Silicon carbide composite ceramic material for ceramic probe and preparation method thereof
By using specific silicon nitride, silicon carbide and metal oxides in ceramic probe materials, the problems of uneven resistivity and poor high temperature resistance and poor stability are solved, and high conductivity and long life are achieved ceramic probe material.
Patent Information
- Application Number
- CN202310497297.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-05-05
AI Technical Summary
Existing conductive ceramic materials have problems such as uneven resistivity, low conductivity, high temperature resistance and poor chemical stability, especially in ceramic probe applications, which are difficult to meet high requirements.
By using specific raw material components such as silicon nitride, silicon carbide, etc., and adding specific metal oxides and binders, the silicon carbide ceramic material produced has a dense structure, uniform particle size, uniform resistivity and high conductivity and has high chemical stability, good wear resistance and strong high temperature resistance.
The high conductivity, long service life and good mechanical properties of ceramic probe materials are achieved, with a conductivity of 3-4.5×10-2S/cm, good hardness, high temperature resistance and chemical stability are significantly improved.
Smart Images

Figure BDA0004212628880000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic materials, and specifically designs a silicon carbide composite ceramic material for a ceramic probe and a preparation method thereof. Background Art
[0002] Conductive ceramics refer to ceramics that have electronic (or hole) conductivity or ionic conductivity under certain conditions (temperature, pressure). Conductive ceramics belong to new functional special ceramics and are a type of basic materials. They have various properties of ceramics, such as oxidation resistance, high temperature resistance, corrosion resistance, low cost, good mechanical properties, etc., and have the conductive properties of metal. Its resistivity can be adjusted within a large range, so it is used in many special environments and occasions, such as modern national defense and national economy, in evaporation boats used in aluminum plating industry, pantographs of high-speed trains, solid fuel cell electrodes, gas sensors, electric spark machining and many other fields, which are unmatched by other materials.
[0003] Chinese patent 201510628153.5 discloses a conductive ceramic, and the present invention discloses a conductive ceramic material and a preparation method thereof, wherein the conductive ceramic material is made of the following components in parts by weight: 65-70 parts of aluminum oxide, 25-30 parts of spodumene, 5-8 parts of ferrite, 2-5 parts of titanium carbide, 2-3 parts of antimony trioxide, 1-2 parts of nano silicon carbide powder, 1-2 parts of polyaluminum iron silicate, 0.5-1 parts of strontium carbonate, 0.5-1 parts of tetrabutyl titanate, and 0.02-0.8 parts of ammonium persulfate. The present invention also provides a method for preparing a conductive ceramic material. However, the material has problems such as uneven resistivity, low conductivity, poor high temperature resistance and chemical stability.
[0004] Chinese invention patent CN03139036.6 discloses a conductive ceramic, which is obtained by adding non-metallic conductive materials to a ceramic base material and firing it at high temperature to obtain a ceramic material with a conductive layer in the middle layer. However, the material has problems such as uneven resistivity, easy moisture absorption, and fast aging at high temperature. Summary of the invention
[0005] In view of the above problems, the present invention provides a silicon carbide composite ceramic material for ceramic probes. The silicon carbide ceramic material is prepared by compounding specific raw material components such as silicon nitride and silicon carbide, and adding specific metal oxides and binders and other components. The silicon carbide ceramic material has the advantages of dense structure, uniform particle size, uniform resistivity, and high conductivity; it also has high chemical stability, good wear resistance, strong high temperature resistance, and long service life.
[0006] The invention provides a silicon carbide composite ceramic material for a ceramic probe. The raw materials include 30-50 parts of silicon nitride, 40-60 parts of silicon carbide, 5-8 parts of metal oxide, 3-5 parts of aluminum nitride and 5-15 parts of a binder by weight.
[0007] Preferably, the silicon nitride is silicon nitride with a particle size D50 of 100 nm to 1.0 μm and silicon nitride with a particle size of 1 nm to 100 nm.
[0008] More preferably, the mass ratio of the silicon nitride with a particle size D50 of 100 nm to 1.0 μm to the silicon nitride with a particle size of 1 nm to 100 nm is 3-5:1.
[0009] Preferably, the silicon carbide has a particle size of 200-400 mesh.
[0010] Preferably, the metal oxide is a mixture of one or more of magnesium oxide, aluminum oxide, yttrium oxide and cerium oxide.
[0011] More preferably, the metal oxide is yttrium oxide.
[0012] Preferably, the particle size d50 of the yttrium oxide is less than 1 micron.
[0013] Preferably, the mass ratio of silicon nitride to yttrium oxide is 5-8:1.
[0014] The inventors found in experiments that when specific silicon nitride and silicon carbide are used together, especially when yttrium oxide is added at the same time, the density and conductivity of the ceramic material can be effectively improved, and the resulting ceramic material has excellent strength, toughness and conductivity. The inventors analyzed that this may be because when using silicon nitride-doped silicon carbide materials, N atoms will preferentially occupy the position of C atoms, forming a positive charge and an excess valence electron. The excess valence electrons are bound around the positive charge, but only a small amount of energy is needed to break the bondage, allowing the valence electrons to become conductive electrons that move freely in the lattice, and the N atom that loses a valence electron will become N + This makes silicon carbide conductive and reduces the resistivity of the material.
[0015] At the same time, the inventors found that the conductivity can be further improved, especially when yttrium oxide is added and the mass ratio of silicon nitride and yttrium oxide is 5-8:1. This may be because the silicon nitride and yttrium oxide added at the same time can always cause the phase transition of the β phase to the α phase of silicon carbide in the ceramic material, thereby reducing the resistivity. However, if the content of silicon nitride or yttrium oxide is too high, it will affect the mechanical properties such as strength and toughness of silicon carbide. The inventors analyzed that it may be because if the content of yttrium oxide is too high, it will cause the grains to grow and secondary crystallization will occur, affecting the density and particle size uniformity of the ceramic material, thereby affecting its strength and other mechanical properties.
[0016] Preferably, the binder is a mixture of one or more of PVA, PVB, epoxy resin, phenolic resin and cellulose.
[0017] Preferably, the adhesive is epoxy resin.
[0018] Preferably, the silicon carbide composite ceramic material for the ceramic probe further contains titanium carbide.
[0019] Preferably, the titanium carbide is 20-30 parts.
[0020] Further preferably, the purity of the titanium carbide is greater than 98% and the particle size is less than 10 μm.
[0021] A second aspect of the present invention provides a method for preparing a silicon carbide composite ceramic material for a ceramic probe, the specific steps of which are as follows:
[0022] S1, mixing: dissolving the raw materials except the binder in ethanol, performing ball milling, and drying the slurry obtained by ball milling to obtain a mixed material;
[0023] S2, molding: dissolving the mixture and the binder in ethanol, mixing and stirring to obtain a mixed slurry; injecting the mixed slurry into a mold, and demolding after drying to obtain a ceramic material embryo;
[0024] S3, sintering: placing the green body to be sintered into a sintering furnace, heating it to 1800-2300° C., keeping it warm for 3-6 hours, and cooling it to obtain the ceramic material.
[0025] Preferably, in step S1, the ball milling rate is 1000-1800 r / min, and the ball milling time is 1-5 h.
[0026] Preferably, the sintering step of step S3 is specifically as follows: placing the green embryo into a sintering furnace, evacuating to a pressure of <20Pa; sintering at a high temperature under a protective atmosphere; first heating to 280-320°C, with a pressure of 1-2MPa, keeping warm for 2-3h, and a heating rate of 80°C / h; then heating to 1200-1500°C, keeping warm for 2-3h, pressurizing to 2-3MPa, and a heating rate of 150°C / h; then heating to 1800-2300°C, pressurizing to 3-5MPa, keeping warm for 3-6h, with a heating rate of 50°C / h, and a pressure of 2-4MPa; cooling to 800°C, with a cooling rate of 120°C / h; and finally naturally cooling to obtain the conductive silicon carbide composite ceramic.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The present invention uses specific raw materials such as silicon nitride and silicon carbide to compound, and adds specific metal oxides and binders to obtain silicon carbide ceramic materials with the advantages of dense structure, uniform particle size, uniform resistivity, and high conductivity; and has high chemical stability, good wear resistance, high temperature resistance, and long service life. The ceramic material obtained by the present invention has good hardness and a conductivity of 3-4.5×10-2 S / cm. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be noted that the following embodiments are further descriptions of the present invention, rather than limitations of the present invention.
[0030] Example
[0031] Example 1
[0032] The present embodiment provides a silicon carbide composite ceramic material for a ceramic probe, which includes, by weight, 40 parts of silicon nitride, 50 parts of silicon carbide, 6 parts of metal oxide, 4 parts of aluminum nitride, 10 parts of a binder, and 25 parts of titanium carbide.
[0033] The silicon nitride is silicon nitride with a particle size D50 of 500 nm and silicon nitride with a particle size D50 of 500 nm and a mass ratio of silicon nitride with a particle size D50 of 500 nm and silicon nitride with a particle size D50 of 500 nm and a particle size D50 of 50 nm, which is 4:1. The silicon nitride is purchased from Forsman Technology (Beijing) Co., Ltd.
[0034] Silicon carbide was 300-mesh silicon carbide purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.
[0035] The metal oxide is yttrium oxide; the particle size d50 of the yttrium oxide is less than 1 micron.
[0036] The adhesive is epoxy resin E51.
[0037] The purity of titanium carbide is greater than 98%, and the particle size is less than 10 μm; it was purchased from Hunan Huasheng Technology Co., Ltd.
[0038] A second aspect of this embodiment provides a method for preparing a silicon carbide composite ceramic material for a ceramic probe, and the specific steps are as follows:
[0039] S1, mixing: dissolving the raw materials except the binder in ethanol, ball milling for 1-5 hours at a ball milling rate of 1000-1800 r / min, and drying the slurry obtained by ball milling to obtain a mixed material;
[0040] S2, molding: dissolving the mixture and the binder in ethanol, mixing and stirring to obtain a mixed slurry; injecting the mixed slurry into a mold, and demolding after drying to obtain a ceramic material embryo;
[0041] S3, sintering: put the green embryo into a sintering furnace, evacuate to a pressure of <20Pa; sinter under a protective atmosphere; first heat to 300°C, pressure of 1.5MPa, keep warm for 2h, heating rate of 80°C / h; then heat to 1300°C, keep warm for 2h, pressurize to 3MPa, heating rate of 150°C / h; then heat to 2000°C, pressurize to 4MPa, keep warm for 5h, heating rate of 50°C / h, pressure of 4MPa; cool to 800°C, cooling rate of 120°C / h; then cool naturally to obtain the conductive silicon carbide composite ceramic.
[0042] Example 2
[0043] The present embodiment provides a silicon carbide composite ceramic material for a ceramic probe, which includes, by weight, 30 parts of silicon nitride, 40 parts of silicon carbide, 5 parts of metal oxide, 3 parts of aluminum nitride, 5 parts of binder, and 20 parts of titanium carbide.
[0044] The silicon nitride is silicon nitride with a particle size D50 of 500 nm and silicon nitride with a particle size D50 of 500 nm and a mass ratio of silicon nitride with a particle size D50 of 500 nm and silicon nitride with a particle size D50 of 500 nm and a particle size D50 of 50 nm, which is 4:1. The silicon nitride is purchased from Forsman Technology (Beijing) Co., Ltd.
[0045] Silicon carbide was 300-mesh silicon carbide purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.
[0046] The metal oxide is yttrium oxide; the particle size d50 of the yttrium oxide is less than 1 micron.
[0047] The adhesive is epoxy resin E51.
[0048] The purity of titanium carbide is greater than 98%, and the particle size is less than 10 μm; it was purchased from Hunan Huasheng Technology Co., Ltd.
[0049] A second aspect of this embodiment provides a method for preparing a silicon carbide composite ceramic material for a ceramic probe, and the specific steps are the same as those of the first embodiment.
[0050] Example 3
[0051] The present embodiment provides a silicon carbide composite ceramic material for a ceramic probe, which includes, by weight, 50 parts of silicon nitride, 60 parts of silicon carbide, 8 parts of metal oxide, 5 parts of aluminum nitride, 15 parts of a binder, and 30 parts of titanium carbide.
[0052] The silicon nitride is silicon nitride with a particle size D50 of 500 nm and silicon nitride with a particle size D50 of 500 nm and a mass ratio of silicon nitride with a particle size D50 of 500 nm and silicon nitride with a particle size D50 of 500 nm and a particle size D50 of 50 nm, which is 4:1. The silicon nitride is purchased from Forsman Technology (Beijing) Co., Ltd.
[0053] Silicon carbide was 300-mesh silicon carbide purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.
[0054] The metal oxide is yttrium oxide; the particle size d50 of the yttrium oxide is less than 1 micron.
[0055] The adhesive is epoxy resin E51.
[0056] The purity of titanium carbide is greater than 98%, and the particle size is less than 10 μm; it was purchased from Hunan Huasheng Technology Co., Ltd.
[0057] A second aspect of this embodiment provides a method for preparing a silicon carbide composite ceramic material for a ceramic probe, and the specific steps are the same as those of the first embodiment.
[0058] Comparative Example 1
[0059] This embodiment provides a silicon carbide composite ceramic material for a ceramic probe. The specific implementation method is the same as that of Embodiment 1. The difference from Embodiment 1 is that the metal oxide accounts for 10 parts.
[0060] A second aspect of this embodiment provides a method for preparing a silicon carbide composite ceramic material for a ceramic probe, and the specific steps are the same as those of the first embodiment.
[0061] Comparative Example 2
[0062] This embodiment provides a silicon carbide composite ceramic material for a ceramic probe. The specific implementation method is the same as that of Embodiment 1. The difference from Embodiment 1 is that no metal oxide is added.
[0063] A second aspect of this embodiment provides a method for preparing a silicon carbide composite ceramic material for a ceramic probe, and the specific steps are the same as those of the first embodiment.
[0064] Comparative Example 3
[0065] This embodiment provides a silicon carbide composite ceramic material for a ceramic probe. The specific implementation method is the same as that of Embodiment 1. The difference from Embodiment 1 is that the titanium carbide is 10 parts and the particle size is 20 μm.
[0066] A second aspect of this embodiment provides a method for preparing a silicon carbide composite ceramic material for a ceramic probe, and the specific steps are the same as those of the first embodiment.
[0067] Comparative Example 4
[0068] This embodiment provides a silicon carbide composite ceramic material for a ceramic probe. The specific implementation method is the same as that of Embodiment 1. The difference from Embodiment 1 is that the silicon nitride has a particle size D50 of 1 nm to 100 nm.
[0069] A second aspect of this embodiment provides a method for preparing a silicon carbide composite ceramic material for a ceramic probe, and the specific steps are the same as those of the first embodiment.
[0070] Performance Testing
[0071] 1. Hardness test: Use Vickers hardness tester to perform hardness test.
[0072] 2. Four-point bending strength test: measured in accordance with the test standard ISO14704:2016.
[0073] 3. Conductivity: The four-probe tester collects test data in real time under two combined modes. The collected data is analyzed by computer to obtain the required test results.
[0074] 4. Thermal expansion coefficient: Tested according to GB / T16535-1996 test method.
[0075] The silicon carbide composite ceramic materials of Examples 1-3 and Comparative Examples 1-4 were subjected to the above performance tests, and the test results are shown in Table 1 below.
[0076] Table 1
[0077]
Claims
1. A silicon carbide composite ceramic material for a ceramic probe, It is characterized in that In parts by weight, the raw materials include 30-50 parts of silicon nitride, 40-60 parts of silicon carbide, 5-8 parts of metal oxide, 3-5 parts of aluminum nitride, and 5-15 parts of binder; The silicon nitride includes silicon nitride with a particle size of 100nm~1.0μm and 1nm~100nm; the mass ratio of the silicon nitride with a particle size of 100nm~1.0μm and 1nm~100nm is 3-5:1; The metal oxide is yttrium oxide, and the mass ratio of silicon nitride to yttrium oxide is 5-8:1; The raw material also includes 20-30 parts of titanium carbide, and the particle size of the titanium carbide is less than 10 μm; The electrical conductivity of the silicon carbide composite ceramic material is 3-4.5×10 -2 S / cm.
2. The silicon carbide composite ceramic material for a ceramic probe according to claim 1, It is characterized in that The binder is a mixture of one or more of PVA, PVB, epoxy resin, phenolic resin and cellulose.
3. The method for preparing the silicon carbide composite ceramic material for ceramic probes according to claim 1 or 2, It is characterized in that The specific steps are as follows: S1, mixing: dissolving the raw materials except the binder in ethanol, performing ball milling, and drying the slurry obtained by ball milling to obtain a mixed material; S2, molding: dissolving the mixture and the binder in ethanol, mixing and stirring to obtain a mixed slurry; injecting the mixed slurry into a mold, and demolding after drying to obtain a ceramic material embryo; S3, sintering: placing the green body to be sintered into a sintering furnace, heating it to 1800-2300° C., keeping it warm for 3-6 hours, and cooling it to obtain the ceramic material.