A high temperature corrosion resistant austenitic stainless steel for nuclear power and its manufacturing method

By optimizing the composition and process in austenitic stainless steel and combining the multi-component composite effects of Mo, Ti and Ta, the problem of insufficient strength and corrosion resistance of austenitic stainless steel in high temperature and high pressure environments has been solved, and the problem of insufficient strength and corrosion resistance in high temperature and high pressure environments has been achieved. Excellent performance and low corrosion rate, suitable for nuclear power equipment.

CN116695024BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310621127.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-10-22
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

Existing austenitic stainless steel has low strength and insufficient corrosion resistance in high-temperature and high-pressure environments, making it difficult to meet the needs of nuclear power equipment. In particular, it is easy to cause embrittlement of welded joints during the welding process, reducing the plasticity and toughness of the material.

Method used

An austenitic stainless steel resistant to high temperature corrosion is designed. Its chemical composition includes C 0.04%-0.07%, Si 2.5%-4.5%, Mn 1.20%-1.50%, P≤0.015%, S≤0.005%, Ni 9.0 %-12.0%, Mo 0.85%-1.10%, Cr 13.0%-15.0%, Ti 0.02%-0.04%, Ta 0.15%-0.25%, using the production process of smelting-continuous casting-homogenization treatment-heating-rolling-heat treatment, through the multi-element composite effect of high melting point transition metal elements of Mo, Ti and Ta, Improve the high temperature strength and corrosion resistance of steel.

Benefits of technology

It has improved the room temperature and high temperature strength of the steel plate, has excellent high-temperature tensile properties at 350°C, and has a low corrosion rate in hydrochloric acid solution, meeting the high-temperature and high-pressure environmental requirements of nuclear power equipment. At the same time, the process is simple and the cost is low, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004255412350000071
    Figure BDA0004255412350000071
  • Figure BDA0004255412350000072
    Figure BDA0004255412350000072
  • Figure BDA0004255412350000073
    Figure BDA0004255412350000073
Patent Text Reader

Abstract

The present invention discloses a high temperature corrosion resistant austenitic stainless steel for nuclear power and a manufacturing method thereof. The chemical composition of the steel includes C: 0.04%-0.07%; Si: 2.5%-4.5%; Mn: 1.20%-1.50%; P≤0.015%; S≤0.005%; Ni: 9.0%-12.0%; Mo: 0.85%-1.10%; Cr: 13.0%-15.0%; Ti: 0.02%-0.04%; Ta: 0.15%-0.25%. The production process of smelting, continuous casting, homogenization treatment, heating, rolling and heat treatment is combined to ensure that the steel plate has a good strength level, and the room temperature yield strength (R p0.2 ) and tensile strength (R m ) reached 380MPa and 682MPa respectively; when stretched at 350℃, the yield strength (R p0.2 ) and tensile strength (R m ) reached 338MPa and 656MPa respectively. At the test temperature of 20℃ and 350℃, in 10% hydrochloric acid solution, the immersion time was 40h, and the corrosion rate was ≤1.90g / (m 2 h) and 2.80g / (m 2 h).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal materials, and in particular relates to a high temperature corrosion resistant austenitic stainless steel for nuclear power and a manufacturing method thereof. Background Art

[0002] Nuclear power units operate under high pressure and high temperature conditions. With the rapid development of the nuclear power industry, the demand for equipment materials will become higher and higher. Large-scale equipment and high temperature and high pressure will be important development trends in the future. However, with the increase in temperature, the corrosion rate of materials will also increase accordingly. At the same time, excessive pressure also puts higher requirements on the strength of equipment. At present, the main representative grades of austenitic stainless steel for nuclear power in my country are S30403 or S31603. The room temperature and high temperature strength of such materials are low, and they cannot be well applied to high temperature and high pressure working environments. In order to improve the strength of such materials, some design units will use S30408 ​​or S31608 with higher carbon content as a substitute, but with the increase of carbon content in the material, its resistance to intergranular corrosion will decrease, especially after sensitization treatment, the resistance to intergranular corrosion of the material will deteriorate sharply. In order to improve the intergranular corrosion resistance of the material, material designers generally add a certain amount of titanium or niobium to austenitic stainless steel. Once titanium or niobium is added excessively, it will cause embrittlement of the weld joint during welding and reduce the plasticity and toughness of the material. Therefore, conventional austenitic stainless steel is difficult to meet the requirements and can no longer meet the current industrial needs. Therefore, in order to solve the above problems, it is urgent to develop austenitic stainless steel that is resistant to high temperature corrosion.

[0003] The patent "Heat-resistant and corrosion-resistant austenitic stainless steel and its preparation method" with application number CN201910211762.9 includes, by weight percentage: C 0.006%-0.030%, Si 0.20%-0.70%, Mn 0.30%-1.0%, Cr 18.0%-20.0%, Ni 18.0%-20.0%, Mo 0.75%-1.50%, Al 0.20%-0.50%, Ti0.20%-0.50%, Nb0.10%-0.30%, P≤0.020%, S≤0.002%, N≤0.015%, B0.002%-0.006%, among which Al+Ti≥0.45%, 9≤(Nb+0.4Ti) / (C+N)≤18, and the rest are Fe and unavoidable impurities. The heat-resistant and corrosion-resistant austenitic stainless steel of the invention has excellent resistance to chloride ion pitting, stress corrosion and high-temperature oxidation, as well as good high-temperature strength, and can meet the use requirements of the outer shell material of the electric heating tube for electric water heaters. However, the maximum thickness of the produced steel plate is only 5mm, which is not suitable for the extra-thick austenitic stainless steel plate with a thickness of more than 40mm, and the Ni content in the steel is relatively high.

[0004] The patent "Austenitic stainless steel and its preparation method and application" with application number CN201811296546.0 includes the following components by mass percentage: C 0.04%-0.08%, Cr 16.5%-20.0%, Ni 14.5%-16.5%, Si1.0%-3.0%, Mn 1.5%-3.0%, Ti 0.2%-0.5%, Mo 1.3%-2.5%, B 0.003%-0.004%, and the balance is Fe. The austenitic stainless steel of this invention has higher room temperature and medium temperature tensile strength and excellent plasticity; after medium temperature aging treatment, the alloy strength increases, the plasticity does not decrease significantly, no harmful phase precipitation, and good organizational stability; it has excellent resistance to lead and lead-bismuth liquid metal corrosion and radiation resistance, and can better meet the material selection requirements of key components of lead-based fast reactors. However, the forging cost is high, the yield rate is low, and the finished product obtained by the invention has small size specifications and is not suitable for industrial production.

[0005] The patent "Austenitic stainless steel and its preparation method" with application number CN201811220143.8, by weight percentage, includes: C 0.04%-0.08%, Si 0.5%-1.5%, Mn 1.0%-3.0%, Cr 16%-18%, Ni 8%-10%, Nb 0.50%-1.00%, N 0.02%-0.06%, P≤0.025%, S≤0.010%, (0.5×Nb) / (30×C+50×N)≤0.12, and the balance is Fe and unavoidable impurities. The austenitic stainless steel of this invention can serve for a long time under high temperature conditions, with high yield and tensile strength of 400-600℃, which fully meets the requirements of molten salt storage tanks of solar thermal power stations. However, its corrosion resistance, especially high temperature corrosion resistance, cannot be guaranteed. Summary of the invention

[0006] The purpose of the present invention is to provide a high temperature corrosion resistant austenitic stainless steel for nuclear power and a manufacturing method thereof, and to design an alloy composition with appropriate process and cost considerations so that it has good high temperature performance and high temperature corrosion resistance.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A high temperature corrosion resistant austenitic stainless steel for nuclear power, the chemical composition of which, by weight percentage, comprises C: 0.04%-0.07%; Si: 2.5%-4.5%; Mn: 1.20%-1.50%; P≤0.015%; S≤0.005%; Ni: 9.0%-12.0%; Mo: 0.85%-1.10%; Cr: 13.0%-15.0%; Ti: 0.02%-0.04%; Ta: 0.15%-0.25%, and the balance is Fe and unavoidable impurities.

[0009] Furthermore, the chemical composition of stainless steel is Mo+Ti+Ta: 1.1%-1.3%.

[0010] Furthermore, the stainless steel plate has a thickness of 10-100 mm.

[0011] Furthermore, the room temperature yield strength Rp0.2 of the stainless steel reaches more than 380 MPa, the tensile strength Rm reaches more than 682 MPa, the elongation A reaches more than 25.5%, and the cross-sectional shrinkage Z reaches more than 72%; when stretched at a high temperature of 350°C, the yield strength Rp0.2 reaches more than 338 MPa, the tensile strength Rm reaches more than 656 MPa, the elongation A reaches more than 26.5%, and the cross-sectional shrinkage Z reaches more than 72%.

[0012] Furthermore, under the conditions of a test temperature of 20°C, a 10% hydrochloric acid solution, and an immersion time of 40 hours, the corrosion rate of stainless steel is ≤1.90g / (m 2 ·h); Under the conditions of test temperature of 350℃, 10% hydrochloric acid solution, immersion time of 40h, the corrosion rate of stainless steel is ≤2.80g / (m 2 h).

[0013] A method for manufacturing austenitic stainless steel for nuclear power with high temperature corrosion resistance, the production process includes: smelting, continuous casting, homogenization treatment, heating, rolling, heat treatment, wherein:

[0014] Homogenization treatment: put the continuous casting billet into the furnace, heat it up with the furnace, the heat treatment system is 1140-1160℃, keep it warm for 10-13h, and cool it with the furnace after the insulation is completed;

[0015] Heating: The continuous casting billet after homogenization treatment is heated with the furnace, the heating temperature is 1250-1270℃, and the soaking period in the furnace is 6h-8h;

[0016] Rolling: Two-stage controlled rolling is adopted. In the first stage, the starting rolling temperature is 1100-1150℃, the average reduction rate of the first three passes is controlled at 15%-20%, and the final rolling temperature is ≥970℃; in the second stage, the starting rolling temperature is 880-950℃, and the final rolling temperature is 780-850℃;

[0017] Heat treatment: pretreatment is carried out first, with heating temperature of 850-880℃ and holding time of 4-6h, and air cooling to room temperature after being taken out of the furnace; then solution heat treatment is carried out at 1100-1140℃, with holding time of 0.5-4.5h, and water cooling to room temperature after being taken out of the furnace.

[0018] Furthermore, the smelting adopts induction furnace + LF + RH. The induction furnace uses industrial pure iron and alloy to complete the melting and composition adjustment. The steel-out temperature of the induction furnace is ≥1650℃. LF completes the control of S and the removal of inclusions. RH performs vacuum treatment of the molten steel with a treatment vacuum degree of ≤0.2kPa.

[0019] Furthermore, the continuous casting pouring temperature is controlled at 1490-1510°C, and the pulling speed is controlled at 1.0-1.3 m / min.

[0020] Furthermore, the ingots are immediately stacked and slowly cooled for more than 48 hours after coming off the production line.

[0021] Furthermore, the thickness of the ingot is 200-300 mm.

[0022] In terms of component design, the present invention, on the basis of low-carbon component design, simultaneously adds Mo, Ti and Ta high-melting-point transition metal elements to strengthen the steel through multi-component composite effect, especially to increase the Si content in the steel, so that the steel has higher high-temperature strength and high-temperature corrosion resistance, and increases the passivation ability of stainless steel. The production process of smelting-continuous casting-homogenization treatment-heating-rolling-heat treatment is combined to ensure that the steel plate has good room temperature and high-temperature strength, good key indicators, and fully meets the requirements of subsequent equipment manufacturing. After solution treatment, the steel of the present invention has a good strength level, and the room temperature yield strength (R p0.2 ) and tensile strength (R m ) reached 380MPa and 682MPa respectively; when stretched at 350℃, the yield strength (R p0.2 ) and tensile strength (R m ) reached 338MPa and 656MPa respectively, which is significantly higher than other steel grades. At the test temperature of 20℃ and 350℃, in 10% hydrochloric acid solution, the immersion time is 40h, the corrosion rate is ≤1.90g / (m 2 h) and 2.80g / (m 2 h). The austenitic stainless steel for nuclear power of the present invention takes into account strength, corrosion resistance, high temperature performance and efficient and economical production process. At the same time, the process is simple and stable, the requirements for the rolling system are not high, the rolling cost is low, the operability is strong, and it can better meet the use requirements of various application fields. The steel plate of the invention has stable performance, high safety factor and broad application prospects. DETAILED DESCRIPTION

[0023] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The invention provides a high-temperature corrosion-resistant austenitic stainless steel for nuclear power, the chemical composition of which is as follows by weight percentage: C: 0.04%-0.07%; Si: 2.5%-4.5%; Mn: 1.20%-1.50%; P≤0.015%; S≤0.005%; Ni: 9.0%-12.0%; Mo: 0.85%-1.10%; Cr: 13.0%-15.0%; Ti: 0.02%-0.04%, Ta: 0.15%-0.25%, Mo+Ti+Ta: 1.1%-1.3%, and the balance is Fe and unavoidable impurities.

[0025] The reasons for adopting the above components are as follows:

[0026] C: can significantly improve the strength of steel through solid solution. It is the most basic strengthening element in steel and has a significant impact on the yield strength, tensile strength and welding performance of steel. Part of the carbon in the steel enters the steel matrix to cause solid solution strengthening, and the other part of the carbon will combine with the carbide-forming elements in the alloy elements to form alloy carbides. However, too high a carbon content will cause a variety of negative effects, such as a decrease in the welding performance and corrosion resistance of the steel. According to the use needs and performance requirements, the present invention selects to add a C content of 0.04%-0.07%.

[0027] Si: In the present invention, Si can form a passivation film of SiO2 on the surface of the steel, and at the same time form a composite passivation film with Cr2O3, which increases the pitting potential by inhibiting the cathode reaction. When in a strong oxidizing medium, it can significantly improve the corrosion resistance of the steel. However, if the Si content is too high, it will promote the solute redistribution during the solidification of the alloy, and serious element segregation will occur at the front of the solidification interface, forming an obvious dendrite structure accompanied by the precipitation of a large number of harmful phases, which will not only seriously affect the uniformity of the structure and composition of the ingot, but also weaken the grain boundary strength, leading to cracking in the subsequent rolling process. While increasing the Si content, the present invention uses elements such as Mo, Ti and Ta in combination to exert the beneficial effect of Si and inhibit the formation of delta ferrite. Taking all factors into consideration, the Si content of the present invention is selected in the range of 2.5%-4.5%.

[0028] Mn: It can improve the strength of steel in the form of solid solution strengthening, make up for the deficiency caused by the reduction of C, and is the main alloy element that affects strength, hardenability and weldability, and is also low in cost. However, too high a Mn content has an adverse effect on toughness and high-temperature performance, and is prone to segregation, making the matrix material composition and structure uneven. The present invention adds an appropriate amount of Mn, which, on the one hand, stabilizes austenite, dissolves more carbides into the matrix during high-temperature solid solution, and combines with other strong carbide elements to form carbides, giving full play to the beneficial effects, and on the other hand, avoids adverse effects on material toughness and thermal fatigue resistance. Therefore, the present invention selects the addition of Mn content of 1.20%-1.50%.

[0029] P and S: are harmful elements in the steel of the present invention, which have an adverse effect on the thermoplasticity and corrosion resistance of the steel. P is easy to segregate at the austenite grain boundary, which weakens the atomic bonding force at the grain boundary of the matrix material, resulting in large temper brittleness of the material. S is distributed in the steel in the form of MnS, which will aggravate the anisotropy of the steel and reduce the thermal stability of the steel. In addition, too much S and P will affect the homogeneity and purity of the steel. Therefore, the lower the content, the better. However, considering the steelmaking conditions and costs, the present invention requires that P≤0.015% and S≤0.005% in the steel be controlled.

[0030] Ni: The main synthetic element of stainless steel. Adding an appropriate amount of Ni helps to obtain a single-phase austenite structure, significantly improving corrosion resistance and plasticity. Ni can also work with Cr to form a layer of protective spinel oxide film NiO·Cr2O3 composite oxide film within a certain temperature range, effectively improving the corrosion resistance and high-temperature oxidation resistance of steel. However, excessive Ni will increase the cost on the one hand, and reduce the diffusion rate of carbon in the matrix on the other hand, delaying the dissolution process of undissolved carbides into austenite, reducing the strength. Therefore, the present invention sets its content to 9.0%-12.0%.

[0031] Mo: The role of Mo in the steel of the present invention is to combine with carbon in the steel to form small short rod-shaped Mo2C carbides, which can enhance the strength of the steel by solid solution strengthening. At the same time, it can improve the pitting corrosion resistance of the steel. 2- It dissolves in the form of and is adsorbed on the metal surface to form a passivation film, which increases the pitting potential of the steel and reduces the pitting rate, thereby improving the pitting resistance. At the same time, in the present invention, Ti microalloying and Mo addition have a significant effect on the refinement of the structure. However, too much Mo content will promote the formation of harmful phases such as delta ferrite, resulting in deterioration of the hot working performance of the steel and adverse effects. Therefore, the present invention selects to add Mo content of 0.85%-1.10%.

[0032] Cr: The main alloying element in stainless steel. It interacts with Ni to form a stable austenite structure in the steel, which can passivate the steel and give it good corrosion resistance and stainlessness. When the chromium content in the stainless steel of the present invention exceeds 13%, the steel can have good high-temperature oxidation resistance and corrosion resistance. However, excessive Cr has a high cost and will cause ferrite structure in the steel. Therefore, the present invention selects to add 13.0%-15.0% Cr.

[0033] Ti: used to improve the as-cast structure. Adding a proper amount of Ti to the steel can form Ti carbon and nitride with C and N elements, which has a good grain refinement effect, making the coarse network structure uniform and fine, reducing segregation and improving the quality of the ingot. However, if too much Ti is added, the structure will be coarsened and loose due to dynamic recrystallization, which is not conducive to improving the strength of the steel. The Ti content in the steel of the present invention is designed to be 0.02%-0.04%.

[0034] Ta: It plays a role of solid solution strengthening in steel. In the present invention, Ta exists in the form of carbides and oxide particles, which can refine the grains and improve the strength without affecting the plasticity and toughness of the steel. At the same time, Ta has high chemical stability, strong resistance to liquid metal corrosion, and a large dielectric constant of the surface oxide film, which can improve the high-temperature corrosion resistance of steel. However, too high a content will result in the inability of elements such as Ti and Mo to play their role, so the present invention chooses to add Ta: 0.15%-0.25%.

[0035] The present invention adopts the composite effect of high melting point transition metal elements Mo, Ti and Ta to strengthen the steel, so that it has good high temperature performance and high temperature corrosion resistance. Therefore, the present invention selects to add Mo+Ti+Ta=1.1%-1.3%.

[0036] The present invention discloses a method for manufacturing austenitic stainless steel for nuclear power with high temperature corrosion resistance. The production process of the steel plate is: smelting - continuous casting - homogenization treatment - heating - rolling - heat treatment. The specific contents are as follows:

[0037] (1) Smelting: The smelting of molten steel is completed by three steps of induction furnace + LF + RH. The induction furnace uses industrial pure iron and alloy to complete the melting and composition adjustment. The tapping temperature of the induction furnace is ≥1650℃. LF completes the control of S and the removal of inclusions. RH performs vacuum treatment of molten steel with a vacuum degree of ≤0.2kPa to remove gases such as hydrogen, oxygen and nitrogen.

[0038] (2) Continuous casting: The pouring temperature is 1490-1510℃, and electromagnetic stirring is used at the end of continuous casting. The billet drawing speed is controlled at 1.0-1.3m / min to fully ensure the internal and external quality of the billet. The billet is immediately stacked and slowly cooled for more than 48 hours after it comes off the line. The preferred thickness of the billet is 200-300mm.

[0039] (3) Homogenization treatment: In order to eliminate the element segregation of the ingot, promote the dissolution of the precipitated phase and the ablation of the dendrite, and effectively deal with the problem of thermal deformation and cracking, the ingot is homogenized. The continuous casting ingot is loaded into the furnace and heated with the furnace. The heat treatment system is 1140-1160℃, and the net heat preservation is 10-13h. After the heat preservation is completed, it is cooled with the furnace.

[0040] (4) Heating: The continuous casting slab after homogenization treatment is heated with the furnace, the heating temperature is 1250-1270℃, and the soaking period is in the furnace for 6h-8h. Since metal elements such as Mo, Ti and Ta are added in the present invention, a higher heating temperature is used to fully dissolve the alloy elements, which plays a role in solid solution strengthening. At the same time, a reasonable heating system can improve the non-uniformity of the slab composition during the continuous casting process and reduce internal microsegregation.

[0041] (5) Rolling: The steel plate rolling adopts two-stage controlled rolling. In the first stage, the rolling temperature is 1100-1150℃, and the reduction rate is controlled at 15-20% in the first three passes. The large reduction rate is conducive to the formation of fine and uniform grains and the improvement of center defects. The final rolling temperature is ≥970℃. In the second stage, the rolling temperature is 880-950℃, the final rolling temperature is 780-850℃, and the steel plate thickness is 10-100mm.

[0042] (6) Heat treatment: In order to prevent the corrosion resistance from decreasing due to the reduction of TiC during solution treatment, the steel needs to be heated to a certain temperature so that the C and Ti in the steel form stable TiC without precipitating chromium carbides. The finished steel plate is pretreated after rolling, with a heating temperature of 850-880℃ and a holding time of 4-6h. It is then air-cooled to room temperature after being taken out of the furnace. After that, in order to allow the carbides to fill and melt and be preserved in austenite at room temperature, a single-phase austenite structure is obtained, giving the steel the strongest corrosion resistance. Then, a solid solution heat treatment is carried out at 1100-1140℃, with a holding time of 0.5-4.5h, and it is water-cooled to room temperature after being taken out of the furnace.

[0043] A high temperature corrosion resistant austenitic stainless steel for nuclear power and a manufacturing method thereof, the specific implementation methods are as follows:

[0044] Table 1 shows the components involved in each embodiment, Table 2 shows the process parameters of slab smelting, continuous casting and homogenization heat treatment in the embodiment, Table 3 shows the rolling in the embodiment, Table 4 shows the heat treatment process parameters in each embodiment, Table 5 shows the tensile properties in each embodiment, and Table 6 shows the corrosion resistance of each embodiment after immersion in hydrochloric acid solution at 20°C and 350°C for 40 hours.

[0045] Table 1 Chemical composition of steel smelting in each example (%)

[0046]

[0047] Table 2 Process parameters for smelting, continuous casting and homogenization heat treatment of steel in each example

[0048]

[0049] Table 3 Rolling process parameters of each example steel

[0050]

[0051]

[0052] Table 4 Heat treatment process parameters of each example steel

[0053]

[0054] Table 5 Tensile properties of each embodiment

[0055]

[0056] Table 6 Corrosion resistance of each embodiment at 20℃ and 350℃, 10% hydrochloric acid solution, immersed for 40h

[0057]

[0058]

[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high temperature corrosion resistant austenitic stainless steel for nuclear power, characterized in that: The chemical composition of steel by weight percentage includes C: 0.04%-0.07%; Si: 2.5%-4.5%; Mn: 1.20%-1.50%; P≤0.015%; S≤0.005%; Ni: 9.0%-12.0%; Mo: 0.85%-1.10%; Cr: 13.0%-15.0%; Ti: 0.02%-0.04%; Ta: 0.15%-0.25%, the balance is Fe and unavoidable impurities; room temperature yield strength R p0.2 Reaching more than 380MPa, tensile strength R m Reaching 682MPa or more, elongation A Reach more than 25.5%, and the cross-sectional shrinkage rate Z reaches more than 72%; when stretched at 350℃, the yield strength R p0.2 Reaching more than 338MPa, tensile strength R m Reaching 656MPa or more, elongation A Reach more than 26.5%, and the cross-sectional shrinkage Z reaches more than 72%; the production process includes: smelting, continuous casting, homogenization treatment, heating, rolling, and heat treatment. Among them, homogenization treatment: the continuous casting billet is heated with the furnace, the heating temperature is 1140-1160℃, the net heat preservation is 10-13h, and the furnace is cooled after the heat preservation; heating: the continuous casting billet after homogenization treatment is heated with the furnace, the heating temperature is 1250-1270℃, and the heat soaking section is in the furnace for 6h-8h; rolling: two-stage controlled rolling is adopted, the first In the first stage, the rolling temperature is 1100-1150℃, the average reduction rate of the first three passes is controlled at 15%-20%, and the final rolling temperature is ≥970℃; in the second stage, the rolling temperature is 880-950℃, and the final rolling temperature is 780-850℃; heat treatment: pretreatment is carried out first, the heating temperature is 850-880℃, the holding time is 4-6h, and air cooling to room temperature after being taken out of the furnace; then solution heat treatment is carried out at 1100-1140℃, the holding time is 0.5-4.5h, and water cooling to room temperature after being taken out of the furnace.

2. The high temperature corrosion resistant austenitic stainless steel for nuclear power according to claim 1, characterized in that: Mo+Ti+Ta:1.1%-1.3%.

3. The high temperature corrosion resistant austenitic stainless steel for nuclear power according to claim 1, characterized in that: The thickness of stainless steel plate is 10-100mm.

4. The high temperature corrosion resistant austenitic stainless steel for nuclear power according to claim 1, characterized in that: In the test temperature of 20℃, 10% hydrochloric acid solution, the immersion time is 40h, the corrosion rate is ≤1.90g / (m 2 ·h); Under the conditions of test temperature of 350℃, 10% hydrochloric acid solution, immersion time of 40h, corrosion rate ≤2.80g / (m 2 ·h).

5. According to the method for manufacturing austenitic stainless steel for nuclear power with high temperature corrosion resistance as claimed in claim 1, the production process comprises: Smelting, continuous casting, homogenization, heating, rolling, heat treatment, characterized in that: Homogenization treatment: The continuous casting billet is heated with the furnace, the heating temperature is 1140-1160℃, the net heat preservation is 10-13h, and the billet is cooled with the furnace after the heat preservation is completed; Heating: The continuous casting billet after homogenization treatment is heated with the furnace, the heating temperature is 1250-1270℃, and the soaking period in the furnace is 6h-8h; Rolling: Two-stage controlled rolling is adopted. In the first stage, the starting rolling temperature is 1100-1150℃, the average reduction rate of the first three passes is controlled at 15%-20%, and the final rolling temperature is ≥970℃; in the second stage, the starting rolling temperature is 880-950℃, and the final rolling temperature is 780-850℃; Heat treatment: pretreatment is carried out first, with heating temperature of 850-880℃ and holding time of 4-6h, and air cooling to room temperature after being taken out of the furnace; then solution heat treatment is carried out at 1100-1140℃, with holding time of 0.5-4.5h, and water cooling to room temperature after being taken out of the furnace.

6. The method for manufacturing austenitic stainless steel for nuclear power use resistant to high temperature corrosion according to claim 5, characterized in that: The smelting adopts induction furnace + LF + RH. The induction furnace uses industrial pure iron and alloy to complete the melting and composition adjustment. The steel-making temperature of the induction furnace is ≥1650℃. LF completes the control of S and the removal of inclusions. RH performs vacuum treatment of molten steel with a vacuum degree of ≤0.2kPa.

7. The method for manufacturing austenitic stainless steel for nuclear power use resistant to high temperature corrosion according to claim 5, characterized in that: The continuous casting pouring temperature is controlled at 1490-1510℃, and the pulling speed is controlled at 1.0-1.3m / min.

8. The method for manufacturing austenitic stainless steel for nuclear power use resistant to high temperature corrosion according to claim 5, characterized in that: The ingots are immediately stacked and slowly cooled after coming off the production line, with the slow cooling time being more than 48 hours.

9. The method for manufacturing austenitic stainless steel for nuclear power use resistant to high temperature corrosion according to claim 5, characterized in that: The thickness of continuous casting slab is 200-300mm.

Citation Information

Cited By

  • Niobium-containing 304 austenitic stainless steel plate for nuclear power and preparation method thereof

    CN121780997A