminum, and nickel-zinc-iron. The molar ratio of divalent to trivalent metals is 1-6.
[0007] The tertiary carbon-containing polymers are polypropylene, polybutene, and polypentene.
[0008] The beneficial effects of this invention are as follows:
[0009] (1) This invention utilizes the tunability of LDHs to introduce transition metal elements such as Co, Fe, and Ni, as well as elements such as Al and Zn that can dissolve in an alkaline environment, into the LDHs layer. By using an alkaline-controlled etching method, selective removal of metal elements such as Al and Zn is achieved, thus preparing Co with tunable metal defect structure. x Zn 1-x Fe y Al 1-y -CO3-LDH and Ni x Zn 1- x Fe y Al 1-y -CO3-LDH enables the regulation of the surface electron distribution state of LDHs, enhances the nucleophilic attack of LDHs on tertiary carbons, promotes the full oxidation of polymer decomposition products into invisible gases such as CO2, and reduces the smoke density during combustion of polymer products containing tertiary carbons; adding 5 phr of Co2Fe to 100g of polypropylene 0.5 Al 0.5 -LDH can reduce the maximum smoke density by 55.1% compared to the blank sample;
[0010] (2) By introducing nucleophilic elements into LDHs and controlling the electronic state of the layer surface through the creation of defect structures, they can act as nucleophilic reagents to effectively attack the more active carbons in the carbon chain, realize the "end of the chain" oxidation of the polymer, oxidize the thermal decomposition products of the polymer containing tertiary carbon into invisible smoke, and thus achieve a better smoke suppression effect.
[0011] (3) The present invention Co x Zn 1-x Fe y Al 1-y-CO3-LDH and Ni x Zn 1-x Fe y Al 1-y -CO3-LDH has significant advantages such as simple preparation, low manufacturing cost, and green environmental protection, making it a promising method for manufacturing materials with catalytic oxidation and smoke suppression properties. Attached Figure Description
[0012] Figure 1 Co2Fe prepared in Example 1 0.5 Al 0.5 XRD pattern of -LDH.
[0013] Figure 2 Co2Fe prepared in Example 1 0.5 Al 0.5 Fourier infrared spectrum of -LDH.
[0014] Figure 3 Co2Fe prepared in Example 1 0.5 Al 0.5 SEM image of -LDH.
[0015] Figure 4 The images show the TG-IR spectra of Example 1, Comparative Example 1, and blank PP sample, with the left image at 2968 cm⁻¹. -1 2358cm on the right -1 .
[0016] Figure 5 XPS images of LDHs samples from Example 1 and Comparative Example 1, with Co 2p on the left and Fe 2p on the right.
[0017] Figure 6 The graphs show the smoke density curves of Example 1, Comparative Example 1, and the blank PP sample. Detailed Implementation
[0018] To better understand the present invention, the following embodiments further illustrate the content of the present invention. However, the content of the present invention is not limited to the following embodiments, and the embodiments should not be regarded as a limitation on the scope of protection of the present invention.
[0019] Example 1
[0020] 21.82 g of Co(NO3)2·6H2O, 7.58 g of Fe(NO3)3·9H2O, and 7.03 g of Al(NO3)3·9H2O were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. 7.95 g of NaOH and 7.2 g of Na2CO3 were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. The mixed solution was placed in the beaker and added to a rotating liquid film reactor at the same flow rate using a peristaltic pump. The salt and alkali solutions were rapidly mixed at 3000 rpm. The solution was then added to a thoroughly dried three-necked flask, and a thermometer, reflux condenser, and stirrer were installed. The reaction was carried out at 100°C and 650 rpm for 6 h. The reaction mixture was washed with deionized water and ethanol until neutral. The product was dried in a 100°C oven for 24 h, then ground into powder to obtain brownish-red Co2Fe. 0.5 Al 0.5 -LDH. Dissolve 5.0 g of powder in 200 ml of deionized water, stir for 30 min until a uniform turbid slurry is formed, then add 1 mol·L⁻¹. -1 Add 20 ml of NaOH to a thoroughly dried three-necked flask and attach the stirrer. React at 650 rpm for 8 hours. Wash the reaction mixture with deionized water and ethanol until neutral. Dry the product in a 100°C oven for 24 hours, then grind it into powder to obtain a brownish-brown etched Co2Fe. 0.5 Al 0.5 -LDH sample. 1.5g of the prepared LDH was weighed out at a ratio of 5 phr and mixed with 30g of polypropylene substrate. The mixture was then thoroughly mixed using a two-roll mill manufactured by Baopin Precision Instruments Co., Ltd. Specific conditions were: 180℃, front-to-back roll speed ratio 1:1.5, and front roll linear speed 8.95 m·min. -1 The mixing time was 5 minutes. The cooled composite sample was then flattened using an electric tablet press with the following parameters: 185℃, pre-compression at 7 MPa for 2 minutes, venting 5 times, and pressurization at 10 MPa for 2 minutes. The resulting tablets yielded Co2Fe. 0.5 Al 0.5 -LDH and polypropylene composites.
[0021] The crystal structure of the LDH sample was characterized using a DX-2700 X-ray diffraction analyzer from Haoyuan Instruments Co., Ltd. Figure 1 The XRD pattern shows that Co2Fe 0.5 Al 0.5The LDH sample exhibits characteristic peaks consistent with the LDH standard card. At lower angles, the (003), (006), and (009) diffraction peaks corresponding to 2θ are sharp and symmetrical, while the (110) and (113) diffraction peaks corresponding to 2θ at higher angles (60-63°) are weaker. (Co2Fe) 0.5 Al 0.5 The -LDH sample was successfully synthesized, exhibiting good crystallinity and was thoroughly purified without any impurity peaks.
[0022] Specific functional groups in the LDH sample were characterized using a VECTOR22 Fourier transform infrared spectroscopy instrument from Bruker, Germany. Figure 2 The image shows an FT-IR spectrum, from which we can obtain Co2Fe 0.5 Al 0.5 The infrared curve of the LDH sample is consistent with the LDH standard spectrum, with the value at 3451 cm⁻¹. -1 The absorption peak at 1363 cm⁻¹ is attributed to the stretching vibration peaks of the uniformly distributed -OH groups on the LDH layers and the interlayer crystal water or adsorbed water. -1 The absorption peak at that point is attributed to the CO3 anion from the LDH intercalation layer. 2- The asymmetric vibration peak of the OCO bond, 400–700 cm⁻¹ -1 The absorption peak at this point is attributed to the stretching vibration peak of the OMO bond lattice vibration on the LDH layer. Infrared analysis results indicate that Co₂Fe 0.5 Al 0.5 -LDH sample was successfully synthesized and purified.
[0023] The morphology and structure of LDH samples were characterized using a Supra 55 scanning electron microscope from Zeiss GmbH, Germany. Figure 3 This is a SEM image. From the image, we can see that Co2Fe 0.5 Al 0.5 - The LDH sample largely retained its original LDH morphology after etching, without any dissolution or aggregation. After 8 hours of NaOH etching modification, Co2Fe 0.5 Al 0.5 - The edges of the LDH layer are no longer smooth and regular, and the roughness increases. The hexagonal flakes show a tendency to fragment, but still maintain a lamellar structure and no lamellar collapse occurs.
[0024] The thermal degradation process of LDH-PP composite material was analyzed using a PerkinElmer simultaneous thermal analyzer coupled with Fourier transform infrared spectroscopy. The figure shows that after the addition of LDH, the polypropylene decomposed into hydrocarbons (2968 cm⁻¹). -1 The concentration of CO2 in the product decreased (2258 cm⁻¹). -1 The increase was significant, and the change in the product of Example 1 was greater than that of Comparative Example 4.
[0025] The surface charge distribution of LDHs samples before and after NaOH etching was characterized using an XPS instrument manufactured by Shimadzu Corporation (UK). The figure shows the surface charge distribution of Co2Fe-LDHs after NaOH etching. 0.5 Al 0.5 -LDHs contain surface defects, and the electron binding energies of Co and Fe in LDHs change. Compared with Co2Fe-LDH, the alkaline etched Co2Fe... 0.5 Al 0.5 - 2p of Co in LDH 3 / 2 The orbital binding energy is 779.7 eV, 2p 1 / 2 The orbital binding energy is 795.8 eV, which shifts towards a higher energy direction compared to Comparative Example 4, indicating that Co loses electrons and the coordination structure changes, affecting the 2p orbital binding energy of Fe. 3 / 2 The orbital binding energy is 761.9 eV, 2p 1 / 2 The orbital binding energy is 775.8 eV, which shifts towards a lower energy direction compared to Comparative Example 4, indicating that Fe gains electrons and has a stronger nucleophilic ability. Compared to Co2Fe-LDH, the alkaline etched Co2Fe... 0.5 Al 0.5 The changes in the electron binding energies of Co and Fe in -LDH indicate an interaction between the two elements, which modulates the electron distribution state of the metal reactive sites.
[0026] The smoke density of LDH-PP composite material during thermal decomposition was tested using an SDB smoke density tester manufactured by Kunshan Modis Co., Ltd., and the measured smoke density value was 124.94. The figure shows that the smoke density of polypropylene decreased after the addition of LDH, and the decrease in Example 1 was greater than that in Comparative Example 4.
[0027] Example 2
[0028] 21.82 g of Co(NO3)2·6H2O, 11.36 g of Fe(NO3)3·9H2O, and 3.52 g of Al(NO3)3·9H2O were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. 7.95 g of NaOH and 7.2 g of Na2CO3 were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. The mixed solution was placed in the beaker and added to a rotating liquid film reactor at the same flow rate using a peristaltic pump. The salt and alkali solutions were rapidly mixed at 3000 rpm. The solution was then added to a thoroughly dried three-necked flask, and a thermometer, reflux condenser, and stirrer were installed. The reaction was carried out at 100°C and 650 rpm for 6 h. The reaction mixture was washed with deionized water and ethanol until neutral. The product was dried in a 100°C oven for 24 h, then ground into powder to obtain a brownish-brown Co2Fe. 0.75 Al 0.25 -LDH. Dissolve 5.0 g of powder in 200 ml of deionized water, stir for 30 min until a uniform turbid slurry is formed, then add 1 mol·L⁻¹. -1 Add 20 ml of NaOH to a thoroughly dried three-necked flask and attach the stirrer. React at 650 rpm for 8 hours. Wash the reaction mixture with deionized water and ethanol until neutral. Dry the product in a 100°C oven for 24 hours, then grind it into powder to obtain a brownish-brown etched Co2Fe. 0.75 Al 0.25 -LDH sample. 1.5g of the prepared LDH was weighed out at a ratio of 5 phr and mixed with 30g of polypropylene substrate. The mixture was then thoroughly mixed using a two-roll mill manufactured by Baopin Precision Instruments Co., Ltd. Specific conditions were: 180℃, front-to-back roll speed ratio 1:1.5, and front roll linear speed 8.95 m·min. -1 The mixing time was 5 minutes. The cooled composite sample was then flattened using an electric tablet press with the following parameters: 185℃, pre-compression at 7 MPa for 2 minutes, venting 5 times, and pressurization at 10 MPa for 2 minutes. The resulting tablets yielded Co2Fe. 0.75 Al 0.25 -LDH and polypropylene composite material, the smoke density test value is 129.57.
[0029] Example 3
[0030] 21.82 g of Co(NO3)2·6H2O, 13.64 g of Fe(NO3)3·9H2O, and 1.41 g of Al(NO3)3·9H2O were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. 7.95 g of NaOH and 7.2 g of Na2CO3 were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. The mixed solution was placed in the beaker and added to a rotating liquid film reactor at the same flow rate using a peristaltic pump. The salt and alkali solutions were rapidly mixed at 3000 rpm. The solution was then added to a thoroughly dried three-necked flask, and a thermometer, reflux condenser, and stirrer were installed. The reaction was carried out at 100°C and 650 rpm for 6 h. The reaction mixture was washed with deionized water and ethanol until neutral. The product was dried in a 100°C oven for 24 h, then ground into powder to obtain a brownish-brown Co2Fe. 0.9 Al 0.1 -LDH. Dissolve 5.0 g of powder in 200 ml of deionized water, stir for 30 min until a uniform turbid slurry is formed, then add 1 mol·L⁻¹. -1 Add 20 ml of NaOH to a thoroughly dried three-necked flask and attach the stirrer. React at 650 rpm for 8 hours. Wash the reaction mixture with deionized water and ethanol until neutral. Dry the product in a 100°C oven for 24 hours, then grind it into powder to obtain a brownish-brown etched Co2Fe. 0.9 Al 0.1 -LDH sample. 1.5g of the prepared LDH was weighed out at a ratio of 5 phr and mixed with 30g of polypropylene substrate. The mixture was then thoroughly mixed using a two-roll mill manufactured by Baopin Precision Instruments Co., Ltd. Specific conditions were: 180℃, front-to-back roll speed ratio 1:1.5, and front roll linear speed 8.95 m·min. -1 The mixing time was 5 minutes. The cooled composite sample was then flattened using an electric tablet press with the following parameters: 185℃, pre-compression at 7 MPa for 2 minutes, venting 5 times, and pressurization at 10 MPa for 2 minutes. The resulting tablets yielded Co2Fe. 0.9 Al 0.1 -LDH and polypropylene composite material, the smoke density test value is 134.22.
[0031] Comparative Example 1
[0032] 21.82 g of Co(NO3)2·6H2O and 15.15 g of Fe(NO3)3·9H2O were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. 7.95 g of NaOH and 7.2 g of Na2CO3 were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. The mixed solution was placed in the beaker and added to a rotating liquid film reactor at the same flow rate using a peristaltic pump. The salt and alkali solutions were rapidly mixed at 3000 rpm. The solution was then added to a thoroughly dried three-necked flask, and a thermometer, reflux condenser, and stirrer were installed. The reaction was carried out at 100°C and 650 rpm for 6 h. The reaction mixture was washed with deionized water and ethanol until neutral. The product was dried in a 100°C drying oven for 24 h, then ground into powder to obtain a brownish-red Co2Fe-LDH sample. Weigh 1.5g of the prepared LDH at a ratio of 5 phr and mix it with 30g of polypropylene substrate. The mixture is then thoroughly mixed using a two-roll mill manufactured by Baopin Precision Instruments Co., Ltd. Specific conditions include: 180℃, front-to-back roll speed ratio of 1:1.5, and a front roll linear speed of 8.95 m / min. -1 The mixing time was 5 minutes. The cooled composite sample was then flattened using an electric tablet press with the following parameters: 185℃, pre-compression at 7 MPa for 2 minutes, venting 5 times, and pressurization at 10 MPa for 2 minutes. After tableting, a Co2Fe-LDH and polypropylene composite material was obtained, with Co having a 2p... 3 / 2 The orbital binding energy is 779.0 eV, 2p 1 / 2 The orbital binding energy is 795.0 eV, and the 2p orbital binding energy of Fe is... 3 / 2 The orbital binding energy is 763.9 eV, 2p 1 / 2 The orbital binding energy is 776.9 eV. Its smoke density test value is 136.09.
[0033] Example 4
[0034] 21.82 g of Co(NO3)2·6H2O, 7.58 g of Fe(NO3)3·9H2O, and 5.56 g of Zn(NO3)2·6H2O were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. 7.95 g of NaOH and 7.2 g of Na2CO3 were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. The mixed solution was placed in the beaker and added to a rotating liquid film reactor at the same flow rate using a peristaltic pump. The salt and alkali solutions were rapidly mixed at 3000 rpm. The solution was then added to a thoroughly dried three-necked flask, and a thermometer, reflux condenser, and stirrer were installed. The reaction was carried out at 100°C and 650 rpm for 6 h. The reaction mixture was washed with deionized water and ethanol until neutral. The product was dried in a 100°C oven for 24 h, then ground into powder to obtain a brownish-red Co2Zn. 0.5 Fe 0.5 -LDH. Dissolve 5.0 g of powder in 200 ml of deionized water, stir for 30 min until a uniform turbid slurry is formed, then add 1 mol·L⁻¹. -1 Add 20 ml of NaOH to a thoroughly dried three-necked flask and attach the stirrer. React at 650 rpm for 8 hours. Wash the reaction mixture with deionized water and ethanol until neutral. Dry the product in a 100°C oven for 24 hours, then grind it into powder to obtain a brownish-brown etched Co2Zn. 0.5 Fe 0.5 -LDH sample. 1.5g of the prepared LDH was weighed out at a ratio of 5 phr and mixed with 30g of polybutene substrate. The mixture was then thoroughly mixed using a two-roll mill manufactured by Baopin Precision Instruments Co., Ltd. Specific conditions were: 180℃, front-to-back roll speed ratio 1:1.5, and front roll linear speed 8.95 m·min. -1 The mixing time was 5 minutes. The cooled composite sample was then flattened using an electric tablet press with the following parameters: 185℃, pre-compression at 7 MPa for 2 minutes, venting 5 times, and pressurization at 10 MPa for 2 minutes. Co2Zn was obtained after tableting. 0.5 Fe 0.5 The smoke density of the LDH and polybutene composite material was 187.43.
[0035] Example 5
[0036] 21.82 g of Co(NO3)2·6H2O, 7.58 g of Fe(NO3)3·9H2O, and 5.56 g of Zn(NO3)2·6H2O were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. 7.95 g of NaOH and 7.2 g of Na2CO3 were stirred and sonicated for 10 min, then dissolved in 150 ml of homemade deionized water in a beaker. The mixed solution was placed in the beaker and added to a rotating liquid film reactor at the same flow rate using a peristaltic pump. The salt and alkali solutions were rapidly mixed at 3000 rpm. The solution was then added to a thoroughly dried three-necked flask, and a thermometer, reflux condenser, and stirrer were installed. The reaction was carried out at 100°C and 650 rpm for 6 h. The reaction mixture was washed with deionized water and ethanol until neutral. The product was dried in a 100°C oven for 24 h, then ground into powder to obtain a brownish-red Co2Zn. 0.5 Fe 0.5 -LDH. Dissolve 5.0 g of powder in 200 ml of deionized water, stir for 30 min until a uniform turbid slurry is formed, then add 1 mol·L⁻¹. -1 Add 20 ml of NaOH to a thoroughly dried three-necked flask and attach the stirrer. React at 650 rpm for 8 hours. Wash the reaction mixture with deionized water and ethanol until neutral. Dry the product in a 100°C oven for 24 hours, then grind it into powder to obtain a brownish-brown etched Co2Zn. 0.5 Fe 0.5 -LDH sample. 1.5g of the prepared LDH was weighed out at a ratio of 5 phr and mixed with 30g of polypentene substrate. The mixture was then thoroughly mixed using a two-roll mill manufactured by Baopin Precision Instruments Co., Ltd. Specific conditions were: 180℃, front-to-back roll speed ratio 1:1.5, and front roll linear speed 8.95 m·min. -1 The mixing time was 5 minutes. The cooled composite sample was then flattened using an electric tablet press with the following parameters: 185℃, pre-compression at 7 MPa for 2 minutes, venting 5 times, and pressurization at 10 MPa for 2 minutes. Co2Zn was obtained after tableting. 0.5 Fe 0.5 The smoke density of the composite material of -LDH and polypentene was 137.54.
Claims
1. A method for preparing a smoke suppressant containing tertiary carbon polymers, characterized in that, The specific operation of the preparation method is as follows: 1-10g of hydrotalcite is dispersed in 100-300ml of deionized water, and then 5-50ml of sodium hydroxide solution is added dropwise while stirring. The concentration of the sodium hydroxide solution is 1-5mol / L. After the addition is completed, stirring is continued for 1-24h to allow NaOH to fully react with the surface of the hydrotalcite. Finally, the surface is washed with deionized water and ethanol until neutral. The filter cake is dried at 50-120℃ and ground to obtain hydrotalcite with defects, which is the smoke suppressant containing tertiary carbon polymer. The layer metals of the hydrotalcite are cobalt-iron-aluminum, cobalt-zinc-iron, nickel-iron-aluminum, and nickel-zinc-iron; The molar ratio of divalent to trivalent metals in the layers of the hydrotalcite is 1-6.
2. The preparation method according to claim 1, characterized in that, The tertiary carbon-containing polymers are polypropylene, polybutene, and polypentene.