A luminescent material, a preparation method thereof and an LED luminescent device containing the material

Through the chemical composition and synthesis process of A0.75M11D17.25:xEu2+,yMn2+, the problems of narrow band and insufficient quantum yield of existing green light-emitting materials are solved, and efficient narrow-band green light emission and stable LED luminescence performance are achieved.

CN116731716BActive Publication Date: 2024-10-01XIAMEN INST OF RARE EARTH MATERIALS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210195614.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-01
Publication Date
2024-10-01
Estimated Expiration
2042-03-01

AI Technical Summary

Technical Problem

Existing green light-emitting materials have insufficient narrowband and quantum yield, and poor stability at high temperatures and high humidity, making it difficult to meet the needs of LED light-emitting devices.

Method used

Using the chemical composition of A0.75M11D17.25:xEu2+,yMn2+, the luminescent material is synthesized through pre-calcination and calcination steps, using Eu2+ and Mn2+ as luminescent center ions, controlling the flux content to adjust the excitation spectrum, achieving narrow-band green light emission and high-efficiency quantum Yield.

Benefits of technology

It achieves narrow-band blue and green light emission, with an internal quantum yield of 95% and an external quantum yield of 75%. It also has excellent thermal stability and high temperature and high humidity stability, making it suitable for widespread use in LED light-emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116731716B_ABST
    Figure CN116731716B_ABST
Patent Text Reader

Abstract

The present invention discloses a luminescent material, characterized in that the chemical composition of the luminescent material is A 0.75 M 11 D 17.25 :xEu 2+ ,yMn 2+ ; wherein, A is one, two or more of Be, Mg, Ca, Sr, Ba, Li, Na, K, Rb, Cs, M is one, two or more of B, Al, Ga, In, Ti, Sc, C, Si, Ge, Sn, Pb, D is one, two or more of O, S, Se, Te, N, P, As, F, Cl, Br, I, Eu 2+ and Mn 2+ are luminescent center ions, 0 at.% ≤ x ≤ 100 at.%; 0 at.% < y ≤ 100 at.%. The luminescent material of the present invention uses Eu 2+ and Mn 2+ as luminescent center ions, can be effectively excited in the range of ultraviolet and blue light, emits blue light at 450 nm and green light at 515 nm, the full width at half maximum of the blue light is 50 nm, and the full width at half maximum of the green light is 27 nm, solving the problem that the emission wavelength of the existing green luminescent material is not narrow enough.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of luminescent materials, and in particular, relates to a luminescent material, a preparation method thereof and an LED luminescent device comprising the material. Background Art

[0002] As a new generation of solid-state light sources, phosphor conversion LEDs have the advantages of energy saving, environmental protection, and high efficiency, and have been widely used in lighting, display, and detection. At present, there are two main preparation routes for phosphor conversion LEDs. One is to coat red and green light luminescent materials with blue light chips to make white light LEDs; the other is to coat red, green, and blue light luminescent materials with purple light chips to make white light LEDs. This means that more types of high-quality luminescent materials are needed to meet the needs of different LED devices. High-quality luminescent materials usually need to meet the following requirements: 1. High luminous intensity; 2. Good thermal stability; 3. Good high temperature and high humidity stability; 4. High quantum yield. At present, narrow-band green light materials are still relatively scarce among luminescent materials, so the research and development of narrow-band green light luminescent materials is of great significance for LED luminescence.

[0003] In the β-alumina material system, CN201680017262.6 reported a series of green light emitting materials containing halogen elements or nitrogen elements, which can be excited in the ultraviolet region to achieve green light emission with a peak value of about 520nm; the current commercial green light emitting material β-SiAlON:Eu 2+ The emission peak is 540nm and the half-height width is 54nm. Due to the large half-height width, the color gamut area of ​​the LED device made using this luminescent material is not ideal (Chemistry of Materials, 2018, 30(2):494-505); In addition, Eu 2+ Doped alkali metal lithium silicates achieve narrow-band green light emission, but their quantum yield and high temperature and high humidity stability limit their further applications (Advanced Optical Materials, 2019, 7(6):1801631). 2+ Doped aluminate luminescent materials due to Mn 2+ The emission belongs to a spin-forbidden transition, resulting in a low quantum yield (Advanced Optical Materials, 2019, 7(6): 1801419). Therefore, it is urgent to develop a luminescent material that emits narrow-band green light and has both high quantum yield and stability. Summary of the invention

[0004] The present invention provides a luminescent material, the chemical composition of the luminescent material is A 0.75 M 11 D 17.25 :xEu2+ ,yMn 2+ ;

[0005] Wherein, A is one, two or more of Be, Mg, Ca, Sr, Ba, Li, Na, K, Rb, Cs, M is one, two or more of B, Al, Ga, In, Ti, Sc, C, Si, Ge, Sn, Pb, D is one, two or more of O, S, Se, Te, N, P, As, F, Cl, Br, I, Eu 2+ and Mn 2+ is the luminescent central ion, 0at.%≤x≤100at.%; 0at.% <y≤100at.%。

[0006] According to the technical solution of the present invention, A is one, two or more of Be, Mg, Ca, Sr, Ba, Li, Na, K, Rb, and Cs, and is preferably at least one of Be, Sr, Ba, Mg, and Ca.

[0007] According to the technical solution of the present invention, M is one, two or more of B, Al, Ga, In, Ti, Sc, C, Si, Ge, Sn, and Pb, and is preferably at least one of B, Al, Ga, and In.

[0008] According to the technical solution of the present invention, D is one, two or more of O, S, Se, Te, N, P, As, F, Cl, Br, and I, and is preferably at least one of O and S.

[0009] According to the technical solution of the present invention, x represents Eu 2+ The amount of substitution of the lattice site of A, and the substitution amount, that is, the range of x can be 0at.% to 100at.%, and further, the range of x can be 0.01at.%≤x≤80at.%, such as 0.01at.%≤x≤10at.%, or 0.1at.%≤x≤20at.%, or 1at.%≤x≤30at.%, preferably 2at.%≤x≤20at.%, and more preferably 4at.%≤x≤12at.%. y represents Mn 2+ The amount of replacing the lattice position of M, and the range of the substitution amount, i.e., y, can be greater than 0 at.% to 100 at.%, further, the range of y can be 0.01 at.% ≤ y ≤ 90 at.%, for example, 0.01 at.% ≤ y ≤ 20 at.%, or 0.5 at.% ≤ y ≤ 40 at.%, or 10 at.% ≤ y ≤ 60 at.%, preferably 5 at.% ≤ y ≤ 20 at.%.

[0010] According to the technical solution of the present invention, the chemical composition of the luminescent material can be Be 0.75 B11 THE 17.25 :10%I 2 + ,20%Mn 2+ 、Be 0.75 Al 11 THE 17.25 :12%I 2+ ,23%Mn 2+ 、Be 0.75 Ga 11 THE 17.25 :15%I 2+ ,21%Mn 2+ 、Mg 0.75 B 11 THE 17.25 :11%I 2+ ,22%Mn 2+ 、Mg 0.75 Al 11 THE 17.25 :17%I 2+ ,28%Mn 2+ ,Here 0.75 B 11 THE 17.25 :25%Me 2+ ,51%Mn 2+ ,Here 0.75 Al 11 THE 17.25 :13%I 2+ ,24%Mn 2+ 、Sr 0.75 B 11 THE 17.25 :14%I 2+ ,27%Mn 2+ 、Sr 0.75 Al 11 THE 17.25 :16%I 2+ ,21%Mn 2+ 、Ba 0.75 B 11 THE 17.25 :32%I 2+ ,46%Mn 2+ 、Ba 0.75 In 11 S 17.25 :12%I 2+ ,36%Mn 2+ 、Ba 0.75 Al 11 THE 17.25 :25%Me 2+ ,56%Mn 2+ 、Ba 0.75Al 11 O 17.25 :8%Eu 2+ ,6%Mn 2+ , Sr 0.75 B 11 O 17.25 :4%Eu 2+ ,8%Mn 2+ Mg 0.75 In 11 O 17.25 :2%Eu 2+ ,5%Mn 2+ , Ca 0.75 Ga 11 O 17.25 :9%Eu 2+ ,15%Mn 2+ , Sr 0.75 In 11 O 17.25 :3%Eu 2+ ,12%Mn 2+ , Ca 0.75 B 11 O 17.25 :14%Eu 2+ ,24%Mn 2+ Mg 0.75 Ga 11 O 17.25 :6%Mn 2+ .

[0011] According to the technical solution of the present invention, the luminescent material is a powder with an average particle size of 5-40 μm, such as 5-20 μm or 10-30 μm or 20-30 μm.

[0012] According to the technical solution of the present invention, the luminescent material can be excited by violet light and / or blue light, for example, by light in the range of 200-480nm, preferably, by light in the range of 300-400nm, illustratively, can be excited by 365nm, 380nm violet light.

[0013] According to the technical solution of the present invention, the luminescent material has narrow-band blue and green light emission properties, for example, it can emit blue light with a wavelength of 450nm and a half-width of 50nm and green light with a wavelength of 515nm and a half-width of 27nm.

[0014] According to the technical solution of the present invention, the internal quantum yield of the luminescent material of the present invention can reach 95%, the external quantum yield can reach 75%, and the absorption efficiency can reach 79%.

[0015] According to the technical solution of the present invention, the luminescent material of the present invention has excellent thermal stability, and the integrated luminescence intensity at 200° C. remains the same as the initial intensity.

[0016] According to the technical solution of the present invention, the luminescent material of the present invention has excellent high temperature and high humidity stability. After aging for seven days at 85°C and 85% humidity, the luminescent intensity and quantum efficiency of the luminescent material remain unchanged compared with the initial values.

[0017] The present invention also provides a method for preparing the luminescent material, which comprises the following steps:

[0018] (1) According to chemical formula A 0.75 M 11 D 17.25 :xEu 2+ ,yMn 2+ The raw materials of the compound containing the A element, the compound containing the M element, the compound containing the Eu element, the compound containing the Mn element, and the flux are mixed to obtain a mixture according to the stoichiometric ratio of the elements in the mixture;

[0019] (2) pre-calcining the mixture obtained in step (1) under an air atmosphere to obtain a pre-calcined product;

[0020] (3) calcining the pre-calcined product obtained in step (2) under a reducing atmosphere to obtain the luminescent material.

[0021] According to the technical solution of the present invention, in step (1), at least one compound among the compound containing element A, the compound containing element M, optionally the compound containing element Eu, the compound containing element Mn, and the flux contains element D.

[0022] According to the technical solution of the present invention, in step (1), the compound containing element A is selected from at least one of carbonates containing element A, oxides containing element A, nitrides containing element A, halides containing element A, nitrates containing element A, sulfides containing element A, sulfates containing element A, oxalates containing element A, gallates containing element A, germanates containing element A, selenides containing element A, and tellurides containing element A; preferably at least one of carbonates containing element A and oxides containing element A, exemplified by at least one of BaO, BaCO3, SrO, SrCO3, MgO, MgCO3, CaCO3, and CaO.

[0023] According to the technical solution of the present invention, in step (1), the compound containing the M element is selected from at least one of carbonates containing the M element, oxides containing the M element, nitrides containing the M element, halides containing the M element, nitrates containing the M element, sulfides containing the M element, sulfates containing the M element, oxalates containing the M element, gallates containing the M element, germanates containing the M element, selenides containing the M element, and tellurides containing the M element; preferably, it is an oxide containing the M element, exemplarily at least one of Al2O3, H3BO3, In2O3, and Ga2O3.

[0024] According to the technical solution of the present invention, the compound containing the Eu element can be selected from the oxide of the Eu element, such as Eu2O3.

[0025] According to the technical solution of the present invention, the compound containing the Mn element can be selected from at least one of the oxide and carbonate of the Mn element, such as MnO2 or MnCO3.

[0026] According to the technical solution of the present invention, the mixed material in step (1) is preferably prepared in a mortar or a ball mill, or by dissolving the raw materials in a solvent. Preferably, the solvent is at least one of ethanol, propanol, and isopropanol.

[0027] According to the technical solution of the present invention, in step (1), the flux is selected from at least one of alkali metal carbonates, alkali metal or alkaline earth metal halides, ammonium ion carbonates or fluorides, boric acid, etc., preferably alkali metal carbonates or alkali metal halides; for example, the flux is selected from Li2CO3, K2CO3, LiCl, NH4F, AlF3, BaF2, SrF2, CaF2, NaF, KF, etc., preferably Li2CO3 or LiCl.

[0028] The amount of the flux is 0.1-50wt.%, for example 1-30wt.%, preferably 10-30wt.%, of the total mass of the raw materials in step (1), and is exemplarily 0.1wt.%, 1wt.%, 10wt.%, 15wt.%, 20wt.%, 25wt.%, 30wt.%, 35wt.%, 40wt.% or 50wt.%.

[0029] According to the technical solution of the present invention, by adding flux and controlling its content, a wider and stronger excitation spectrum can be obtained, for example, the strongest excitation peak is red-shifted, and the excitation intensity is increased by about 3 times.

[0030] According to the technical solution of the present invention, in step (2), the pre-calcination temperature is 500°C-2000°C, preferably 600-1800°C, more preferably 1000-1500°C, exemplarily 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1200°C, 1400°C, 1600°C, 1800°C or 2000°C; the pre-calcination time is 1-60h, preferably 3-20h, more preferably 4-16h. Exemplarily, pre-calcination is performed at 1400°C for 8h.

[0031] Exemplarily, in step (2), pre-calcination is carried out in a high-temperature furnace; preferably, pre-calcination is carried out in a muffle furnace.

[0032] According to an embodiment of the present invention, in step (2), the mixed material is placed in a boron nitride or alumina or graphite crucible, and then placed in a high-temperature furnace for pre-calcination, preferably a muffle furnace.

[0033] According to an embodiment of the present invention, in step (2), after the pre-calcination is completed, a cooling treatment is performed; illustratively, it can be naturally cooled to room temperature.

[0034] According to the technical solution of the present invention, in step (3), the calcination temperature is 500°C-2000°C, preferably 600-1800°C, more preferably 1000-1500°C, exemplarily 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1200°C, 1400°C, 1600°C, 1800°C or 2000°C; the calcination time is 1-60h, preferably 3-20h, more preferably 4-16h. Exemplarily, calcination is performed at 1400°C for 8h.

[0035] According to an embodiment of the present invention, in step (3), the pre-calcined product in step (2) is calcined in a high temperature furnace, preferably an atmosphere furnace.

[0036] According to an embodiment of the present invention, in step (3), the reducing atmosphere is a reducing atmosphere such as H2, CO, etc.

[0037] According to an embodiment of the present invention, in step (3), the calcined product is cooled to obtain the luminescent material, for example, naturally cooled to room temperature.

[0038] According to an embodiment of the present invention, the number of calcinations is at least one, for example, two, three or more times. Before the next calcination, the calcined product of the previous time may be ground. Preferably, the temperature and time of each calcination are within the temperature and time ranges defined above, and more preferably, the specific temperature and specific time of each calcination may be the same or different.

[0039] According to an embodiment of the present invention, in step (3), the calcined product may be subjected to post-treatment, and the post-treatment may include grinding the calcined product and sieving and grading the ground product. Further, the post-treatment may include washing, centrifuging and drying the sieving and grading product in sequence.

[0040] Furthermore, the calcined block sample has an irregular morphology, a large particle size, and an uneven particle size distribution. The grinding time is preferably 30 minutes to 1 hour. After grinding, a luminescent material with a regular morphology, a small particle size, and a uniform particle size distribution can be obtained.

[0041] The present invention also provides a light-emitting device, which includes an excitation light source and at least one fluorescence conversion layer, wherein the fluorescence conversion layer contains at least one of the luminescent materials.

[0042] Preferably, the excitation light source is an LED chip, wherein the emission peak wavelength of the LED chip is 200-480nm, preferably 300-400nm.

[0043] According to an embodiment of the present invention, the number of the fluorescence conversion layer is 1, for example, the fluorescence conversion layer absorbs the primary light emitted by the excitation light source and converts it into secondary light with a longer wavelength.

[0044] According to an embodiment of the present invention, in addition to the luminescent material described in the present invention, the fluorescent conversion layer may also include other luminescent materials, and the other luminescent materials may be K2TiF6:Mn 4+ or K2SiF6:Mn 4+ And other fluoride luminescent materials.

[0045] According to an embodiment of the present invention, the fluorescence conversion layer is coated on an LED chip, and the LED chip is used to carry the fluorescence conversion layer.

[0046] According to an embodiment of the present invention, the fluorescent conversion layer may further include an encapsulant, wherein the luminescent material is uniformly dispersed in the encapsulant. The encapsulant may be epoxy resin, polycarbonate or silicone; preferably silicone. There is no particular limitation on the amount of the encapsulant, as long as it can be uniformly applied to the LED chip according to known operations in the art.

[0047] Furthermore, the fluorescent conversion layer includes the luminescent material and K2TiF6:Mn 4+ or K2SiF6:Mn 4+ For example, the fluorescent conversion layer includes the luminescent material and K2TiF6:Mn 4+ .

[0048] According to an embodiment of the present invention, the light emitting device may further include a base, and the base is used to fix the fluorescent conversion layer. Exemplarily, the base is a packaging substrate.

[0049] Beneficial effects of the present invention:

[0050] 1. The present invention provides a luminescent material, comprising Eu 2+ and Mn 2+ It is the luminescent central ion, which can be effectively excited in the range of purple and blue light, emitting 450nm blue light and 515nm green light. The half-width of blue light is 50nm, and the half-width of green light is 27nm, which solves the problem that the emission wavelength of existing green light luminescent materials is not narrow enough.

[0051] 2. The luminescent material provided by the present invention can regulate the excitation spectrum of the luminescent material, that is, the excitation spectrum of the luminescent material can be regulated by controlling the content of the added flux during synthesis, so that the excitation range is widened and the absorption of the excitation light is strengthened.

[0052] 3. The luminescent material provided by the present invention can be synthesized by a high-temperature solid-phase method, and the required equipment is simple, easy to operate, and low-cost. It can be industrially produced in large quantities, can generate huge social and economic benefits, and is suitable for widespread promotion and use.

[0053] 4. The luminescent material proposed in the present invention has an internal quantum yield of 95%, an external quantum yield of 75%, and an absorption efficiency of 79%; it has excellent thermal stability, and the integrated luminescence intensity at 200°C remains the same as the initial intensity; it also has excellent high-temperature and high-humidity stability. After aging for seven days at 85°C and 85% humidity, the luminescence intensity and quantum efficiency of the luminescent material remain unchanged compared to the initial values, so it has the advantages of high efficiency, energy saving and environmental protection.

[0054] 5. The present invention is based on rare earth ion Eu 2+ and transition metal ions Mn 2+ The efficient energy transfer between the two obtains a luminescent material that emits narrow-band green light, which has the characteristics of high quantum yield and good thermal stability. At the same time, the LED device containing the luminescent material has a wide color gamut value. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 This is the X-ray diffraction (XRD) pattern of the luminescent material prepared in Example 1.

[0056] Figure 2 This is a scanning electron microscope (SEM) image of the luminescent material prepared in Example 1.

[0057] Figure 3 These are the excitation spectrum and emission spectrum of the luminescent material prepared in Example 1.

[0058] Figure 4 It is a comparison chart of the excitation spectra of the luminescent materials prepared in Example 1 and Comparative Example 1.

[0059] Figure 5 This is the luminescence thermal stability curve of the luminescent material prepared in Example 1.

[0060] Figure 6 This is a diagram of the quantum yield of the luminescent material prepared in Example 1.

[0061] Figure 7 This is a double 85 aging diagram of the luminescent material prepared in Example 1. DETAILED DESCRIPTION

[0062] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0063] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0064] Example 1

[0065] Ba 0.75 Al 11 O 17.25 :8%Eu 2+ ,6%Mn 2+ Preparation of luminescent materials

[0066] (1) According to the chemical formula Ba 0.75 Al 11 O 17.25 :8%Eu 2+ ,6%Mn 2+ The stoichiometric ratio of each element in the raw materials BaCO3, Eu2O3, MnO2, Al2O3 and 20wt% of the total amount of Li2CO3 (flux) are weighed respectively, and the raw materials are ground and mixed evenly to obtain a mixed material. The specific amounts of BaCO3, Eu2O3, MnO2, Al2O3 and Li2CO3 are shown in Table 1 below.

[0067] (2) The mixed material obtained in step (1) is pre-calcined in an air atmosphere at a temperature of 1400° C. for 8 hours. After naturally cooling to room temperature, the mixture is ground into powder to obtain a pre-calcined product.

[0068] (3) The pre-calcined product obtained in step (2) is calcined in a reducing atmosphere at a temperature of 1400° C. for 8 hours. After naturally cooling to room temperature, the product is taken out and ground into powder to obtain the luminescent material sample.

[0069] The reducing atmosphere is a nitrogen-hydrogen mixed gas (5v.% H2+95v.% N2), that is, the volume ratio of hydrogen in the mixed gas is 5vol%.

[0070] Example 2-7 and Comparative Example 1-2: A 0.75 M 11 D 17.25 :xEu 2+ ,yMn 2+ Preparation of luminescent materials

[0071] Examples 2-7 and Comparative Examples 1-2 were synthesized by solid phase reaction method, and the preparation steps were the same as those in Example 1, except for the types and amounts of raw materials, flux, synthesis temperature, synthesis time, reducing atmosphere, etc. The specific reaction conditions are shown in Table 1 below.

[0072] Table 1 Preparation parameters of luminescent materials of Examples 1-7 and Comparative Examples 1-2

[0073]

[0074]

[0075] In Table 1, “-” represents that the step is not included.

[0076] The properties of the luminescent materials obtained in Example 1, Comparative Example 1 and Comparative Example 2 are listed in Table 2.

[0077] Table 2 Comparison of luminous performance of Example 1, Comparative Example 1 and Comparative Example 2

[0078]

[0079] Among them, the test method for internal quantum yield, external quantum yield and absorption efficiency is: use FLS980 (Edinburgh Instruments) fluorescence spectrometer equipped with a 450W xenon lamp coupled with an optical integrating sphere, and then use a standard halogen tungsten lamp to calibrate the optical response of the above instrument, and then test the internal quantum yield, external quantum yield and absorption efficiency.

[0080] Test method for thermal stability (200℃ / 25℃): Place the luminescent material on a heating platform (77-873K, THMS600, Linkam Scientific Instruments), control the temperature of the sample holder through a temperature control program, and use an FLS980 (Edinburgh Instruments) fluorescence spectrometer to collect the emission spectra of the samples at different temperatures (25-200℃). The thermal stability of the material is analyzed and evaluated through the integrated intensity values ​​of the emission spectra at different temperatures.

[0081] The test method for high temperature and high humidity stability (double 85 aging for seven days / no aging): Place the sample in a constant temperature and humidity test chamber (Aipei Technology, AP-HX-50AS), set 85℃ / 85% humidity as the aging conditions, and use FLS980 (Edinburgh Instruments) fluorescence spectrometer to test the luminescence intensity and luminescence quantum yield of the sample after different aging times, so as to evaluate the high temperature and high humidity stability of the material.

[0082] Example 8: Preparation of LED light-emitting device

[0083] This embodiment prepares an LED light-emitting device, which includes a packaging substrate, an ultraviolet 365nm LED chip, silica gel, and a red light emitting material K2TiF6:Mn 4+ and the luminescent material Ba prepared in Example 1 0.75 Al 11 O 17.25 :8%Eu 2+ ,6%Mn 2+ . The red light emitting material K2TiF6:Mn 4+ The luminescent material prepared in Example 1 is uniformly dispersed in silica gel at a mass ratio of 1:1, covered on the ultraviolet LED chip in a coating manner, placed in an oven at 120°C for curing for 2 hours, taken out and naturally cooled to obtain the LED light-emitting device of the present invention.

[0084] The phase analysis test of the luminescent materials in the embodiments was carried out using an X-ray diffractometer (DMAX 2500PC, Rigaku Corporation, Japan), the morphology and particle size of the luminescent materials in the embodiments were observed using a field emission scanning electron microscope (Apreo S LoVac), and the excitation spectrum and emission spectrum of the luminescent materials in the embodiments were tested using an FLS980 (Edinburgh Instruments) fluorescence spectrometer.

[0085] Figure 1 It is the X-ray powder diffraction (XRD) pattern of the sample of Example 1. The test results show that the prepared material is pure phase and matches the PDF#75-0707 standard card.

[0086] Figure 2This is a scanning electron microscope (SEM) image of the sample of Example 1. The results show that the luminescent material particles of Example 1 have obvious layered characteristics, good crystallinity, and a particle size of 20-30 μm.

[0087] Figure 3 It is the excitation and emission spectrum diagram of the sample in Example 1. The results show that the sample has a wide excitation peak at 250-420nm, and the dual emission peaks are 450nm, blue with a half-height width of 50nm, and 515nm, green with a half-height width of 27nm.

[0088] Figure 4 is the excitation spectrum comparison of the sample in Example 1 and the sample in Comparative Example 1. Figure 4 It can be seen that after adding Li2CO3 flux (also an ion compensator), the excitation spectrum of the luminescent material will be broadened accordingly, and the strongest excitation will be red-shifted from 310nm to 365nm. The excitation intensity at 365nm is about three times that of 310nm.

[0089] Figure 5 It is the luminescence thermal stability curve of the sample in Example 1. The results show that the overall integrated intensity of the sample in Example 1 at 200°C remains the same as the initial intensity. In the heating and cooling cycle of 25-200°C, the luminescence performance has good reproducibility, which reflects the excellent thermal stability of the luminescent material of the present invention.

[0090] Figure 6 It is a graph of the quantum yield of the sample of Example 1. The quantum yield of Example 1 is 95%.

[0091] Figure 7 This is the double 85 aging graph of the sample in Example 1. After aging for seven days at 85°C and 85% humidity, the luminous intensity and quantum efficiency of the luminescent material remain at 100%, that is, remain unchanged compared to the initial value, and have excellent high temperature and high humidity stability.

[0092] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a luminescent material, characterized in that: The chemical composition of the luminescent material is A 0.75 M 11 D 17.25 :xEu 2+ ,yMn 2+ ; Wherein, A is one, two or more of Be, Mg, Ca, Sr, Ba, M is one, two or more of B, Al, Ga, In, D is O, Eu 2+ and Mn 2+ For the luminescent central ion, 1 at.%≤x≤30 at.%; 0.5 at.%≤y≤40 at.%; The method comprises the following steps: (1) According to chemical formula A 0.75 M 11 D 17.25 :xEu 2+ ,yMn 2+ The raw materials of the compound containing the A element, the compound containing the M element, the compound containing the Eu element, the compound containing the Mn element, and the flux are mixed to obtain a mixture; and at least one of the compound containing the A element, the compound containing the M element, the compound containing the Eu element, and the compound containing the Mn element contains the D element; (2) pre-calcining the mixture obtained in step (1) under an air atmosphere to obtain a pre-calcined product; (3) calcining the pre-calcined product obtained in step (2) under a reducing atmosphere to obtain the luminescent material; The flux is selected from Li2CO3 and LiCl; In step (2), the pre-calcination temperature is 900°C-2000°C.

2. The method according to claim 1, characterized in that The chemical composition of the luminescent material is Be 0.75 B 11 O 17.25 : 10% Eu 2+ , 20% Mn 2+ 、Be 0.75 Al 11 O 17.25 : 12% Eu 2+ , 23% Mn 2+ 、Be 0.75 Ga 11 O 17.25 : 15% Eu 2+ , 21% Mn 2+ 、Mg 0.75 B 11 O 17.25 : 11% Eu 2+ , 22% Mn 2+ 、Mg 0.75 Al 11 O 17.25 : 17% Eu 2+ , 28% Mn 2+ 、Ca 0.75 B 11 O 17.25 : 25% Eu 2+ , 51% Mn 2+ 、Ca 0.75 Al 11 O 17.25 : 13% Eu 2+ , 24% Mn 2+ 、Sr 0.75 B 11 O 17.25 : 14% Eu 2+ , 27% Mn 2+ 、Sr 0.75 Al 11 O 17.25 : 16% Eu 2+ , 21% Mn 2+ 、Ba 0.75 B 11 O 17.25 : 32% Eu 2+ , 46% Mn 2+ 、Ba 0.75 In 11 S 17.25 : 12% Eu 2+ , 36% Mn 2+ 、Ba 0.75 Al 11 O 17.25 : 25% Eu 2+ , 56% Mn 2+ 、Ba 0.75 Al 11 THE 17.25 :8%Me 2+ ,6%Mn 2+ 、Sr 0.75 B 11 THE 17.25 :4%Me 2+ ,8%Mn 2 + 、Mg 0.75 In 11 THE 17.25 :2%Me 2+ ,5%Mn 2+ ,Here 0.75 Ga 11 THE 17.25 :9%Me 2+ ,15%Mn 2+ 、Sr 0.75 In 11 THE 17.25 :3%Me 2+ ,12%Mn 2+ ,Here 0.75 B 11 THE 17.25 :14%Me 2+ ,24%Mn 2+ 、Mg 0.75 Ga 11 THE 17.25 :6%Mn 2+ 。 3. The method according to claim 1, characterized in that: The luminescent material is powder, and the average particle size thereof is 5-40 μm.

4. The method according to claim 1, characterized in that The luminescent material can be excited by violet light and / or blue light.

5. The method according to claim 4, characterized in that The luminescent material can be excited by light in the range of 200-480 nm.

6. The method according to claim 1, characterized in that The luminescent material has narrow-band blue and green light emission properties.

7. The method according to claim 6, characterized in that The luminescent material emits blue light with a wavelength of 450 nm and a half-width of 50 nm and green light with a wavelength of 515 nm and a half-width of 27 nm.

8. The method according to claim 1, characterized in that The internal quantum yield of the luminescent material reaches 95%, the external quantum yield reaches 75%, and the absorption efficiency reaches 79%; The luminescent material has excellent thermal stability, and the luminescent integrated intensity remains the same as the initial intensity at 200°C; The luminescent material has excellent high-temperature and high-humidity stability. After aging for seven days at 85° C. and 85% humidity, the luminescent intensity and quantum efficiency of the luminescent material remain unchanged compared to the initial values.

9. The method according to claim 1, characterized in that: In step (1), the compound containing element A is selected from at least one of carbonates containing element A, oxides containing element A, nitrides containing element A, halides containing element A, nitrates containing element A, sulfides containing element A, sulfates containing element A, oxalates containing element A, gallates containing element A, germanates containing element A, selenides containing element A, and tellurides containing element A; In step (1), the compound containing the M element is selected from at least one of a carbonate containing the M element, an oxide containing the M element, a nitride containing the M element, a halide containing the M element, a nitrate containing the M element, a sulfide containing the M element, a sulfate containing the M element, an oxalate containing the M element, a gallate containing the M element, a germanate containing the M element, a selenide containing the M element, and a telluride containing the M element.

10. The method according to claim 9, characterized in that The compound containing element A is selected from at least one of BaO, BaCO3, SrO, SrCO3, MgO, MgCO3, CaCO3, and CaO; The compound containing the M element is selected from at least one of Al2O3, H3BO3, In2O3, and Ga2O3.

11. The method according to claim 1, characterized in that: The compound containing the Eu element is selected from the oxide of the Eu element; The compound containing the Mn element is selected from at least one of an oxide and a carbonate of the Mn element; The amount of the flux is 0.1-50 wt.% of the total mass of the raw materials in step (1); In step (2), the pre-calcination time is 1-60 hours; in step (3), the calcination temperature is 500° C.-2000° C.; and the calcination time is 1-60 hours.

12. The method according to claim 1, characterized in that The compound containing the Eu element is selected from Eu2O3; The compound containing the Mn element is selected from MnO2 or MnCO3.

13. A light emitting device, characterized in that: The invention comprises an excitation light source and at least one fluorescence conversion layer, wherein the fluorescence conversion layer comprises at least one luminescent material prepared by the method according to any one of claims 1 to 12.

14. The light emitting device according to claim 13, characterized in that: The fluorescent conversion layer also includes other luminescent materials, and the other luminescent materials are K2TiF6:Mn 4+ or K2SiF6:Mn 4+ Fluoride luminescent materials.

15. The light emitting device according to claim 13, characterized in that: The fluorescent conversion layer is coated on the LED chip, and the LED chip is used to carry the fluorescent conversion layer.

16. The light emitting device according to claim 13, characterized in that: The light emitting device further comprises a base.