Long-life monitoring method for stress corrosion and fatigue of nuclear power steam turbines throughout their life cycle

Through the monitoring methods and devices for the full life of stress corrosion and fatigue long life of nuclear power turbines, the problem of stress corrosion in nuclear power turbines is solved, and the comprehensive monitoring of stress corrosion and fatigue is achieved, ensuring the long life and safe operation of the equipment.

CN116776589BActive Publication Date: 2024-11-05SHANGHAI POWER EQUIPMENT RESEARCH INSTITUTE CO LTD +4
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310716848.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-15
Publication Date
2024-11-05
Estimated Expiration
2043-06-15

AI Technical Summary

Technical Problem

Nuclear power turbines fail to effectively consider stress corrosion during operation, resulting in insufficient safety monitoring of crack growth life, affecting the long life and safe operation of the equipment.

Method used

A method and device for monitoring stress corrosion and fatigue long life of nuclear power turbines is proposed. By determining the stress corrosion crack proliferation life and fatigue crack proliferation life of target monitoring components, including low-period fatigue and high-period fatigue, based on these data Crack proliferation life safety monitoring.

Benefits of technology

It realizes safety monitoring of the long-life life of nuclear power turbines, comprehensively considers stress corrosion and fatigue, and ensures the safe operation of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116776589B_ABST
    Figure CN116776589B_ABST
Patent Text Reader

Abstract

The present disclosure provides a method for long-life monitoring of stress corrosion and fatigue during the entire life of a nuclear power steam turbine. The method comprises: determining one or more target monitoring components from the components to be monitored; determining the long-life monitoring data required for the target monitoring components, wherein the long-life monitoring data comprises stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life comprises at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life; based on the long-life monitoring data required for the target monitoring components, the target monitoring components are subjected to crack growth life safety monitoring. Thus, the target monitoring components can be subjected to crack growth life safety monitoring taking stress corrosion and fatigue into consideration comprehensively, so as to ensure the long-life safe operation of the nuclear power steam turbine during the entire life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of nuclear power steam turbines, and in particular to a method, device, electronic equipment, storage medium and platform for long-life monitoring of stress corrosion and fatigue of nuclear power steam turbines throughout their entire life cycle. Background Art

[0002] At present, with the aggravation of energy shortage, people are in urgent need of developing new energy to meet people's energy needs. Nuclear power is a clean energy, with no carbon dioxide emissions and little environmental impact; nuclear power is an efficient energy with high energy density and low resource consumption; nuclear power is a stable energy without intermittency, long utilization hours and stable power supply capacity; nuclear power is a safe energy with low possibility of accidents, and is an important option to enhance energy security. Nuclear power turbines are important equipment in nuclear power technology. In related technologies, crack propagation life safety monitoring of nuclear power turbines is required to ensure the normal operation of nuclear power turbines. However, the crack propagation life safety monitoring of nuclear power turbines does not take stress corrosion into consideration. Summary of the invention

[0003] The present disclosure aims to solve one of the technical problems in the above-mentioned technologies at least to some extent.

[0004] To this end, the first objective of the present disclosure is to provide a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine throughout its entire life cycle.

[0005] The second objective of the present disclosure is to provide a stress corrosion and fatigue long-life monitoring device for a nuclear power steam turbine throughout its entire life cycle.

[0006] A third objective of the present disclosure is to provide an electronic device.

[0007] A fourth objective of the present disclosure is to provide a computer-readable storage medium.

[0008] The fifth objective of the present disclosure is to provide a monitoring platform suitable for nuclear power steam turbines.

[0009] The first aspect of the present disclosure provides a method for long-life monitoring of stress corrosion and fatigue of a nuclear power steam turbine throughout its entire life cycle, comprising: determining one or more target monitoring components from the components to be monitored; determining long-life monitoring data required for the target monitoring components, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life; based on the long-life monitoring data required for the target monitoring components, performing crack growth life safety monitoring on the target monitoring components.

[0010] The second aspect embodiment of the present disclosure proposes a long-life monitoring device for stress corrosion and fatigue of a nuclear power steam turbine throughout its life cycle, comprising: a first determination module, used to determine one or more target monitoring components from the components to be monitored; a second determination module, used to determine the long-life monitoring data required for the target monitoring components, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life; a monitoring module, used to perform crack growth life safety monitoring of the target monitoring components based on the long-life monitoring data required for the target monitoring components.

[0011] The third aspect embodiment of the present disclosure proposes an electronic device, including: a memory, a processor, and a computer program stored in the memory and executable on the processor. When the processor executes the program, the stress corrosion and fatigue long-life monitoring method for the entire life cycle of a nuclear power steam turbine as described in the first aspect embodiment of the present disclosure is implemented.

[0012] The fourth aspect of the present application provides a computer-readable storage medium on which a computer program is stored. When the program is executed by a processor, the method for monitoring stress corrosion and fatigue long life of a nuclear power steam turbine throughout its life cycle as described in the first aspect of the present disclosure is implemented.

[0013] The fifth aspect embodiment of the present application proposes a monitoring platform suitable for a nuclear power steam turbine, comprising a stress corrosion and fatigue long-life monitoring device for the entire life cycle of a nuclear power steam turbine as described in the second aspect embodiment of the present disclosure; or an electronic device as described in the third aspect embodiment of the present disclosure; or a computer-readable storage medium as described in the fourth aspect embodiment of the present disclosure.

[0014] The technical solution provided by the embodiment of the present disclosure brings at least the following beneficial effects: determining one or more target monitoring components from the components to be monitored, determining the long-life monitoring data required for the target monitoring components, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life, and based on the long-life monitoring data required for the target monitoring components, the target monitoring components are subjected to crack growth life safety monitoring. Thus, the target monitoring components can be subjected to crack growth life safety monitoring taking stress corrosion and fatigue into consideration comprehensively, so as to ensure the long-life safe operation of the nuclear power steam turbine throughout its life cycle.

[0015] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The above and / or additional aspects and advantages of the present disclosure will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:

[0017] Figure 1 A schematic flow chart of a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to an embodiment of the present disclosure;

[0018] Figure 2 It is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine during its entire life cycle according to another embodiment of the present disclosure;

[0019] Figure 3 A schematic diagram of a process for obtaining stress corrosion crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to an embodiment of the present disclosure;

[0020] Figure 4 A schematic diagram of a process for obtaining stress corrosion crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0021] Figure 5 A schematic diagram of a process for obtaining stress corrosion crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0022] Figure 6 A schematic diagram of a process for obtaining stress corrosion crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0023] Figure 7 A schematic diagram of a process for obtaining stress corrosion crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0024] Figure 8 A schematic diagram of a process for obtaining low-cycle fatigue crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to an embodiment of the present disclosure;

[0025] Fig. 9 A schematic diagram of a process for obtaining low-cycle fatigue crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0026] Fig.10 A schematic diagram of a process for obtaining low-cycle fatigue crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0027] Fig.11 A schematic diagram of a process for obtaining low-cycle fatigue crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0028] Fig.12 A schematic diagram of a process for obtaining low-cycle fatigue crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0029] Fig.13 A schematic diagram of a process for obtaining low-cycle fatigue crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0030] Fig.14 A schematic diagram of a process for obtaining high cycle fatigue crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to an embodiment of the present disclosure;

[0031] Fig.15 A schematic diagram of a process for obtaining high-cycle fatigue crack growth life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0032] Fig.16 It is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine during its entire life cycle according to another embodiment of the present disclosure;

[0033] Fig.17 A schematic diagram of a process for obtaining crack growth calendar life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to an embodiment of the present disclosure;

[0034] Fig.18 A schematic diagram of a process for obtaining crack growth calendar life in a method for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to another embodiment of the present disclosure;

[0035] Fig.19 It is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine during its entire life cycle according to another embodiment of the present disclosure;

[0036] Fig. 20 It is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine during its entire life cycle according to another embodiment of the present disclosure;

[0037] Fig.21 It is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine during its entire life cycle according to another embodiment of the present disclosure;

[0038] Fig. 22A schematic diagram of the structure of a stress corrosion and fatigue long-life monitoring device for a nuclear power steam turbine during its entire life cycle according to an embodiment of the present disclosure;

[0039] Fig.23 The figure is a schematic diagram of the structure of an electronic device according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0040] Embodiments of the present disclosure are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present disclosure, and should not be construed as limiting the present disclosure.

[0041] The following describes the stress corrosion and fatigue long-life monitoring method, device, electronic equipment, storage medium and platform for a nuclear power steam turbine throughout its life cycle in conjunction with the accompanying drawings according to the embodiments of the present disclosure.

[0042] Figure 1 The present invention is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine during its entire life cycle according to an embodiment of the present invention.

[0043] like Figure 1 As shown, the stress corrosion and fatigue long-life monitoring method for a nuclear power steam turbine during its entire life cycle according to an embodiment of the present disclosure includes:

[0044] S101, determining one or more target monitoring components from components to be monitored.

[0045] It should be noted that the stress corrosion and fatigue long-life monitoring method for the entire life cycle of a nuclear power steam turbine according to the embodiment of the present disclosure can be executed by the stress corrosion and fatigue long-life monitoring device for the entire life cycle of a nuclear power steam turbine according to the embodiment of the present disclosure, and the stress corrosion and fatigue long-life monitoring device for the entire life cycle of a nuclear power steam turbine according to the embodiment of the present disclosure can be configured in any monitoring platform suitable for a nuclear power steam turbine to execute the stress corrosion and fatigue long-life monitoring method for the entire life cycle of a nuclear power steam turbine according to the embodiment of the present disclosure.

[0046] It should be noted that the components to be monitored refer to the components of the nuclear power steam turbine, and the target monitoring components are part or all of the components to be monitored. There is no excessive limitation on the number of target monitoring components. For example, the target monitoring components may include the rotor blade root slot, cylinder, rotor, etc. of the nuclear power steam turbine.

[0047] In one embodiment, determining one or more target monitoring components from the components to be monitored includes identifying whether the components to be monitored meet set monitoring conditions, and if the components to be monitored meet the set monitoring conditions, determining the components to be monitored as target monitoring components. It should be noted that there are no excessive restrictions on the set monitoring conditions.

[0048] In one embodiment, determining one or more target monitoring components from the components to be monitored includes obtaining a crack extension life safety monitoring instruction, extracting an identifier of the target monitoring component from the crack extension life safety monitoring instruction, and determining one or more target monitoring components from the components to be monitored based on the identifier of the target monitoring component. It should be noted that there are no excessive restrictions on the crack extension life safety monitoring instruction. For example, the crack extension life safety monitoring instruction sent by the remote client can be obtained, or the electronic device can generate the crack extension life safety monitoring instruction by itself.

[0049] In one embodiment, determining one or more target monitoring components from the components to be monitored further includes obtaining a crack extension life safety monitoring instruction sent by a remote client, and determining the components to be monitored associated with the remote client as the target monitoring components. It is understandable that an association relationship between the remote client and the components to be monitored can be established in advance, and one remote client can establish an association relationship with at least one component to be monitored.

[0050] S102, determining the long-life monitoring data required for the target monitoring component, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life.

[0051] It should be noted that the stress corrosion crack growth life refers to the crack growth life of the monitored component when the damage type to which the monitored component is subjected includes stress corrosion; the low-cycle fatigue crack growth life refers to the crack growth life of the monitored component when the damage type to which the monitored component is subjected includes low-cycle fatigue; and the high-cycle fatigue crack growth life refers to the crack growth life of the monitored component when the damage type to which the monitored component is subjected includes high-cycle fatigue.

[0052] It should be noted that obtaining the stress corrosion crack growth life, low cycle fatigue crack growth life, and high cycle fatigue crack growth life of the monitored components can all be achieved by using relevant technologies, and no excessive restrictions are made here.

[0053] In one embodiment, determining the long-life monitoring data required for the target monitoring component includes obtaining a mapping relationship between the target monitoring component and the long-life monitoring data, and determining the long-life monitoring data required for the target monitoring component based on the mapping relationship. It is understandable that the above mapping relationship can be pre-calibrated based on actual conditions.

[0054] In one embodiment, the long-life monitoring data required for the target monitoring component is determined, including if the target monitoring component is a rotor blade root slot or a rotor, determining that the long-life monitoring data required for the target monitoring component includes stress corrosion crack growth life, low cycle fatigue crack growth life, and high cycle fatigue crack growth life; if the target monitoring component is a cylinder, determining that the long-life monitoring data required for the target monitoring component includes stress corrosion crack growth life and low cycle fatigue crack growth life.

[0055] S103, based on the long-life monitoring data required by the target monitoring component, perform crack propagation life safety monitoring on the target monitoring component.

[0056] In one embodiment, based on the long-life monitoring data required by the target monitoring component, crack propagation life safety monitoring is performed on the target monitoring component, including determining whether the long-life monitoring data required by the target monitoring component meets the monitoring qualification conditions, so as to perform crack propagation life safety monitoring on the target monitoring component.

[0057] It should be noted that there are not too many restrictions on the monitoring qualification conditions. For example, the long-life monitoring data required by the target monitoring component can be greater than the set threshold value, which can be determined as the monitoring qualification condition, and there are not too many restrictions on the set threshold value.

[0058] In one embodiment, based on the long-life monitoring data required by the target monitoring component, crack propagation life safety monitoring is performed on the target monitoring component, including obtaining the monitoring criterion value of the target monitoring component, if the long-life monitoring data required by the target monitoring component is greater than or equal to the monitoring criterion value, determining that the long-life monitoring data required by the target monitoring component meets the monitoring qualification conditions, if the long-life monitoring data required by the target monitoring component is less than the monitoring criterion value, determining that the long-life monitoring data required by the target monitoring component does not meet the monitoring qualification conditions.

[0059] In some examples, a mapping relationship between the model of the monitoring component and the monitoring criterion value can be established in advance to obtain the monitoring criterion value of the target monitoring component, including querying the monitoring criterion value in the above mapping relationship based on the model of the target monitoring component, and determining the queried monitoring criterion value as the monitoring criterion value of the target monitoring component.

[0060] In one embodiment, if the long-life monitoring data required by the target monitoring component does not meet the monitoring qualification conditions, it also includes generating indication information for indicating that a safety abnormality has occurred in the target monitoring component, so as to promptly inform the user that a safety abnormality has occurred in the target monitoring component.

[0061] In summary, according to the stress corrosion and fatigue long-life monitoring method for the whole life of a nuclear power steam turbine of the embodiment of the present disclosure, one or more target monitoring components are determined from the components to be monitored, and the long-life monitoring data required for the target monitoring components are determined, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life. Based on the long-life monitoring data required by the target monitoring component, the target monitoring component is subjected to crack growth life safety monitoring. Thus, the target monitoring component can be subjected to crack growth life safety monitoring by comprehensively considering stress corrosion and fatigue, so as to ensure the long-life safe operation of the nuclear power steam turbine throughout its whole life.

[0062] Figure 2 The present invention is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine throughout its entire life cycle according to another embodiment of the present invention.

[0063] like Figure 2 As shown, the stress corrosion and fatigue long-life monitoring method for a nuclear power steam turbine during its entire life cycle according to an embodiment of the present disclosure includes:

[0064] S201, determining one or more target monitoring components from the components to be monitored.

[0065] For the relevant contents of step S201, please refer to the above embodiment, which will not be described again here.

[0066] S202, obtaining a set of crack extension dimensions of a target monitored component.

[0067] It should be noted that there are no excessive restrictions on the crack extension size set.

[0068] In one embodiment, obtaining a set of crack extension dimensions of a target monitoring component includes obtaining basic stress calculation data of the target monitoring component, obtaining basic material test data of the target monitoring component, and determining a set of crack extension dimensions based on the basic stress calculation data and the basic material test data. Thus, the method can comprehensively consider the basic stress calculation data and the basic material test data to determine the set of crack extension dimensions.

[0069] It should be noted that there are no excessive restrictions on the basic data for stress calculation and the basic data for material testing.

[0070] In one implementation, based on stress calculation basic data and material experiment basic data, a set of crack extension sizes is determined, including the following possible implementations:

[0071] Method 1: Determine the stress corrosion crack extension size threshold of the target monitoring component based on the crack shape parameters of the target monitoring component, the stress corrosion fracture toughness of the material of the target monitoring component, and the maximum stress at the crack site of the target monitoring component under steady-state conditions of nuclear power steam turbine under load operation.

[0072] Method 2: Determine the low-cycle fatigue critical crack size of the target monitoring component under the set operating condition of the nuclear power steam turbine based on the crack shape parameters of the target monitoring component, the fracture toughness of the material of the target monitoring component and the maximum stress at the crack site of the target monitoring component under the set operating condition of the nuclear power steam turbine.

[0073] Method 3: Determine the high cycle fatigue crack extension size threshold of the target monitoring component based on the crack shape parameters of the target monitoring component, the test value of the high cycle fatigue crack extension threshold of the material of the target monitoring component, and the high cycle fatigue stress range of the crack location of the target monitoring component under steady-state conditions of nuclear power steam turbine under load operation.

[0074] Method 4: Determine the high cycle fatigue critical crack size of the target monitoring component based on the crack shape parameters of the target monitoring component, the fracture toughness of the material of the target monitoring component, and the maximum stress at the crack site of the target monitoring component under steady-state conditions of nuclear power steam turbine operation with load.

[0075] The following takes the rotor as an example of the target monitoring component to describe the method of obtaining the crack extension size set of the rotor.

[0076] For example, the crack growth size set includes the stress corrosion crack growth size threshold a SCC , high cycle fatigue crack growth size threshold value a th , high cycle fatigue critical crack size a cH , Low cycle fatigue critical crack size a of the rotor of nuclear power steam turbine under normal shutdown transient condition cn 、Critical crack size of low cycle fatigue of rotor in transient condition of nuclear power steam turbine 110% overspeed test a c110% , Low cycle fatigue critical crack size a of the rotor of nuclear power steam turbine under transient condition of 120% overspeed operation c120% wait.

[0077] In one implementation, based on stress calculation basic data and material experiment basic data, a set of crack extension sizes of a rotor is determined, including the following possible implementations:

[0078] Method 1: Determine the threshold value of the rotor stress corrosion crack extension size based on the rotor crack shape parameters, the rotor material stress corrosion fracture toughness and the maximum stress at the rotor crack site under steady-state conditions of nuclear power steam turbine under load operation.

[0079] Method 2: Determine the high-cycle fatigue crack extension size threshold of the rotor based on the crack shape parameters of the rotor, the test value of the high-cycle fatigue crack extension threshold of the rotor material, and the high-cycle fatigue stress range of the rotor under steady-state conditions of load operation of the nuclear power steam turbine.

[0080] Method 3: Determine the high cycle fatigue critical crack size of the rotor based on the crack shape parameters of the rotor, the fracture toughness of the rotor material, and the maximum stress at the rotor crack site under steady-state conditions of nuclear power steam turbine operation with load.

[0081] Method 4: Based on the crack shape parameters of the rotor, the fracture toughness of the rotor material, and the maximum stress at the rotor crack site under the normal shutdown transient condition of the nuclear power steam turbine, the low-cycle fatigue critical crack size of the rotor under the normal shutdown transient condition of the nuclear power steam turbine is determined.

[0082] Method 5: Based on the crack shape parameters of the rotor, the fracture toughness of the rotor material, and the maximum stress at the rotor crack site under the transient operating condition of the nuclear power steam turbine 110% overspeed test, the low-cycle fatigue critical crack size of the rotor under the transient operating condition of the nuclear power steam turbine 110% overspeed test is determined.

[0083] Method 6: Based on the crack shape parameters of the rotor, the fracture toughness of the rotor material, and the maximum stress at the rotor crack site under the transient operating condition of 120% overspeed of the nuclear power steam turbine, the low-cycle fatigue critical crack size of the rotor under the transient operating condition of 120% overspeed of the nuclear power steam turbine is determined.

[0084] For example, for a certain type of 1200MW nuclear power steam turbine, the weak part of the weld life of the welded low-pressure rotor is the weld on the outer surface of the rotor. During the design stage of the nuclear power steam turbine, the basic data for stress calculation and material testing of the welded low-pressure rotor are shown in Tables 1 and 2 respectively.

[0085] Table 1 Basic data for stress calculation of welded low-pressure rotor

[0086]

[0087] Table 2 Basic data of material test for welded low-pressure rotor

[0088]

[0089]

[0090] The calculation process of the crack growth size set of the welded low-pressure rotor is as follows:

[0091]

[0092]

[0093]

[0094]

[0095]

[0096]

[0097] The following takes the rotor blade root slot as an example of the target monitoring component to describe how to obtain the crack extension size set of the rotor blade root slot.

[0098] For example, the basic data for stress calculation include the high-cycle fatigue stress range Δσ at the crack position of the rotor blade root slot of a nuclear power steam turbine under steady-state load operation. H and the maximum stress σ at the crack of the rotor blade root slot maxH , the maximum stress σ at the crack of the rotor blade root slot under normal shutdown transient conditions maxn , Maximum stress σ at the crack site of the rotor blade root slot under transient conditions of 110% overspeed test max110% , Maximum stress σ at the crack site of the rotor blade root slot under 120% overspeed transient condition max120% wait.

[0099] For example, the basic data of material testing include the fracture toughness K of the rotor material. IC , Stress corrosion fracture toughness K of rotor material ISCC , annual average stress corrosion crack growth rate test value Crack shape parameter Q, high cycle fatigue crack growth threshold of rotor material Test values, etc.

[0100] For example, the crack growth size set includes the stress corrosion crack growth size threshold a SCC , high cycle fatigue crack growth size threshold value a th , high cycle fatigue critical crack size a cH , Low cycle fatigue critical crack size a of the rotor blade root slot in the transient condition of normal shutdown of nuclear power steam turbine cn , Low cycle fatigue critical crack size a of the rotor blade root slot in transient condition of nuclear power steam turbine 110% overspeed test c110% , Low cycle fatigue critical crack size a of the rotor blade root slot of a nuclear power steam turbine under transient operating conditions of 120% overspeed c120% wait.

[0101] In some examples, based on stress calculation basic data and rotor material experimental basic data, a set of crack extension sizes is determined, including the following possible implementations:

[0102] Method 1: Determine the threshold value of the stress corrosion crack extension size of the rotor blade root slot based on the crack shape parameters of the rotor blade root slot, the stress corrosion fracture toughness of the rotor material and the maximum stress at the crack site of the rotor blade root slot under steady-state conditions of load operation of a nuclear power steam turbine.

[0103] Method 2: Determine the high cycle fatigue crack extension size threshold of the rotor blade root slot based on the crack shape parameters of the rotor blade root slot, the test value of the high cycle fatigue crack extension threshold of the rotor material, and the high cycle fatigue stress range of the rotor blade root slot crack location under steady-state conditions of nuclear power steam turbine load operation.

[0104] Method 3: Based on the crack shape parameters of the rotor blade root slot, the fracture toughness of the rotor material, and the maximum stress at the crack site of the rotor blade root slot under steady-state conditions of load operation of a nuclear power steam turbine, the high-cycle fatigue critical crack size of the rotor blade root slot is determined.

[0105] Method 4: Based on the crack shape parameters of the rotor blade root slot, the fracture toughness of the rotor material, and the maximum stress at the crack site of the rotor blade root slot under the normal shutdown transient condition of the nuclear power steam turbine, the low-cycle fatigue critical crack size of the rotor blade root slot under the normal shutdown transient condition of the nuclear power steam turbine is determined.

[0106] Method 5: Based on the crack shape parameters of the rotor blade root slot, the fracture toughness of the rotor material, and the maximum stress at the crack site of the rotor blade root slot under the transient condition of the nuclear power steam turbine 110% overspeed test, the low-cycle fatigue critical crack size of the rotor blade root slot under the transient condition of the nuclear power steam turbine 110% overspeed test is determined.

[0107] Method 6: Based on the crack shape parameters of the rotor blade root slot, the fracture toughness of the rotor material, and the maximum stress at the crack site of the rotor blade root slot under the transient operating condition of 120% overspeed of the nuclear power steam turbine, the low-cycle fatigue critical crack size of the rotor blade root slot under the transient operating condition of 120% overspeed of the nuclear power steam turbine is determined.

[0108] For example, the new type of the 5th blade root groove of the No. 1 low-pressure rotor of a certain model of 1000MW nuclear power steam turbine A is an inverted T-shaped blade root groove, which works in the transition zone between superheated steam and wet steam, near the saturated steam line (Wilson), and is prone to stress corrosion cracking. The material grade of the No. 1 low-pressure rotor of nuclear power steam turbine A is 30Cr2Ni4MoV (3.5% NiCrMoV). During the manufacturing stage of nuclear power steam turbine A, the 5th blade root groove of the No. 1 low-pressure rotor of nuclear power steam turbine A was subjected to phased array nondestructive testing, and no cracks were found. In the case that no cracks were found in the phased array nondestructive testing, the crack depth a of the load-bearing tooth surface of the 5th inverted T-shaped blade root groove of the No. 1 low-pressure rotor of nuclear power steam turbine A was given. i =2mm=0.002m.

[0109] For example, a certain model of 1000MW nuclear power steam turbine B has been in operation for 20 years. During the planned overhaul, the phased array nondestructive testing and crack propagation life safety monitoring were performed on the 5th stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B. The low-pressure rotor operates in the transition zone between superheated steam and wet steam, near the saturated steam line (Wilson), and is prone to stress corrosion cracking. The material grade of the low-pressure rotor is 30Cr2Ni4MoV (3.5% NiCrMoV). During the service stage of nuclear power steam turbine B, the phased array nondestructive testing was performed on the 5th stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B, and the crack depth a of the load-bearing tooth surface of the 5th stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B was obtained. i =5mm=0.005m.

[0110] For example, a certain model of 1000MW nuclear power steam turbine C has been in operation for 20 years. During the planned overhaul, the phased array nondestructive testing and crack propagation life safety monitoring were performed on the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C. The low-pressure rotor operates in the transition zone between superheated steam and wet steam, near the saturated steam line (Wilson), and is prone to stress corrosion cracking. The material grade of the low-pressure rotor is 30Cr2Ni4MoV (3.5% NiCrMoV). During the service stage of nuclear power steam turbine C, the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of nuclear power steam turbine C was nondestructively monitored, and the crack depth a of the load-bearing tooth surface of the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of nuclear power steam turbine C was obtained. i =10mm=0.010m.

[0111] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the stress calculation basic data and rotor material test basic data of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A are shown in Tables 3 and 4 respectively.

[0112] Table 3 Basic data for stress calculation of the fifth stage inverted T-shaped blade root groove of the low-pressure rotor of a nuclear power steam turbine

[0113]

[0114] Table 4 Basic data of low-pressure rotor material test for nuclear power steam turbine

[0115]

[0116]

[0117] Among them, the maximum stress at the crack of the rotor blade root slot under normal shutdown transient conditions includes the maximum stress at the rotor surface weld under normal shutdown transient conditions σ maxn .

[0118] The calculation process of the crack growth size set of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of nuclear power steam turbine A is as follows:

[0119]

[0120]

[0121]

[0122]

[0123]

[0124]

[0125] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the stress calculation basic data and rotor material test basic data of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B are shown in Tables 3 and 4 respectively.

[0126] The calculation process of the crack growth size set of the 5th stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B is as follows:

[0127]

[0128]

[0129]

[0130]

[0131]

[0132]

[0133] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the stress calculation basic data and rotor material test basic data of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C are shown in Tables 3 and 4 respectively.

[0134] The calculation process of the crack growth size set of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of nuclear power steam turbine C is as follows:

[0135]

[0136]

[0137]

[0138]

[0139]

[0140]

[0141] The following takes the target monitoring component as a cylinder as an example to describe how to obtain the crack extension size set of the cylinder.

[0142] For example, the basic data for stress calculation include the maximum stress σ at the cylinder crack site of a nuclear power steam turbine under steady-state load operation. max0 , the maximum stress σ at the cylinder crack position of nuclear power steam turbine during cold start transient condition maxc , the maximum stress σ at the cylinder crack position of nuclear power steam turbine during warm start transient condition maxw , the maximum stress σ at the cylinder crack position of nuclear power steam turbine hot start transient condition maxh wait.

[0143] For example, the basic data of material testing includes the fracture toughness K of the cylinder material. IC , stress corrosion fracture toughness K of cylinder material ISCC , annual average stress corrosion crack growth rate test value Crack shape parameters Q, etc.

[0144] For example, the crack growth size set includes the stress corrosion crack growth size threshold a SCC , Low cycle fatigue critical crack size a of the cylinder of nuclear power steam turbine under transient cold start condition cc , Low cycle fatigue critical crack size a of cylinder of nuclear power steam turbine under transient condition of warm start cw , Low cycle fatigue critical crack size a of cylinder of nuclear power steam turbine under transient condition of hot start ch wait.

[0145] In some examples, based on stress calculation basic data and material experiment basic data, a set of crack extension sizes is determined, including the following possible implementations:

[0146] Method 1: Determine the threshold value of the stress corrosion crack extension size of the cylinder based on the crack shape parameters of the cylinder, the stress corrosion fracture toughness of the cylinder material and the maximum stress at the cylinder crack site under steady-state conditions of nuclear power steam turbine under load operation.

[0147] Method 2: Based on the crack shape parameters of the cylinder, the fracture toughness of the cylinder material, and the maximum stress at the cylinder crack site under the transient operating conditions of the nuclear power steam turbine cold start, the low-cycle fatigue critical crack size of the cylinder under the transient operating conditions of the nuclear power steam turbine cold start is determined.

[0148] Method 3: Based on the crack shape parameters of the cylinder, the fracture toughness of the cylinder material, and the maximum stress at the cylinder crack site under the transient condition of warm start of the nuclear power steam turbine, the low-cycle fatigue critical crack size of the cylinder under the transient condition of warm start of the nuclear power steam turbine is determined.

[0149] Method 4: Based on the crack shape parameters of the cylinder, the fracture toughness of the cylinder material, and the maximum stress at the cylinder crack site under the transient working condition of the nuclear power steam turbine hot start, the low-cycle fatigue critical crack size of the cylinder under the transient working condition of the nuclear power steam turbine hot start is determined.

[0150] For example, the inner cylinder of the No. 1 low-pressure cylinder of a certain model of 1000MW nuclear power steam turbine E is made of Q235B. It has a tendency to suffer from stress corrosion cracking when the water vapor contains NaOH and seawater leaked from the condenser. The weak part of the low-pressure inner cylinder is the connection between the low-pressure inner cylinder and the second-stage steam extraction pipe. The radius of the structural transition fillet at the structural discontinuity of the second-stage steam extraction pipe and the low-pressure connection is 5mm. This part works in the transition zone between superheated steam and wet steam, near the saturated steam line (Wilson), and is prone to stress corrosion cracking. During the design stage of the nuclear power steam turbine E, the safety of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E was monitored.

[0151] For example, the No. 1 low-pressure inner cylinder of a certain model of 1000MW nuclear power steam turbine A is made of Q235B. It tends to suffer from stress corrosion cracking when the water vapor contains NaOH or the condenser leaks seawater. The weak part of the low-pressure inner cylinder is the connection between the low-pressure inner cylinder and the second-stage steam extraction pipe. The radius of the structural transition fillet at the structural discontinuity of the connection between the second-stage steam extraction pipe and the low-pressure inner cylinder is 20mm. This part works in the transition zone between superheated steam and wet steam, near the saturated steam line (Wilson), and is prone to stress corrosion cracking. During the manufacturing stage of nuclear power steam turbine A, the No. 1 low-pressure inner cylinder of nuclear power steam turbine A was subjected to phased array nondestructive testing, and no cracks were found. When no cracks were found in the phased array nondestructive testing, the crack depth a at the connection between the No. 1 low-pressure inner cylinder and the second-stage steam extraction pipe of nuclear power steam turbine A was given. i =2mm=0.002m.

[0152] For example, the No. 2 low-pressure inner cylinder of a certain model of 1000MW nuclear power steam turbine B is made of Q235B. It tends to suffer from stress corrosion cracking when the water vapor contains NaOH or the condenser leaks seawater. The weak part of the low-pressure inner cylinder is the connection between the low-pressure inner cylinder and the second-stage steam extraction pipe. The radius of the structural transition fillet at the structural discontinuity of the connection between the second-stage steam extraction pipe and the low-pressure inner cylinder is 20mm. This part works in the transition zone between superheated steam and wet steam, near the saturated steam line (Wilson), and is prone to stress corrosion cracking. During the manufacturing stage of nuclear power steam turbine B, phased array nondestructive testing was performed on the No. 2 low-pressure inner cylinder of nuclear power steam turbine B, and the crack depth a at the connection between the No. 2 low-pressure inner cylinder of nuclear power steam turbine B and the second-stage steam extraction pipe was obtained. i =5mm=0.005m.

[0153] For example, a certain model of 1000MW nuclear power steam turbine C has been in operation for 20 years. During the planned overhaul, the No. 1 low-pressure inner cylinder of nuclear power steam turbine C was subjected to phased array nondestructive testing and crack propagation life safety monitoring. The material of the low-pressure inner cylinder is Q235B, which has a tendency to undergo stress corrosion cracking when the water vapor contains NaOH or the condenser leaks seawater. The weak part of the low-pressure inner cylinder life is the connection between the low-pressure inner cylinder and the second-stage steam extraction pipe. The structural transition fillet radius of the structural discontinuity at the connection between the second-stage steam extraction pipe and the low-pressure inner cylinder is 20mm. This part works in the transition zone between superheated steam and wet steam, near the saturated steam line (Wilson), and is prone to stress corrosion cracking. During the service stage of nuclear power steam turbine C, the No. 1 low-pressure inner cylinder of nuclear power steam turbine C was subjected to phased array nondestructive testing, and the crack depth a at the connection between the No. 1 low-pressure inner cylinder of nuclear power steam turbine C and the second-stage steam extraction pipe was obtained. i =5mm=0.005m.

[0154] For example, a certain model of 1000MW nuclear power steam turbine D has been in operation for 20 years. During the planned overhaul, the No. 2 low-pressure inner cylinder of nuclear power steam turbine D was subjected to phased array nondestructive testing and crack propagation life safety monitoring. The low-pressure inner cylinder is made of Q235B, which has a tendency to undergo stress corrosion cracking when the water vapor contains NaOH or the condenser leaks seawater. The weak part of the life of the No. 2 low-pressure inner cylinder of nuclear power steam turbine D is the connection between the low-pressure inner cylinder and the second-stage steam extraction pipe. The radius of the structural transition fillet at the structural discontinuity of the connection between the second-stage steam extraction pipe and the low-pressure inner cylinder is 20mm. This part works in the transition zone between superheated steam and wet steam, near the saturated steam line (Wilson), and is prone to stress corrosion cracking. During the service stage of nuclear power steam turbine D, the No. 1 low-pressure inner cylinder of nuclear power steam turbine C was subjected to phased array nondestructive testing, and the crack depth a at the connection between the No. 2 low-pressure inner cylinder of nuclear power steam turbine D and the second-stage steam extraction pipe was obtained. i =10mm=0.010m.

[0155] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E in the above embodiment as an example, the stress calculation basic data and material test basic data of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E are shown in Tables 5 and 6 respectively.

[0156] Table 5 Basic data for stress calculation of low pressure inner cylinder

[0157]

[0158]

[0159] Table 6 Basic data of material test for low pressure inner cylinder

[0160]

[0161] The calculation process of the crack growth size set of the No. 1 low-pressure inner cylinder of nuclear power steam turbine E is as follows:

[0162]

[0163]

[0164]

[0165]

[0166] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A in the above embodiment as an example, the stress calculation basic data and material test basic data of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A are shown in Tables 7 and 8 respectively.

[0167] Table 7 Basic data for stress calculation of low pressure inner cylinder

[0168]

[0169] Table 8 Basic data of material test for low pressure inner cylinder

[0170]

[0171] The calculation process of the crack growth size set of the No. 1 low-pressure inner cylinder of nuclear power steam turbine A is as follows:

[0172]

[0173]

[0174]

[0175]

[0176] For example, continuing to take the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B in the above embodiment as an example, the stress calculation basic data and material test basic data of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B are shown in Tables 7 and 8 respectively.

[0177] The calculation process of the crack growth size set of the No. 2 low-pressure inner cylinder of nuclear power steam turbine B is as follows:

[0178]

[0179]

[0180]

[0181]

[0182] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C in the above embodiment as an example, the stress calculation basic data and material test basic data of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C are shown in Tables 7 and 8 respectively.

[0183] The calculation process of the crack growth size set of the No. 1 low-pressure inner cylinder of nuclear power steam turbine C is as follows:

[0184]

[0185]

[0186]

[0187]

[0188] For example, continuing to take the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D in the above embodiment as an example, the stress calculation basic data and material test basic data of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D are shown in Tables 7 and 8 respectively.

[0189] The calculation process of the crack growth size set of the No. 2 low-pressure inner cylinder of nuclear power steam turbine D is as follows:

[0190]

[0191]

[0192]

[0193]

[0194] S203, determining the long-life monitoring data required for the target monitoring component based on the crack extension size set.

[0195] In one embodiment, obtaining long-life monitoring data required for a target monitoring component based on a crack extension size set includes obtaining long-life monitoring data required for a target monitoring component based on at least one crack extension size in the crack extension size set.

[0196] In one embodiment, based on a crack extension size set, obtaining a stress corrosion crack extension life includes obtaining at least one crack extension size that matches the stress corrosion crack extension life from the crack extension size set, and obtaining the stress corrosion crack extension life based on at least one crack extension size that matches the stress corrosion crack extension life.

[0197] It should be noted that, based on the crack growth size set, the low-cycle fatigue crack growth life and the high-cycle fatigue crack growth life can be obtained. The relevant content of obtaining the stress corrosion crack growth life based on the crack growth size set can be referred to, which will not be repeated here.

[0198] S204, based on the long-life monitoring data required by the target monitoring component, perform crack propagation life safety monitoring on the target monitoring component.

[0199] For the relevant contents of step S204, please refer to the above embodiment, which will not be repeated here.

[0200] In summary, according to the stress corrosion and fatigue long-life monitoring method for the entire life of a nuclear power steam turbine in the embodiment of the present disclosure, a set of crack extension dimensions of a target monitoring component is obtained, and based on the set of crack extension dimensions, the long-life monitoring data required for the target monitoring component is determined. Thus, the set of crack extension dimensions of the target monitoring component can be determined by comprehensively considering the basic data for stress calculation and the basic data for material experiment, and based on the set of crack extension dimensions, the long-life monitoring data required for the target monitoring component can be obtained.

[0201] On the basis of any of the above embodiments, based on the crack extension size set, the stress corrosion crack extension life is obtained, including the stress corrosion crack extension life based on the first parameter of the target monitoring component, the annual average stress corrosion crack extension rate test value of the material of the target monitoring component, and the low cycle fatigue critical crack size of the target monitoring component under the set working condition of the nuclear power steam turbine. Among them, the first parameter is the phased array detection crack depth of the target monitoring component or the stress corrosion crack extension size threshold value. Therefore, the method can comprehensively consider the first parameter of the target monitoring component, the annual average stress corrosion crack extension rate test value of the material of the target monitoring component, and the low cycle fatigue critical crack size of the target monitoring component under the set working condition of the nuclear power steam turbine to obtain the stress corrosion crack extension life.

[0202] The following takes the rotor as an example of the target monitoring component to describe how to obtain the stress corrosion crack growth life of the rotor.

[0203] Based on any of the above embodiments, Figure 3 As shown, the stress corrosion crack growth life of the rotor is obtained, including:

[0204] S301, obtaining basic stress calculation data and material test basic data of a nuclear power steam turbine rotor.

[0205] S302, determining a threshold value of a stress corrosion crack extension size of the rotor based on stress calculation basic data and material test basic data.

[0206] S303, based on the stress calculation basic data and the material test basic data, determine the low cycle fatigue critical crack size of the rotor of the nuclear power steam turbine in the normal shutdown transient condition.

[0207] For the relevant contents of steps S301 - S303 , please refer to the above embodiment and will not be described again here.

[0208] S304, based on the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the rotor material, and the low-cycle fatigue critical crack size of the rotor under normal shutdown transient conditions of the nuclear power steam turbine, the stress corrosion crack growth life is obtained.

[0209] In one embodiment, the calculation process of stress corrosion crack growth life is as follows:

[0210]

[0211] For example, continuing to take the welded low-pressure rotor of a certain type of 1200MW nuclear power steam turbine in the above embodiment as an example, the basic data for stress corrosion life damage design monitoring of the welded low-pressure rotor is shown in Table 9.

[0212] Table 9 Basic data for stress corrosion life damage design monitoring of welded low-pressure rotors

[0213]

[0214] The calculation process of stress corrosion crack growth life of welded low-pressure rotor is as follows:

[0215]

[0216] Therefore, if the target monitored component in this method is the rotor, the stress corrosion crack growth life can be obtained by comprehensively considering the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the rotor material, and the low-cycle fatigue critical crack size of the rotor under normal shutdown transient conditions of the nuclear power steam turbine.

[0217] The following takes the rotor blade root slot as an example of the target monitoring component to describe how to obtain the stress corrosion crack growth life of the rotor blade root slot.

[0218] Based on any of the above embodiments, if the target monitoring component is a rotor blade root slot, such as Figure 4 As shown, the stress corrosion crack growth life under different crack growth categories is obtained, including:

[0219] S401, based on the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the rotor material, and the low-cycle fatigue critical crack size of the rotor blade root slot under the normal shutdown transient condition of the nuclear power steam turbine, the stress corrosion crack growth life under any one of the first crack growth category, the third crack growth category, and the fourth crack growth category is obtained.

[0220] S402, based on the crack depth detected by phased array, the annual average stress corrosion crack growth rate test value of the rotor material, and the low-cycle fatigue critical crack size of the rotor blade root slot under the normal shutdown transient condition of the nuclear power steam turbine, the stress corrosion crack growth life under the second crack growth category is obtained.

[0221] In one embodiment, the calculation process of the stress corrosion crack growth life under any one of the first crack growth category, the third crack growth category and the fourth crack growth category is as follows:

[0222]

[0223] Among them, N fSCC1 is the stress corrosion crack growth life under the first crack growth category, N fSCC2 is the stress corrosion crack growth life under the third crack growth category, N fSCC4 It is the stress corrosion crack growth life under the fourth crack growth category.

[0224] In one embodiment, the stress corrosion crack growth life N under the second crack growth category fSCC2 The calculation process is as follows:

[0225]

[0226] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is the first crack growth category, and the stress corrosion crack growth life N of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A under the first crack growth category is fSCC1 The calculation process is as follows:

[0227]

[0228] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the crack extension category of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B is the first crack extension category, and the stress corrosion crack extension life N of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B under the first crack extension category is fSCC1 The calculation process is as follows:

[0229]

[0230] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the crack extension category of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is the second crack extension category, and the stress corrosion crack extension life N of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C under the second crack extension category is Fscc2 The calculation process is as follows:

[0231]

[0232] Therefore, in this method, if the target monitoring component is the rotor blade root slot, the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the rotor material, and the low cycle fatigue critical crack size of the rotor blade root slot under the normal shutdown transient condition of the nuclear power steam turbine can be comprehensively considered to obtain the stress corrosion crack growth life under any one of the first crack growth category, the third crack growth category, and the fourth crack growth category. In addition, the crack depth detected by the phased array, the annual average stress corrosion crack growth rate test value of the rotor material, and the low cycle fatigue critical crack size of the rotor blade root slot under the normal shutdown transient condition of the nuclear power steam turbine can be comprehensively considered to obtain the stress corrosion crack growth life under the second crack growth category.

[0233] The following takes the target monitoring component as a cylinder as an example to describe how to obtain the stress corrosion crack growth life of the cylinder.

[0234] Based on any of the above embodiments, Figure 5 As shown, the stress corrosion crack growth life of the cylinder is obtained, including:

[0235] S501, obtaining basic data for stress calculation and basic data for material testing of a cylinder of a nuclear power steam turbine.

[0236] S502, determining a set of crack extension dimensions based on stress calculation basic data and material experiment basic data.

[0237] For the relevant contents of steps S501-S502, please refer to the above embodiment and will not be repeated here.

[0238] S503, based on the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient working condition of the nuclear power steam turbine cold start, the first stress corrosion crack growth life is obtained.

[0239] In one embodiment, the first stress corrosion crack growth life N fSCC1 The calculation process is as follows:

[0240]

[0241] S504, based on the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient working condition of warm start of nuclear power steam turbine, the second stress corrosion crack growth life is obtained.

[0242] In one embodiment, the second stress corrosion crack growth life N fSCC2 The calculation process is as follows:

[0243]

[0244] S505, based on the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient working condition of the nuclear power steam turbine hot start, the third stress corrosion crack growth life is obtained.

[0245] In one embodiment, the third stress corrosion crack growth life N fSCC3 The calculation process is as follows:

[0246]

[0247] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E in the above embodiment as an example, the basic data for stress corrosion cracking design monitoring of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E is shown in Table 10.

[0248] Table 10 Basic data for design monitoring of stress corrosion cracking of low pressure inner cylinder

[0249]

[0250] The calculation process of the multi-type stress corrosion crack growth life of the No. 1 low-pressure inner cylinder of nuclear power steam turbine E is as follows:

[0251]

[0252]

[0253]

[0254] S506, determining the minimum value among the first stress corrosion crack growth life, the second stress corrosion crack growth life, and the third stress corrosion crack growth life as the stress corrosion crack growth life.

[0255] For example, taking the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E in the above embodiment as an example, the first stress corrosion crack growth life N of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E is fSCC1 The second stress corrosion crack growth life is 12.836 years. fSCC2 The third stress corrosion crack growth life is 11.690 years. fSCC3 =16.457 years, the stress corrosion crack growth life N of the No. 1 low-pressure inner cylinder of nuclear power steam turbine E fSCC The calculation process is as follows:

[0256] N fSCC =min{N fSCC1 ,N fSCC2 ,N fSCC3}=min{12.836,11.690,16.457}=11.690years

[0257] Therefore, if the target monitored component in this method is a cylinder, the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the cylinder material and the low-cycle fatigue critical crack size can be comprehensively considered to obtain multiple types of stress corrosion crack growth lives, and the minimum value of the multiple types of stress corrosion crack growth lives can be determined as the stress corrosion crack growth life.

[0258] The following takes the target monitoring component as an example of a cylinder to describe how to obtain the stress corrosion crack growth life under different crack growth categories.

[0259] Based on any of the above embodiments, if the target monitoring component is a cylinder, such as Figure 6 As shown, the stress corrosion crack growth life under the first crack growth category is obtained, including:

[0260] S601, based on the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient working condition of the nuclear power steam turbine cold start, the first stress corrosion crack growth life under the first crack growth category is obtained.

[0261] In one embodiment, the first stress corrosion crack growth life N under the first crack growth category fSCC1,1 The calculation process is as follows:

[0262]

[0263] S602, based on the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient working condition of warm start of nuclear power steam turbine, the second stress corrosion crack growth life under the first crack growth category is obtained.

[0264] In one embodiment, the first stress corrosion crack growth life N under the first crack growth category fSCC1,2 The calculation process is as follows:

[0265]

[0266] S603, based on the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient working condition of the nuclear power steam turbine hot start, the third stress corrosion crack growth life under the first crack growth category is obtained.

[0267] In one embodiment, the third stress corrosion crack growth life N under the first crack growth category fSCC1,3 The calculation process is as follows:

[0268]

[0269] S604, determining the stress corrosion crack growth life under the first crack growth category based on the first stress corrosion crack growth life under the first crack growth category, the second stress corrosion crack growth life under the first crack growth category, and the third stress corrosion crack growth life under the first crack growth category.

[0270] In one embodiment, based on the first stress corrosion crack growth life under the first crack growth category, the second stress corrosion crack growth life under the first crack growth category, and the third stress corrosion crack growth life under the first crack growth category, the stress corrosion crack growth life under the first crack growth category is determined, including taking a weighted average of the first stress corrosion crack growth life under the first crack growth category, the second stress corrosion crack growth life under the first crack growth category, and the third stress corrosion crack growth life under the first crack growth category to obtain the stress corrosion crack growth life under the first crack growth category.

[0271] In one embodiment, based on the first stress corrosion crack growth life under the first crack growth category, the second stress corrosion crack growth life under the first crack growth category, and the third stress corrosion crack growth life under the first crack growth category, the stress corrosion crack growth life under the first crack growth category is determined, including determining the minimum value of the first stress corrosion crack growth life under the first crack growth category, the second stress corrosion crack growth life under the first crack growth category, and the third stress corrosion crack growth life under the first crack growth category as the stress corrosion crack growth life under the first crack growth category.

[0272] For example, the stress corrosion crack growth life N under the first crack growth category is fSCC01 The calculation process is as follows:

[0273] N fSCC01 =min{N fSCC1,1 ,N fSCC1,2 ,N fSCC1,3}

[0274] For example, taking the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A in the above embodiment as an example, the crack growth category of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A is the first crack growth category, and the stress corrosion crack growth life N of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A under the first crack growth category is fSCC01 The calculation process is as follows:

[0275]

[0276]

[0277]

[0278] N fSCC01 =min{N fSCC1,1 ,N fSCC1,2 ,N fSCC1,3}=min{22.741,19.832,26.477}=19.832years

[0279] For example, taking the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B in the above embodiment as an example, the crack growth category of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B is the first crack growth category, and the stress corrosion crack growth life N of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B under the first crack growth category is fSCC01 The calculation process is as follows:

[0280]

[0281]

[0282]

[0283] N fSCC01 =min{N fSCC1,1 ,N fSCC1,2 ,N fSCC1,3}=min{22.741,19.832,26.477}=19.832years

[0284] For example, taking the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C in the above embodiment as an example, the crack growth category of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C is the first crack growth category, and the stress corrosion crack growth life N of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C under the first crack growth category is fSCC01 The calculation process is as follows:

[0285]

[0286]

[0287]

[0288] N fSCC01 =min{N fSCC1,1 ,N fSCC1,2 ,N fSCC1,3}=min{22.741,19.832,26.477}=19.832years

[0289] Therefore, in this method, if the target monitored component is a cylinder, the stress corrosion crack growth size threshold value, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size can be comprehensively considered to obtain the first to third stress corrosion crack growth lives under the first crack growth category, and then determine the stress corrosion crack growth life under the first crack growth category.

[0290] Based on any of the above embodiments, if the target monitoring component is a cylinder, such as Figure 7 As shown, the stress corrosion crack growth life under the second crack growth category is obtained, including:

[0291] S701, based on the crack depth detected by phased array, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient working condition of the nuclear power steam turbine cold start, the first stress corrosion crack growth life under the second crack growth category is obtained.

[0292] In one embodiment, the first stress corrosion crack growth life N under the second crack growth category fSCC2,1 The calculation process is as follows:

[0293]

[0294] S702, based on the crack depth detected by phased array, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient working condition of warm start of nuclear power steam turbine, the second stress corrosion crack growth life under the second crack growth category is obtained.

[0295] In one embodiment, the second stress corrosion crack growth life N under the second crack growth category fSCC2,2 The calculation process is as follows:

[0296]

[0297] S703, based on the crack depth detected by phased array, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size of the cylinder under the transient condition of hot start of nuclear power steam turbine, the third stress corrosion crack growth life under the second crack growth category is obtained.

[0298] In one embodiment, the third stress corrosion crack growth life N under the second crack growth category fSCC2,3 The calculation process is as follows:

[0299]

[0300] S703, determining the stress corrosion crack growth life under the second crack growth category based on the first stress corrosion crack growth life under the second crack growth category, the second stress corrosion crack growth life under the second crack growth category, and the third stress corrosion crack growth life under the second crack growth category.

[0301] In one embodiment, based on the first stress corrosion crack growth life under the second crack growth category, the second stress corrosion crack growth life under the second crack growth category, and the third stress corrosion crack growth life under the second crack growth category, the stress corrosion crack growth life under the second crack growth category is determined, including weighted averaging the first stress corrosion crack growth life under the second crack growth category, the second stress corrosion crack growth life under the second crack growth category, and the third stress corrosion crack growth life under the second crack growth category to obtain the stress corrosion crack growth life under the second crack growth category.

[0302] In one embodiment, based on the first stress corrosion crack growth life under the second crack growth category, the second stress corrosion crack growth life under the second crack growth category, and the third stress corrosion crack growth life under the second crack growth category, the stress corrosion crack growth life under the second crack growth category is determined, including determining the minimum value of the first stress corrosion crack growth life under the second crack growth category, the second stress corrosion crack growth life under the second crack growth category, and the third stress corrosion crack growth life under the second crack growth category as the stress corrosion crack growth life under the second crack growth category.

[0303] For example, the stress corrosion crack growth life N under the second crack growth category is fSCC02 The calculation process is as follows:

[0304] N fSCC02 =min{N fSCC2,1 ,N fSCC2,2 ,N fSCC2,3}

[0305] For example, taking the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D in the above embodiment as an example, the crack extension category of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D is the second crack extension category, and the stress corrosion crack extension life N of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D under the second crack extension category is fSCC02 The calculation process is as follows:

[0306]

[0307]

[0308]

[0309] N fSCC02 =min{N fSCC2,1 ,N fSCC2,2 ,N fSCC2,3}=min{21.583,18.675,25.319}=18.675 years

[0310] Therefore, if the target monitored component in this method is a cylinder, the crack depth detected by the phased array, the annual average stress corrosion crack growth rate test value of the cylinder material, and the low-cycle fatigue critical crack size can be comprehensively considered to obtain the first to third stress corrosion crack growth lives under the second crack growth category, and then determine the stress corrosion crack growth life under the second crack growth category.

[0311] The following describes how to obtain the crack propagation category of the target monitoring component.

[0312] In one embodiment, the method further includes obtaining a crack depth of the target monitored component detected by the phased array, and obtaining a crack extension category of the target monitored component based on the crack depth detected by the phased array.

[0313] It should be noted that the phased array detection of crack depth refers to the crack depth of the target monitoring component obtained by performing phased array detection on the target monitoring component. The phased array detection can be implemented by any phased array detection method in the relevant technology.

[0314] In some examples, the phased array detection crack depth of the target monitoring component of the nuclear power steam turbine is obtained, including performing phased array detection on the target monitoring component through a phased array ultrasonic flaw detector and a phased array probe to obtain the phased array detection crack depth. If no crack is found in the phased array detection of the target monitoring component, the phased array detection crack depth is given as a set value. It should be noted that the set value is not too limited, for example, it can be 0.002m (meter).

[0315] In some examples, based on the crack depth detected by the phased array, the crack extension category of the target monitored component is obtained, including obtaining the set interval in which the crack depth detected by the phased array is located, and based on the mapping relationship between the set interval and the crack extension category, the crack extension category of the target monitored component is obtained. It can be understood that a plurality of set intervals can be pre-divided for the crack depth detected by the phased array, and different set intervals can map different crack extension categories, or can map the same crack extension category.

[0316] For example, based on the crack depth detected by the phased array, the crack extension category of the target monitored component is obtained, including if the crack depth detected by the phased array is in a first set interval, determining the first crack extension category as the crack extension category of the target monitored component, or, if the crack depth detected by the phased array is in a second set interval, determining the second crack extension category as the crack extension category of the target monitored component.

[0317] In some examples, obtaining a crack extension category of a target monitored component based on crack depth detected by a phased array includes obtaining a crack extension category of a target monitored component based on crack depth detected by the phased array and a set of crack extension sizes.

[0318] In some examples, based on the phased array detection crack depth and crack extension size set, the crack extension category of the target monitoring component is obtained, including performing calculation processing on the crack depth detected by the phased array and the crack extension size in the crack extension size set to obtain a calculation result, and obtaining the crack extension category based on the correspondence between the calculation result and the crack extension category. The calculation processing can be implemented by at least one calculation processing method in the relevant technology, which is not limited here, for example, it can include addition, subtraction, multiplication, division, etc.

[0319] In some examples, the crack extension category of the target monitored component is obtained based on the phased array detected crack depth and the crack extension size set, including obtaining the size relationship between the phased array detected crack depth and at least one crack extension size in the crack extension size set, and determining the crack extension category of the target monitored component based on the corresponding relationship between the size relationship and the crack extension category.

[0320] The following takes the rotor blade root slot as an example of the target monitoring component to describe how to obtain the crack extension category of the rotor blade root slot.

[0321] In some examples, based on the phased array detection of crack depth and crack extension size set, the crack extension category of the rotor blade root slot is obtained, including the following possible implementations:

[0322] Method 1: If the crack depth detected by the phased array is less than the stress corrosion crack growth size threshold value, and the stress corrosion crack growth size threshold value is less than the high cycle fatigue crack growth size threshold value, the crack growth category is determined to be the first crack growth category.

[0323] In some examples, if the crack growth category is the first crack growth category, and the first crack growth category includes three stages, wherein in the first stage, the crack size of the rotor blade root slot is detected from the crack depth a detected by the phased array. i Extend to the stress corrosion crack growth size threshold a SCC In the second stage, the crack size of the rotor blade root groove increases from the stress corrosion crack growth threshold value a SCC Extended to the high cycle fatigue crack growth size threshold a th In the third stage, the crack size of the rotor blade root slot increases from the high cycle fatigue crack growth threshold value a th Extended to the critical crack size of low cycle fatigue a cj Among them, the critical crack size of low cycle fatigue is a cj for a cn or a c110% or a c120% .

[0324] Method 2: If the stress corrosion crack growth size threshold is smaller than the crack depth detected by the phased array, and the crack depth detected by the phased array is smaller than the high cycle fatigue crack growth size threshold, the crack growth category is determined to be the second crack growth category.

[0325] In some examples, if the crack growth category is the second crack growth category, and the second crack growth category includes two stages, wherein in the first stage, the crack size of the rotor blade root slot is detected from the crack depth a detected by the phased array. i Extended to the high cycle fatigue crack growth size threshold a thIn the second stage, the crack size of the rotor blade root slot increases from the high cycle fatigue crack growth threshold value a th Extended to the critical crack size of low cycle fatigue a cj .

[0326] Method 3: If the crack depth detected by the phased array is less than the high cycle fatigue crack growth size threshold value, and the high cycle fatigue crack growth size threshold value is less than the stress corrosion crack growth size threshold value, the crack growth category is determined to be the third crack growth category.

[0327] In some examples, if the crack growth category is the third crack growth category, and the third crack growth category includes three stages, wherein in the first stage, the crack size of the rotor blade root slot is detected from the crack depth a detected by the phased array. i Extended to the high cycle fatigue crack growth size threshold a th In the second stage, the crack size of the rotor blade root slot increases from the high cycle fatigue crack growth threshold value a th Extend to the stress corrosion crack growth size threshold a SCC In the third stage, the crack size of the rotor blade root groove increases from the stress corrosion crack growth threshold value a SCC Extended to the critical crack size of low cycle fatigue a cj .

[0328] Method 4: If the high cycle fatigue crack extension size threshold is smaller than the crack depth detected by the phased array, and the crack depth detected by the phased array is smaller than the stress corrosion crack extension size threshold, the crack extension category is determined to be the fourth crack extension category.

[0329] In some examples, if the crack growth category is the fourth crack growth category, and the fourth crack growth category includes two stages, wherein in the first stage, the crack size of the rotor blade root slot is detected from the crack depth a detected by the phased array. i Extend to the stress corrosion crack growth size threshold a SCC In the second stage, the crack size of the rotor blade root groove increases from the stress corrosion crack growth threshold value a SCC Extended to the critical crack size of low cycle fatigue a cj .

[0330] For example, taking the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the stress corrosion crack size threshold value a SCC The high cycle fatigue crack extension size threshold value a is 0.007980m. th The crack depth a of the phased array nondestructive testing is 0.023619m. i is 0.002m, due to a SCC =0.007980m th =0.023619m and a​i =0.002m SCC =0.007980m, the crack extension category of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of nuclear power steam turbine A is the first crack extension category.

[0331] For example, taking the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the stress corrosion crack size threshold value a SCC The high cycle fatigue crack extension size threshold value a is 0.007980m. th The crack depth a of the phased array nondestructive testing is 0.023619m. i is 0.005m, due to a SCC =0.007980m th =0.023619m and a i =0.005m SCC =0.007980m, the crack extension category of the 5th stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B is the first crack extension category.

[0332] For example, taking the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the stress corrosion crack size threshold value a SCC The high cycle fatigue crack extension size threshold value a is 0.007980m. th The crack depth a of the phased array nondestructive testing is 0.023619m. i is 0.010m, due to a SCC =0.007980m th =0.023619m and a i =0.010m>a SCC =0.007980m, the crack extension category of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of nuclear power steam turbine C is the second crack extension category.

[0333] The following takes the target monitoring component as a cylinder as an example to describe how to obtain the crack growth category of the cylinder.

[0334] In some examples, based on the phased array detection of crack depth and crack extension size set, the crack extension category of the cylinder is obtained, including the following possible implementations:

[0335] Method 1: If the crack depth detected by the phased array is less than the stress corrosion crack growth size threshold, the crack growth category is determined to be the first crack growth category.

[0336] ​​​​In some examples, if the crack growth category is the first crack growth category, and the first crack growth category includes two stages, wherein in the first stage, the crack size of the cylinder is detected from the crack depth a detected by the phased array. i Extend to the stress corrosion crack growth size threshold a SCC In the second stage, the crack size of the cylinder increases from the stress corrosion crack growth threshold value a SCC Extended to the critical crack size of low cycle fatigue a cj Among them, the critical crack size of low cycle fatigue is a cj for a cc or a cw or a ch .

[0337] Method 2: If the crack depth detected by the phased array is greater than the stress corrosion crack growth size threshold, the crack growth category is determined to be the second crack growth category.

[0338] In some examples, if the crack growth category is the second crack growth category, and the second crack growth category includes a stage, wherein in the first stage, the crack size of the cylinder is detected from the crack depth a detected by the phased array. i Extended to the critical crack size of low cycle fatigue a cj .

[0339] For example, taking the No. 1 low-pressure inner cylinder of nuclear power steam turbine A in the above embodiment as an example, the stress corrosion crack size threshold value a SCC The crack depth a of the phased array nondestructive testing is 0.008624m. i is 0.002m, due to a i =0.002m SCC =0.008624m, the crack extension category of the No. 1 low-pressure inner cylinder of nuclear power steam turbine A is the first crack extension category.

[0340] For example, taking the No. 2 low-pressure inner cylinder of nuclear power steam turbine B in the above embodiment as an example, the stress corrosion crack size threshold value a SCC The crack depth a of the phased array nondestructive testing is 0.008624m. i is 0.005m, due to a i =0.005m SCC =0.008624m, the crack extension category of the No. 2 low-pressure inner cylinder of nuclear power steam turbine B is the first crack extension category.

[0341] For example, taking the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C in the above embodiment as an example, the stress corrosion crack size threshold value a SCC The crack depth a of the phased array nondestructive testing is 0.008624m. i is 0.005m, due to a​​i =0.005m SCC =0.008624m, the crack extension category of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C is the first crack extension category.

[0342] For example, taking the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D in the above embodiment as an example, the stress corrosion crack size threshold value a SCC The crack depth a of the phased array nondestructive testing is 0.008624m. i is 0.010m, due to a i =0.010m>a SCC =0.008624m, the crack extension category of the No. 2 low-pressure inner cylinder of nuclear power steam turbine D is the second crack extension category.

[0343] On the basis of any of the above embodiments, the fatigue crack growth life includes the low-cycle fatigue crack growth life, and based on the crack growth size set, the low-cycle fatigue crack growth life is obtained, including the low-cycle fatigue crack growth life of at least one stage of the nuclear power steam turbine set working condition based on the second parameter of the target monitoring component, the crack shape parameter of the target monitoring component, the low-cycle fatigue crack growth test constant of the material of the target monitoring component, and the maximum stress of the crack part of the target monitoring component under the set working condition of the nuclear power steam turbine. Among them, the second parameter is any parameter in the phased array detection crack depth, initial crack size, and crack growth size set of the target monitoring component. Therefore, the method can comprehensively consider the second parameter of the target monitoring component, the crack shape parameter of the target monitoring component, the low-cycle fatigue crack growth test constant of the material of the target monitoring component, and the maximum stress of the crack part of the target monitoring component under the set working condition of the nuclear power steam turbine, and obtain the low-cycle fatigue crack growth life of at least one stage of the nuclear power steam turbine set working condition.

[0344] The following takes the rotor as an example of the target monitoring component to describe how to obtain the low-cycle fatigue crack growth life of the rotor.

[0345] Based on any of the above embodiments, the crack expansion stage of the rotor includes three stages, wherein in the first stage, the crack size of the rotor increases from the initial crack size a 0 Extended to the high cycle fatigue crack growth size threshold a th In the second stage, the crack size of the rotor increases from the high cycle fatigue crack growth threshold value a th Extend to the stress corrosion crack growth size threshold a SCC In the third stage, the crack size of the rotor increases from the stress corrosion crack growth threshold value a SCC Extended to the critical crack size of low cycle fatigue a cj Among them, the critical crack size of low cycle fatigue is a cj for a cn ​or a c110% or a c120% .

[0346] Based on any of the above embodiments, Figure 8 As shown, the low cycle fatigue crack growth life of the rotor is obtained, including:

[0347] S801, obtaining basic stress calculation data and material test basic data of a nuclear power steam turbine rotor.

[0348] S802: Determine a crack extension size set of the rotor based on stress calculation basic data and material test basic data.

[0349] For the relevant contents of steps S801-S802, please refer to the above embodiment and will not be repeated here.

[0350] S803, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the first stage of the normal shutdown transient condition of the nuclear power steam turbine.

[0351] In one embodiment, based on a crack extension size set, a low-cycle fatigue crack extension life of a first stage of a nuclear power steam turbine normal shutdown transient operating condition is obtained, including an initial crack size of the rotor, a high-cycle fatigue crack extension size threshold value, a crack shape parameter of the rotor, a low-cycle fatigue crack extension test constant of the rotor material, and a maximum stress at a rotor crack site of a nuclear power steam turbine normal shutdown transient operating condition, to obtain a low-cycle fatigue crack extension life of a first stage of a nuclear power steam turbine normal shutdown transient operating condition.

[0352] In some examples, the low-cycle fatigue crack growth life N of the first stage of the normal shutdown transient condition of a nuclear power steam turbine is fn,1 The calculation process is as follows:

[0353]

[0354] Among them, C 0 、m 0 Low cycle fatigue crack growth test constant of rotor material.

[0355] S804, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the second stage of the normal shutdown transient condition of the nuclear power steam turbine.

[0356] In one embodiment, based on the crack growth size set, the low-cycle fatigue crack growth life of the second stage of the normal shutdown transient condition of the nuclear power steam turbine is obtained, including based on the high-cycle fatigue crack growth size threshold value, the stress corrosion crack growth size threshold value, the crack shape parameters of the rotor, the low-cycle fatigue crack growth test constants of the rotor material, and the maximum stress of the rotor crack site of the normal shutdown transient condition of the nuclear power steam turbine, to obtain the low-cycle fatigue crack growth life of the second stage of the normal shutdown transient condition of the nuclear power steam turbine.

[0357] In some examples, the low-cycle fatigue crack growth life N of the second stage of the normal shutdown transient condition of a nuclear power steam turbine is fn,2 The calculation process is as follows:

[0358]

[0359] S805, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the third stage of the normal shutdown transient condition of the nuclear power steam turbine.

[0360] In one embodiment, based on the crack extension size set, the low-cycle fatigue crack extension life of the third stage of the normal shutdown transient condition of the nuclear power steam turbine is obtained, including the low-cycle fatigue critical crack size of the rotor under the normal shutdown transient condition of the nuclear power steam turbine based on the stress corrosion crack extension size threshold value, the low-cycle fatigue critical crack size of the rotor under the normal shutdown transient condition of the nuclear power steam turbine, the crack shape parameters of the rotor, the low-cycle fatigue crack extension test constant of the rotor material, and the maximum stress of the rotor crack site under the normal shutdown transient condition of the nuclear power steam turbine, so as to obtain the low-cycle fatigue crack extension life of the third stage of the normal shutdown transient condition of the nuclear power steam turbine.

[0361] In some examples, the low-cycle fatigue crack growth life N of the third stage of the normal shutdown transient condition of a nuclear power steam turbine is fn,3 The calculation process is as follows:

[0362]

[0363] S806, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the first stage of the nuclear power steam turbine 110% overspeed test transient condition.

[0364] In one embodiment, based on a crack extension size set, a low-cycle fatigue crack extension life of a nuclear power steam turbine in the first stage of a 110% overspeed test transient condition is obtained, including an initial crack size of the rotor, a high-cycle fatigue crack extension size threshold, a crack shape parameter of the rotor, a low-cycle fatigue crack extension test constant of the rotor material, and a maximum stress at a rotor crack site of a nuclear power steam turbine in a 110% overspeed test transient condition, to obtain a low-cycle fatigue crack extension life of a nuclear power steam turbine in the first stage of a 110% overspeed test transient condition.

[0365] In some examples, the low-cycle fatigue crack growth life N of the first stage of transient conditions of a nuclear power steam turbine 110% overspeed test is f110%,1 The calculation process is as follows:

[0366]

[0367] S807, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the second stage of the nuclear power steam turbine 110% overspeed test transient condition.

[0368] In one embodiment, based on the crack extension size set, the low-cycle fatigue crack extension life of the second stage of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including based on the high-cycle fatigue crack extension size threshold value, the stress corrosion crack extension size threshold value, the crack shape parameters of the rotor, the rotor material low-cycle fatigue crack extension test constant, and the maximum stress of the rotor crack site of the nuclear power steam turbine 110% overspeed test transient condition, to obtain the low-cycle fatigue crack extension life of the second stage of the nuclear power steam turbine 110% overspeed test transient condition.

[0369] In some examples, the low-cycle fatigue crack growth life N of the second stage of the transient condition of the nuclear power steam turbine 110% overspeed test is f110%,2 The calculation process is as follows:

[0370]

[0371] S808, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the third stage of the nuclear power steam turbine 110% overspeed test transient condition.

[0372] In one embodiment, based on the crack extension size set, the low-cycle fatigue crack extension life of the third stage of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including the low-cycle fatigue critical crack size of the rotor of the nuclear power steam turbine 110% overspeed test transient condition, the crack shape parameters of the rotor, the rotor material low-cycle fatigue crack extension test constant, and the maximum stress of the rotor crack site of the nuclear power steam turbine 110% overspeed test transient condition, so as to obtain the low-cycle fatigue crack extension life of the third stage of the nuclear power steam turbine 110% overspeed test transient condition.

[0373] In some examples, the low-cycle fatigue crack growth life N of the third stage of transient conditions of a nuclear power steam turbine 110% overspeed test is f110%,3 The calculation process is as follows:

[0374]

[0375] S809, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the first stage of the nuclear power steam turbine 120% overspeed transient operating condition.

[0376] In one embodiment, based on a crack extension size set, a low-cycle fatigue crack extension life of a nuclear power steam turbine in the first stage of a 120% overspeed transient operating condition is obtained, including an initial crack size of the rotor, a high-cycle fatigue crack extension size threshold value, a crack shape parameter of the rotor, a low-cycle fatigue crack extension test constant of the rotor material, and a maximum stress at a rotor crack site in a nuclear power steam turbine in a 120% overspeed transient operating condition, to obtain a low-cycle fatigue crack extension life of a nuclear power steam turbine in the first stage of a 120% overspeed transient operating condition.

[0377] In some examples, the low-cycle fatigue crack growth life N of the first stage of a nuclear power steam turbine transient operating condition of 120% overspeed operation is f120%,1 The calculation process is as follows:

[0378]

[0379] S810, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the second stage of the nuclear power steam turbine 120% overspeed transient operating condition.

[0380] In one embodiment, based on the crack extension size set, the low-cycle fatigue crack extension life of the second stage of the nuclear power steam turbine 120% overspeed transient operating condition is obtained, including based on the high-cycle fatigue crack extension size threshold value, the stress corrosion crack extension size threshold value, the crack shape parameters of the rotor, the rotor material low-cycle fatigue crack extension test constants, and the maximum stress of the rotor crack site of the nuclear power steam turbine 120% overspeed transient operating condition, to obtain the low-cycle fatigue crack extension life of the second stage of the nuclear power steam turbine 120% overspeed transient operating condition.

[0381] In some examples, the low-cycle fatigue crack growth life N of the second stage of a nuclear power steam turbine under 120% overspeed transient condition is f120%,2 The calculation process is as follows:

[0382]

[0383] S811, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the third stage of the nuclear power steam turbine 120% overspeed transient operating condition.

[0384] In one embodiment, based on a crack extension size set, a low-cycle fatigue crack extension life of a third stage of a nuclear power steam turbine under a 120% overspeed transient operating condition is obtained, including a stress corrosion crack extension size threshold value, a low-cycle fatigue critical crack size of a rotor under a 120% overspeed transient operating condition of a nuclear power steam turbine, a crack shape parameter of a rotor, a low-cycle fatigue crack extension test constant of a rotor material, and a maximum stress at a rotor crack site under a 120% overspeed transient operating condition of a nuclear power steam turbine, to obtain a low-cycle fatigue crack extension life of a third stage of a nuclear power steam turbine under a 120% overspeed transient operating condition.

[0385] In some examples, the low-cycle fatigue crack growth life N of the third stage of a nuclear power steam turbine under 120% overspeed transient condition is f120%,3 The calculation process is as follows:

[0386]

[0387] For example, continuing to take the welded low-pressure rotor of a certain type of 1200MW nuclear power steam turbine in the above embodiment as an example, the basic data for low-cycle fatigue life damage design monitoring of the welded low-pressure rotor is shown in Table 11.

[0388] Table 11 Basic data for low cycle fatigue life damage design monitoring of welded low pressure rotor

[0389]

[0390] The calculation process of the low cycle fatigue crack growth life of the rotor is as follows:

[0391]

[0392]

[0393]

[0394]

[0395]

[0396]

[0397]

[0398]

[0399]

[0400] Therefore, in this method, if the target monitoring component is the rotor, the low-cycle fatigue crack growth life can be obtained by comprehensively considering the crack shape parameters of the rotor, the low-cycle fatigue crack growth test constants of the rotor material, the maximum stress at the rotor crack site, and the crack growth size set of the rotor.

[0401] The following takes the rotor blade root slot as an example of the target monitoring component to describe how to obtain the low cycle fatigue crack growth life of the rotor blade root slot.

[0402] Based on any of the above embodiments, if the target monitoring component is a rotor blade root slot, such as Fig. 9 As shown in the figure, the low cycle fatigue crack growth life of nuclear power steam turbine under normal shutdown transient conditions under different crack growth categories is obtained, including:

[0403] S901, obtaining the low cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0404] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine under normal shutdown transient operating conditions is obtained, including crack depth based on phased array detection, stress corrosion crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the rotor blade root slot crack site under normal shutdown transient operating conditions of the nuclear power steam turbine, to obtain the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine under normal shutdown transient operating conditions.

[0405] In some examples, the low-cycle fatigue crack growth life N of the first stage of the first crack growth category of a nuclear power steam turbine in a normal shutdown transient condition is fn1,1 The calculation process is as follows:

[0406]

[0407] Among them, C 0 、m 0 Low cycle fatigue crack growth test constant of rotor material.

[0408] S902, obtaining the low cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0409] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine normal shutdown transient operating condition is obtained, including based on the stress corrosion crack growth size threshold value, the high-cycle fatigue crack growth size threshold value, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress of the rotor blade root slot crack site of the nuclear power steam turbine normal shutdown transient operating condition, to obtain the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine normal shutdown transient operating condition.

[0410] In some examples, the low-cycle fatigue crack growth life N of the second stage of the first crack growth category of a nuclear power steam turbine in a normal shutdown transient condition is fn1,2 The calculation process is as follows:

[0411]

[0412] S903, obtaining the low cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0413] In one embodiment, the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine normal shutdown transient operating condition is obtained, including the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine normal shutdown transient operating condition based on the high-cycle fatigue crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine normal shutdown transient operating condition, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constants, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine normal shutdown transient operating condition, so as to obtain the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine normal shutdown transient operating condition.

[0414] In some examples, the low-cycle fatigue crack growth life N of the third stage of the first crack growth category of a nuclear power steam turbine in a normal shutdown transient condition is fn1,3 The calculation process is as follows:

[0415]

[0416] S904, obtaining the low cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0417] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine under normal shutdown transient operating conditions is obtained, including crack depth based on phased array detection, high-cycle fatigue crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the rotor blade root slot crack site under normal shutdown transient operating conditions of the nuclear power steam turbine, to obtain the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine under normal shutdown transient operating conditions.

[0418] In some examples, the low-cycle fatigue crack growth life N of the first stage of the second crack growth category of a nuclear power steam turbine in a normal shutdown transient condition is fn2,1 The calculation process is as follows:

[0419]

[0420] S905, obtaining the low cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0421] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine normal shutdown transient operating condition is obtained, including the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine normal shutdown transient operating condition based on the high-cycle fatigue crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine normal shutdown transient operating condition, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constants, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine normal shutdown transient operating condition, so as to obtain the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine normal shutdown transient operating condition.

[0422] In some examples, the low-cycle fatigue crack growth life N of the second stage of the second crack growth category of a nuclear power steam turbine in a normal shutdown transient condition is fn2,2 The calculation process is as follows:

[0423]

[0424] S906, obtaining the low cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0425] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine under normal shutdown transient operating conditions is obtained, including crack depth based on phased array detection, high-cycle fatigue crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the rotor blade root slot crack site under normal shutdown transient operating conditions of the nuclear power steam turbine, to obtain the low-cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine under normal shutdown transient operating conditions.

[0426] In some examples, the low-cycle fatigue crack growth life N of the first stage of the third crack growth category of a nuclear power steam turbine in normal shutdown transient conditions is fn3,1 The calculation process is as follows:

[0427]

[0428] S907, obtaining the low cycle fatigue crack growth life of the second stage of the third crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0429] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the third crack growth category of the normal shutdown transient condition of the nuclear power steam turbine is obtained, including the low-cycle fatigue crack growth life of the second stage of the third crack growth category of the normal shutdown transient condition of the nuclear power steam turbine based on the high-cycle fatigue crack growth size threshold value, the stress corrosion crack growth size threshold value, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the rotor blade root slot crack site of the normal shutdown transient condition of the nuclear power steam turbine.

[0430] In some examples, the low-cycle fatigue crack growth life N of the second stage of the third crack growth category of a nuclear power steam turbine in normal shutdown transient conditions is fn3,2 The calculation process is as follows:

[0431]

[0432] S908, obtaining the low cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0433] In one embodiment, the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine normal shutdown transient operating condition is obtained, including the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine normal shutdown transient operating condition based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine normal shutdown transient operating condition, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine normal shutdown transient operating condition, so as to obtain the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine normal shutdown transient operating condition.

[0434] In some examples, the low-cycle fatigue crack growth life N of the third stage of the third crack growth category of a nuclear power steam turbine in a normal shutdown transient condition is fn3,3 The calculation process is as follows:

[0435]

[0436] S909, obtaining the low cycle fatigue crack growth life of the first stage of the fourth crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0437] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the fourth crack growth category of the nuclear power steam turbine under normal shutdown transient operating conditions is obtained, including crack depth based on phased array detection, stress corrosion crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the crack site of the rotor blade root slot under normal shutdown transient operating conditions of the nuclear power steam turbine, to obtain the low-cycle fatigue crack growth life of the first stage of the fourth crack growth category of the nuclear power steam turbine under normal shutdown transient operating conditions.

[0438] In some examples, the low-cycle fatigue crack growth life N of the first stage of the fourth crack growth category of a nuclear power steam turbine in a normal shutdown transient condition is fn4,1 The calculation process is as follows:

[0439]

[0440] S910, obtaining the low cycle fatigue crack growth life of the second stage of the fourth crack growth category of the nuclear power steam turbine in the normal shutdown transient condition.

[0441] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the fourth crack growth category of the normal shutdown transient condition of the nuclear power steam turbine is obtained, including the low-cycle fatigue crack growth life of the second stage of the fourth crack growth category of the normal shutdown transient condition of the nuclear power steam turbine based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the normal shutdown transient condition of the nuclear power steam turbine, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot of the normal shutdown transient condition of the nuclear power steam turbine, so as to obtain the low-cycle fatigue crack growth life of the second stage of the fourth crack growth category of the normal shutdown transient condition of the nuclear power steam turbine.

[0442] In some examples, the low-cycle fatigue crack growth life N of the second stage of the fourth crack growth category of a nuclear power steam turbine in a normal shutdown transient condition is fn4,2 The calculation process is as follows:

[0443]

[0444] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is the first crack extension category, and the normal shutdown low-cycle fatigue stress and material test basic data of the No. 1 low-pressure rotor of the nuclear power steam turbine A are shown in Table 12.

[0445] Table 12 Basic data of normal shutdown low-cycle fatigue stress and material test of low-pressure rotor of nuclear power steam turbine

[0446]

[0447] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of nuclear power steam turbine A under normal shutdown transient conditions is as follows:

[0448]

[0449]

[0450]

[0451] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the crack extension category of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B is the first crack extension category, and the normal shutdown low-cycle fatigue stress and material test basic data of the No. 2 low-pressure rotor of the nuclear power steam turbine B are shown in Table 12.

[0452] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B under normal shutdown transient conditions is as follows:

[0453]

[0454]

[0455]

[0456] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is the second crack extension category, and the normal shutdown low-cycle fatigue stress and material test basic data of the No. 3 low-pressure rotor of the nuclear power steam turbine C are shown in Table 12.

[0457] The calculation process of the low-cycle fatigue crack growth life of the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor under the normal shutdown transient condition of nuclear power steam turbine C under the second crack growth category is as follows:

[0458]

[0459]

[0460] Therefore, if the target monitoring component in this method is the rotor blade root slot, the crack shape parameters of the rotor blade root slot, the low-cycle fatigue crack growth test constants of the rotor material, the maximum stress at the crack site of the rotor blade root slot under the normal shutdown transient condition of the nuclear power steam turbine, and the crack growth size set of the rotor blade root slot can be comprehensively considered to obtain the low-cycle fatigue crack growth life under different crack growth categories under the normal shutdown transient condition of the nuclear power steam turbine.

[0461] Based on any of the above embodiments, if the target monitoring component is a rotor blade root slot, such as Fig.10 As shown in the figure, the low cycle fatigue crack growth life of nuclear power steam turbine under different crack growth categories under 110% overspeed test transient conditions is obtained, including:

[0462] S1001, obtaining the low cycle fatigue crack growth life of the first stage of the first crack growth category of a nuclear power steam turbine in a 110% overspeed test transient condition.

[0463] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including crack depth based on phased array detection, stress corrosion crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the rotor blade root slot crack site of the nuclear power steam turbine 110% overspeed test transient condition, to obtain the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0464] In some examples, the low-cycle fatigue crack growth life N of the first stage of the first crack growth category of a nuclear power steam turbine 110% overspeed test transient condition is f110%1,1 The calculation process is as follows:

[0465]

[0466] S1002, obtaining the low cycle fatigue crack growth life of the second stage of the first crack growth category of a nuclear power steam turbine 110% overspeed test transient condition.

[0467] In one embodiment, the low cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including based on the stress corrosion crack growth size threshold value, the high cycle fatigue crack growth size threshold value, the crack shape parameters of the rotor blade root slot, the rotor material low cycle fatigue crack growth test constant, and the maximum stress of the rotor blade root slot crack site of the nuclear power steam turbine 110% overspeed test transient condition, to obtain the low cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0468] In some examples, the low-cycle fatigue crack growth life N of the second stage of the first crack growth category of a nuclear power steam turbine 110% overspeed test transient condition is f110%1,2 The calculation process is as follows:

[0469]

[0470] S1003, obtaining the low cycle fatigue crack growth life of the third stage of the first crack growth category of the transient operating condition of the nuclear power steam turbine 110% overspeed test.

[0471] In one embodiment, the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine 110% overspeed test transient condition based on the high-cycle fatigue crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine 110% overspeed test transient condition, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine 110% overspeed test transient condition, so as to obtain the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0472] In some examples, the low cycle fatigue crack growth life N of the third stage of the first crack growth category of a nuclear power steam turbine transient condition under 110% overspeed test is f110%1,3 The calculation process is as follows:

[0473]

[0474] S1004, obtaining the low cycle fatigue crack growth life of the first stage of the second crack growth category of the transient condition of the nuclear power steam turbine 110% overspeed test.

[0475] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including the crack depth detected by phased array, the high-cycle fatigue crack growth size threshold, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constants, and the maximum stress at the rotor blade root slot crack site of the nuclear power steam turbine 110% overspeed test transient condition, so as to obtain the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0476] In some examples, the low-cycle fatigue crack growth life N of the first stage of the second crack growth category of a nuclear power steam turbine 110% overspeed test transient condition is f110%2,1 The calculation process is as follows:

[0477]

[0478] S1005, obtaining the low cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine in the transient condition of the 110% overspeed test.

[0479] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine 110% overspeed test transient condition based on the high-cycle fatigue crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine 110% overspeed test transient condition, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine 110% overspeed test transient condition, so as to obtain the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0480] In some examples, the low-cycle fatigue crack growth life N of the second stage of the second crack growth category of a nuclear power steam turbine 110% overspeed test transient condition is f110%2,2 The calculation process is as follows:

[0481]

[0482] S1006, obtaining the low cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0483] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including crack depth based on phased array detection, high-cycle fatigue crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the rotor blade root slot crack site of the nuclear power steam turbine 110% overspeed test transient condition, to obtain the low-cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0484] In some examples, the low-cycle fatigue crack growth life N of the first stage of the third crack growth category of a nuclear power steam turbine 110% overspeed test transient condition is f110%3,1 The calculation process is as follows:

[0485]

[0486] S1007, obtaining the low cycle fatigue crack growth life of the second stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0487] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including based on the high-cycle fatigue crack growth size threshold value, the stress corrosion crack growth size threshold value, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the rotor blade root slot crack site of the nuclear power steam turbine 110% overspeed test transient condition, to obtain the low-cycle fatigue crack growth life of the second stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0488] In some examples, the low-cycle fatigue crack growth life N of the second stage of the third crack growth category of a nuclear power steam turbine 110% overspeed test transient condition is f110%3,2 The calculation process is as follows:

[0489]

[0490] S1008, obtaining the low cycle fatigue crack growth life of the third crack growth category and the third stage of the transient operating condition of the nuclear power steam turbine 110% overspeed test.

[0491] In one embodiment, the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine 110% overspeed test transient condition, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine 110% overspeed test transient condition, so as to obtain the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0492] In some examples, the low-cycle fatigue crack growth life N of the third crack growth category and the third stage of the transient condition of the nuclear power steam turbine 110% overspeed test is f110%3,3 The calculation process is as follows:

[0493]

[0494] S1009, obtaining the low cycle fatigue crack growth life of the first stage of the fourth crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0495] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the fourth crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including crack depth based on phased array detection, stress corrosion crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the rotor blade root slot crack site of the nuclear power steam turbine 110% overspeed test transient condition, to obtain the low-cycle fatigue crack growth life of the first stage of the fourth crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0496] In some examples, the low-cycle fatigue crack growth life N of the first stage of the fourth crack growth category of a nuclear power steam turbine 110% overspeed test transient condition is f110%4,1 The calculation process is as follows:

[0497]

[0498] S1010, obtaining the low cycle fatigue crack growth life of the second stage of the fourth crack growth category of a nuclear power steam turbine 110% overspeed test transient condition.

[0499] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the fourth crack growth category of the nuclear power steam turbine 110% overspeed test transient condition is obtained, including based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine 110% overspeed test transient condition, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the rotor blade root slot crack site of the nuclear power steam turbine 110% overspeed test transient condition, to obtain the low-cycle fatigue crack growth life of the second stage of the fourth crack growth category of the nuclear power steam turbine 110% overspeed test transient condition.

[0500] In some examples, the low-cycle fatigue crack growth life N of the second stage of the fourth crack growth category of the transient condition of the nuclear power steam turbine 110% overspeed test is f110%4,2 The calculation process is as follows:

[0501]

[0502] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the crack propagation category of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is the first crack propagation category, and the 110% overspeed test low-cycle fatigue stress and material test basic data of the No. 1 low-pressure rotor of the nuclear power steam turbine A are shown in Table 13.

[0503] Table 13 Basic data of low cycle fatigue stress and material test of low pressure rotor of nuclear power steam turbine in 110% overspeed test

[0504]

[0505] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A110% overspeed test transient condition is as follows:

[0506]

[0507]

[0508]

[0509] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the crack propagation category of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B is the first crack propagation category, and the 110% overspeed test low-cycle fatigue stress and material test basic data of the No. 2 low-pressure rotor of the nuclear power steam turbine B are shown in Table 13.

[0510] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor in the transient condition of the nuclear power steam turbine B110% overspeed test is as follows:

[0511]

[0512]

[0513]

[0514] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the crack propagation category of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is the second crack propagation category, and the 110% overspeed test low-cycle fatigue stress and material test basic data of the No. 3 low-pressure rotor of the nuclear power steam turbine C are shown in Table 13.

[0515] The calculation process of the low-cycle fatigue crack growth life of the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor under the transient condition of the nuclear power steam turbine C110% overspeed test under the second crack growth category is as follows:

[0516]

[0517]

[0518] Therefore, if the target monitoring component in this method is the rotor blade root slot, the crack shape parameters of the rotor blade root slot, the low-cycle fatigue crack growth test constants of the rotor material, the maximum stress at the crack site of the rotor blade root slot under the transient working condition of the nuclear power steam turbine 110% overspeed test, and the crack growth size set of the rotor blade root slot can be comprehensively considered to obtain the low-cycle fatigue crack growth life under different crack growth categories under the transient working condition of the nuclear power steam turbine 110% overspeed test.

[0519] Based on any of the above embodiments, if the target monitoring component is a rotor blade root slot, such as Fig.11 As shown in the figure, the low cycle fatigue crack growth life of nuclear power steam turbine under different crack growth categories under 120% overspeed transient operation conditions is obtained, including:

[0520] S1101, obtaining the low cycle fatigue crack growth life of the first stage of the first crack growth category of a nuclear power steam turbine in a 120% overspeed transient operation condition.

[0521] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation is obtained, including the crack depth based on phased array detection, the stress corrosion crack growth size threshold value, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot in the transient operating condition of 120% overspeed operation of the nuclear power steam turbine, so as to obtain the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation.

[0522] In some examples, the low-cycle fatigue crack growth life N of the first stage of the first crack growth category of a nuclear power steam turbine in a 120% overspeed transient operation condition is f120%1,1 The calculation process is as follows:

[0523]

[0524] S1102, obtaining the low cycle fatigue crack growth life of the second stage of the first crack growth category of a nuclear power steam turbine in a transient operating condition of 120% overspeed operation.

[0525] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation is obtained, including based on the stress corrosion crack growth size threshold value, the high-cycle fatigue crack growth size threshold value, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress of the rotor blade root slot crack site in the transient operating condition of 120% overspeed operation of the nuclear power steam turbine, to obtain the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation.

[0526] In some examples, the low-cycle fatigue crack growth life N of the second stage of the first crack growth category of a nuclear power steam turbine under 120% overspeed transient operation is f120%1,2 The calculation process is as follows:

[0527]

[0528] S1103, obtaining the low cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation.

[0529] In one embodiment, the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine under the transient operating condition of 120% overspeed is obtained, including the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine under the transient operating condition of 120% overspeed based on the high-cycle fatigue crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine under the transient operating condition of 120% overspeed, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine under the transient operating condition of 120% overspeed, so as to obtain the low-cycle fatigue crack growth life of the third stage of the first crack growth category of the nuclear power steam turbine under the transient operating condition of 120% overspeed.

[0530] In some examples, the low-cycle fatigue crack growth life N of the third stage of the first crack growth category of a nuclear power steam turbine in a transient condition of 120% overspeed operation is f120%1,3 The calculation process is as follows:

[0531]

[0532] S1104, obtaining the low cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation.

[0533] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine under the transient operating condition of 120% overspeed is obtained, including the crack depth detected by phased array, the high-cycle fatigue crack growth size threshold, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constants, and the maximum stress of the rotor blade root slot crack site under the transient operating condition of 120% overspeed of the nuclear power steam turbine, so as to obtain the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine under the transient operating condition of 120% overspeed.

[0534] In some examples, the low-cycle fatigue crack growth life N of the first stage of the second crack growth category of a nuclear power steam turbine under 120% overspeed transient operation is f120%2,1 The calculation process is as follows:

[0535]

[0536] S1105, obtaining the low cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation.

[0537] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine under the transient operating condition of 120% overspeed is obtained, including the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine under the transient operating condition of 120% overspeed based on the high-cycle fatigue crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine under the transient operating condition of 120% overspeed, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine under the transient operating condition of 120% overspeed, so as to obtain the low-cycle fatigue crack growth life of the second stage of the second crack growth category of the nuclear power steam turbine under the transient operating condition of 120% overspeed.

[0538] In some examples, the low-cycle fatigue crack growth life N of the second crack growth category and the second stage of the transient condition of nuclear power steam turbine 120% overspeed operation is f120%2,2 The calculation process is as follows:

[0539]

[0540] S1106, obtaining the low cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation.

[0541] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions is obtained, including crack depth based on phased array detection, high-cycle fatigue crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the rotor blade root slot crack site under 120% overspeed transient operating conditions of the nuclear power steam turbine, to obtain the low-cycle fatigue crack growth life of the first stage of the third crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions.

[0542] In some examples, the low-cycle fatigue crack growth life N of the first stage of the third crack growth category of a nuclear power steam turbine under 120% overspeed transient operation is f120%3,1 The calculation process is as follows:

[0543]

[0544] S1107, obtaining the low cycle fatigue crack growth life of the second stage of the third crack growth category of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation.

[0545] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the third crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions is obtained, including based on the high-cycle fatigue crack growth size threshold, the stress corrosion crack growth size threshold, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constants, and the maximum stress at the rotor blade root slot crack site under the nuclear power steam turbine under 120% overspeed transient operating conditions, to obtain the low-cycle fatigue crack growth life of the second stage of the third crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions.

[0546] In some examples, the low-cycle fatigue crack growth life N of the second stage of the third crack growth category of a nuclear power steam turbine under 120% overspeed transient operation is f120%3,2 The calculation process is as follows:

[0547]

[0548] S1108, obtaining the low cycle fatigue crack growth life of the third crack growth category and the third stage of the nuclear power steam turbine in the transient operating condition of 120% overspeed operation.

[0549] In one embodiment, the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine under 120% overspeed transient operation condition is obtained, including the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine under 120% overspeed transient operation condition based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine under 120% overspeed transient operation condition, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constant, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine under 120% overspeed transient operation condition, so as to obtain the low-cycle fatigue crack growth life of the third stage of the third crack growth category of the nuclear power steam turbine under 120% overspeed transient operation condition.

[0550] In some examples, the low-cycle fatigue crack growth life N of the third crack growth category and the third stage of the transient condition of nuclear power steam turbine 120% overspeed operation is f120%3,3 The calculation process is as follows:

[0551]

[0552] S1109, obtaining the low cycle fatigue crack growth life of the first stage of the fourth crack growth category of a nuclear power steam turbine in a transient operating condition of 120% overspeed operation.

[0553] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the fourth crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions is obtained, including crack depth based on phased array detection, stress corrosion crack growth size threshold, crack shape parameters of the rotor blade root slot, rotor material low-cycle fatigue crack growth test constants, and maximum stress at the rotor blade root slot crack site under 120% overspeed transient operating conditions of the nuclear power steam turbine, to obtain the low-cycle fatigue crack growth life of the first stage of the fourth crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions.

[0554] In some examples, the low-cycle fatigue crack growth life N of the first stage of the fourth crack growth category of a nuclear power steam turbine under 120% overspeed transient operation is f120%4,1 The calculation process is as follows:

[0555]

[0556] S1110, obtaining the low cycle fatigue crack growth life of the second stage of the fourth crack growth category of a nuclear power steam turbine in a transient operating condition of 120% overspeed operation.

[0557] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the fourth crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions is obtained, including the low-cycle fatigue crack growth life of the second stage of the fourth crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the rotor blade root slot of the nuclear power steam turbine under 120% overspeed transient operating conditions, the crack shape parameters of the rotor blade root slot, the rotor material low-cycle fatigue crack growth test constants, and the maximum stress at the crack site of the rotor blade root slot of the nuclear power steam turbine under 120% overspeed transient operating conditions, so as to obtain the low-cycle fatigue crack growth life of the second stage of the fourth crack growth category of the nuclear power steam turbine under 120% overspeed transient operating conditions.

[0558] In some examples, the low-cycle fatigue crack growth life N of the second stage of the fourth crack growth category of a nuclear power steam turbine under 120% overspeed transient operation is f120%4,2 The calculation process is as follows:

[0559]

[0560] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the crack propagation category of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is the first crack propagation category, and the 120% overspeed operation low-cycle fatigue stress and material test basic data of the No. 1 low-pressure rotor of the nuclear power steam turbine A are shown in Table 14.

[0561] Table 14 Basic data of low cycle fatigue stress and material test of low pressure rotor of nuclear power steam turbine at 120% overspeed operation

[0562]

[0563]

[0564] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A120% overspeed transient operating condition is as follows:

[0565]

[0566]

[0567]

[0568] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the crack extension category of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B is the first crack extension category, and the 120% overspeed operation low-cycle fatigue stress and material test basic data of the No. 2 low-pressure rotor of the nuclear power steam turbine B are shown in Table 14.

[0569] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B120% overspeed transient operation condition is as follows:

[0570]

[0571]

[0572]

[0573] For example, continuing to take the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the crack extension category of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is the second crack extension category, and the 120% overspeed operation low-cycle fatigue stress and material test basic data of the No. 3 low-pressure rotor of the nuclear power steam turbine C are shown in Table 14.

[0574] The calculation process of the low-cycle fatigue crack growth life of the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine under the second crack growth category of the C120% overspeed transient condition is as follows:

[0575]

[0576]

[0577] Therefore, if the target monitoring component in this method is the rotor blade root slot, the crack shape parameters of the rotor blade root slot, the low-cycle fatigue crack growth test constants of the rotor material, the maximum stress at the crack site of the rotor blade root slot under the transient operating condition of 120% overspeed operation of the nuclear power steam turbine, and the crack growth size set of the rotor blade root slot can be comprehensively considered to obtain the low-cycle fatigue crack growth life under different crack growth categories under the transient operating condition of 120% overspeed operation of the nuclear power steam turbine.

[0578] The following takes the target monitoring component as an example of a cylinder to describe how to obtain the low-cycle fatigue crack growth life of the cylinder.

[0579] Based on any of the above embodiments, the crack expansion stage of the cylinder includes two stages, wherein in the first stage, the crack size of the cylinder increases from the initial crack size a to 0 Extend to the stress corrosion crack growth size threshold a SCC In the second stage, the crack size of the cylinder increases from the stress corrosion crack growth threshold value a SCC Extended to the critical crack size of low cycle fatigue a cj Among them, the critical crack size of low cycle fatigue is a cj for a cc or a cw or a ch .

[0580] Based on any of the above embodiments, Fig.12 As shown, the multi-stage low-cycle fatigue crack growth life of the cylinder is obtained, including:

[0581] S1201, obtaining basic data for stress calculation and basic data for material testing of a cylinder of a nuclear power steam turbine.

[0582] S1202, determining a set of crack extension dimensions of the cylinder based on stress calculation basic data and material test basic data.

[0583] For the relevant contents of steps S1201 - S1202 , please refer to the above embodiments and will not be repeated here.

[0584] S1203, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the first stage of the nuclear power steam turbine cold start transient condition.

[0585] In one embodiment, based on the crack growth size set, the low-cycle fatigue crack growth life of the first stage of the nuclear power steam turbine cold start transient condition is obtained, including the initial crack size of the cylinder, the stress corrosion crack growth size threshold value, the crack shape parameters of the cylinder, the cylinder material low-cycle fatigue crack growth test constant, and the maximum stress at the cylinder crack site of the nuclear power steam turbine cold start transient condition, so as to obtain the low-cycle fatigue crack growth life of the first stage of the nuclear power steam turbine cold start transient condition.

[0586] In some examples, the low-cycle fatigue crack growth life N of the first stage of the cold start transient condition of a nuclear power steam turbine is fc,1 The calculation process is as follows:

[0587]

[0588] Among them, C 0 、m 0 Low cycle fatigue crack growth test constants of cylinder materials.

[0589] S1204, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the second stage of the nuclear power steam turbine cold start transient condition.

[0590] In one embodiment, based on the crack extension size set, the low-cycle fatigue crack extension life of the second stage of the nuclear power steam turbine cold start transient condition is obtained, including based on the stress corrosion crack extension size threshold value, the low-cycle fatigue critical crack size of the cylinder under the nuclear power steam turbine cold start transient condition, the crack shape parameters of the cylinder, the low-cycle fatigue crack extension test constant of the cylinder material, and the maximum stress at the cylinder crack site under the nuclear power steam turbine cold start transient condition, to obtain the low-cycle fatigue crack extension life of the second stage of the nuclear power steam turbine cold start transient condition.

[0591] In some examples, the low-cycle fatigue crack growth life N of the second stage of the cold start transient condition of a nuclear power steam turbine is fc,2 The calculation process is as follows:

[0592]

[0593] S1205, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the first stage of the nuclear power steam turbine warm start transient condition.

[0594] In one embodiment, based on a set of crack extension sizes, a low-cycle fatigue crack extension life of a nuclear power steam turbine in the first stage of a warm start transient condition is obtained, including an initial crack size of the cylinder, a stress corrosion crack extension size threshold, a crack shape parameter of the cylinder, a low-cycle fatigue crack extension test constant of the cylinder material, and a maximum stress at a cylinder crack site in a warm start transient condition of a nuclear power steam turbine, to obtain a low-cycle fatigue crack extension life of a nuclear power steam turbine in the first stage of a warm start transient condition.

[0595] In some examples, the low-cycle fatigue crack growth life N of the first stage of warm start transient conditions of nuclear power steam turbines is fw,1 The calculation process is as follows:

[0596]

[0597] S1206, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the second stage of the warm start transient condition of the nuclear power steam turbine.

[0598] In one embodiment, based on the crack growth size set, the low-cycle fatigue crack growth life of the second stage of the warm start transient condition of the nuclear power steam turbine is obtained, including the low-cycle fatigue critical crack size of the cylinder under the warm start transient condition of the nuclear power steam turbine based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the cylinder under the warm start transient condition of the nuclear power steam turbine, the crack shape parameters of the cylinder, the low-cycle fatigue crack growth test constant of the cylinder material, and the maximum stress at the cylinder crack site under the warm start transient condition of the nuclear power steam turbine, so as to obtain the low-cycle fatigue crack growth life of the second stage of the warm start transient condition of the nuclear power steam turbine.

[0599] In some examples, the low-cycle fatigue crack growth life N of the second stage of warm start transient conditions of nuclear power steam turbines is fw,2 The calculation process is as follows:

[0600]

[0601] S1207, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the first stage of the nuclear power steam turbine hot start transient condition.

[0602] In one embodiment, based on the crack growth size set, the low-cycle fatigue crack growth life of the first stage of the hot start transient condition of the nuclear power steam turbine is obtained, including the initial crack size of the cylinder, the stress corrosion crack growth size threshold value, the crack shape parameters of the cylinder, the low-cycle fatigue crack growth test constant of the cylinder material, and the maximum stress at the cylinder crack site of the hot start transient condition of the nuclear power steam turbine, so as to obtain the low-cycle fatigue crack growth life of the first stage of the hot start transient condition of the nuclear power steam turbine.

[0603] In some examples, the low-cycle fatigue crack growth life N of the first stage of the hot start transient condition of a nuclear power steam turbine is fh,1 The calculation process is as follows:

[0604]

[0605] S1208, based on the crack growth size set, obtain the low cycle fatigue crack growth life of the second stage of the nuclear power steam turbine hot start transient condition.

[0606] In one embodiment, based on the crack growth size set, the low-cycle fatigue crack growth life of the second stage of the nuclear power steam turbine hot start transient condition is obtained, including the low-cycle fatigue critical crack size of the cylinder under the nuclear power steam turbine hot start transient condition, the crack shape parameters of the cylinder, the low-cycle fatigue crack growth test constants of the cylinder material, and the maximum stress at the cylinder crack site under the nuclear power steam turbine hot start transient condition, so as to obtain the low-cycle fatigue crack growth life of the second stage of the nuclear power steam turbine hot start transient condition.

[0607] In some examples, the low-cycle fatigue crack growth life N of the second stage of the hot start transient condition of a nuclear power steam turbine is fh,2 The calculation process is as follows:

[0608]

[0609] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E in the above embodiment as an example, the basic data for low-cycle fatigue cracking design monitoring of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E is shown in Table 15.

[0610] Table 15 Basic data for monitoring the low cycle fatigue cracking design of low pressure inner cylinder

[0611]

[0612] The calculation process of the multi-stage low-cycle fatigue crack growth life of the No. 1 low-pressure inner cylinder of nuclear power steam turbine E is as follows:

[0613]

[0614]

[0615]

[0616]

[0617]

[0618]

[0619] Therefore, in this method, if the target monitoring component is a cylinder, the crack shape parameters of the cylinder, the low-cycle fatigue crack growth test constants of the cylinder material, the maximum stress at the cylinder crack site, and the crack growth size set of the cylinder can be comprehensively considered to obtain the multi-stage low-cycle fatigue crack growth life.

[0620] The following takes the target monitoring component as an example of a cylinder to describe how to obtain the low-cycle fatigue crack growth life of the cylinder.

[0621] Based on any of the above embodiments, if the target monitoring component is a cylinder, such as Fig.13 As shown, the low cycle fatigue crack growth life under different crack growth categories is obtained, including:

[0622] S1301, obtaining the low cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the cold start transient condition.

[0623] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the transient operating condition of cold start is obtained, including the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the transient operating condition of cold start based on phased array detection of crack depth, stress corrosion crack growth size threshold value, cylinder crack shape parameters, cylinder material low-cycle fatigue crack growth test constants, and maximum stress at the cylinder crack site in the transient operating condition of cold start of the nuclear power steam turbine.

[0624] In some examples, the low-cycle fatigue crack growth life N of the first stage of the first crack growth category of a nuclear power steam turbine in a cold start transient condition is fc1,1 The calculation process is as follows:

[0625]

[0626] Among them, C 0 、m 0 Low cycle fatigue crack growth test constants of cylinder materials.

[0627] S1302, obtaining the low cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine in the cold start transient condition.

[0628] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine cold start transient condition is obtained, including based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the cylinder of the nuclear power steam turbine cold start transient condition, the crack shape parameters of the cylinder, the low-cycle fatigue crack growth test constants of the cylinder material, and the maximum stress of the cylinder crack site of the nuclear power steam turbine cold start transient condition, to obtain the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine cold start transient condition.

[0629] In some examples, the low-cycle fatigue crack growth life N of the second stage of the first crack growth category of a nuclear power steam turbine in a cold start transient condition is fc1,2 The calculation process is as follows:

[0630]

[0631] S1303, obtaining the low cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine in the cold start transient condition.

[0632] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine cold start transient condition is obtained, including crack depth detection based on the phased array, low-cycle fatigue critical crack size of the cylinder of the nuclear power steam turbine cold start transient condition, crack shape parameters of the cylinder, low-cycle fatigue crack growth test constants of the cylinder material, and maximum stress of the cylinder crack site of the nuclear power steam turbine cold start transient condition, so as to obtain the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine cold start transient condition.

[0633] In some examples, the low-cycle fatigue crack growth life N of the first stage of the second crack growth category of a nuclear power steam turbine in a cold start transient condition is fc2,1 The calculation process is as follows:

[0634]

[0635] S1304, obtaining the low cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the transient operating condition of warm start.

[0636] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the warm start transient condition is obtained, including based on phased array detection of crack depth, stress corrosion crack growth size threshold, cylinder crack shape parameters, cylinder material low-cycle fatigue crack growth test constants, and maximum stress at the cylinder crack site of the nuclear power steam turbine in the warm start transient condition, to obtain the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the warm start transient condition.

[0637] In some examples, the low-cycle fatigue crack growth life N of the first stage of the first crack growth category of a nuclear power steam turbine during warm start transient conditions is fw1,1 The calculation process is as follows:

[0638]

[0639] S1305, obtaining the low cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine in the warm start transient condition.

[0640] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine warm start transient condition is obtained, including based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the cylinder of the nuclear power steam turbine warm start transient condition, the crack shape parameters of the cylinder, the low-cycle fatigue crack growth test constants of the cylinder material, and the maximum stress of the cylinder crack site of the nuclear power steam turbine warm start transient condition, to obtain the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine warm start transient condition.

[0641] In some examples, the low-cycle fatigue crack growth life N of the second stage of the first crack growth category of a nuclear power steam turbine during warm start transient conditions is fw1,2 The calculation process is as follows:

[0642]

[0643] S1306, obtaining the low cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine in the warm start transient condition.

[0644] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine warm start transient condition is obtained, including crack depth detection based on the phased array, low-cycle fatigue critical crack size of the cylinder of the nuclear power steam turbine warm start transient condition, crack shape parameters of the cylinder, low-cycle fatigue crack growth test constants of the cylinder material, and maximum stress at the cylinder crack site of the nuclear power steam turbine warm start transient condition, so as to obtain the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine warm start transient condition.

[0645] In some examples, the low-cycle fatigue crack growth life N of the first stage of the second crack growth category of a nuclear power steam turbine during warm start transient conditions is fw2,1 The calculation process is as follows:

[0646]

[0647] S1307, obtaining the low cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine in the hot start transient condition.

[0648] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine hot start transient condition is obtained, including based on phased array detection of crack depth, stress corrosion crack growth size threshold, cylinder crack shape parameters, cylinder material low-cycle fatigue crack growth test constants, and maximum stress at the cylinder crack site of the nuclear power steam turbine hot start transient condition, to obtain the low-cycle fatigue crack growth life of the first stage of the first crack growth category of the nuclear power steam turbine hot start transient condition.

[0649] In some examples, the low-cycle fatigue crack growth life N of the first stage of the first crack growth category of a nuclear power steam turbine hot start transient condition is fh1,1 The calculation process is as follows:

[0650]

[0651] S1308, obtaining the low cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine in the hot start transient condition.

[0652] In one embodiment, the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine hot start transient condition is obtained, including based on the stress corrosion crack growth size threshold value, the low-cycle fatigue critical crack size of the cylinder of the nuclear power steam turbine hot start transient condition, the crack shape parameters of the cylinder, the low-cycle fatigue crack growth test constants of the cylinder material, and the maximum stress of the cylinder crack site of the nuclear power steam turbine hot start transient condition, to obtain the low-cycle fatigue crack growth life of the second stage of the first crack growth category of the nuclear power steam turbine hot start transient condition.

[0653] In some examples, the low-cycle fatigue crack growth life N of the second stage of the first crack growth category of a nuclear power steam turbine hot start transient condition is fh1,2 The calculation process is as follows:

[0654]

[0655] S1309, obtaining the low cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine in the hot start transient condition.

[0656] In one embodiment, the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine hot start transient condition is obtained, including crack depth detection based on the phased array, low-cycle fatigue critical crack size of the cylinder of the nuclear power steam turbine hot start transient condition, crack shape parameters of the cylinder, low-cycle fatigue crack growth test constants of the cylinder material, and maximum stress at the cylinder crack site of the nuclear power steam turbine hot start transient condition, so as to obtain the low-cycle fatigue crack growth life of the first stage of the second crack growth category of the nuclear power steam turbine hot start transient condition.

[0657] In some examples, the low-cycle fatigue crack growth life N of the first stage of the second crack growth category of a nuclear power steam turbine hot start transient condition is fh2,1 The calculation process is as follows:

[0658]

[0659] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A in the above embodiment as an example, the crack extension category of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A is the first crack extension category, and the basic data for calculating the life of the cylinder crack position in the cold start transient process, the basic data for calculating the life of the cylinder crack position in the warm start transient process, and the basic data for calculating the life of the cylinder crack position in the hot start transient process of the nuclear power steam turbine A are shown in Tables 16, 17, and 18, respectively.

[0660] Table 16 Basic data for calculating the life of cylinder crack positions during cold start transient process

[0661] Serial number project Data Value 1 <![CDATA[The maximum stress σ at the cylinder crack location under cold start transient conditions maxc / MPa]]> 252.970 2 <![CDATA[Low cycle fatigue crack growth test constant m of cylinder material 0 > 3.15 3 <![CDATA[Low cycle fatigue crack growth test constant C for cylinder material 0 > <![CDATA[4.2×10 -12 ]]> 4 Crack shape parameter Q 0.88

[0662] Table 17 Basic data for calculating the life of cylinder crack positions during warm start transient process

[0663] Serial number project Data Value 1 <![CDATA[The maximum stress σ at the cylinder crack location under warm start transient conditions maxw / MPa]]> 267.093 2 <![CDATA[Low cycle fatigue crack growth test constant m of cylinder material 0 > 3.15 3 <![CDATA[Low cycle fatigue crack growth test constant C of cylinder material 0 > <![CDATA[4.2×10 -12 ]]>

[0664] Table 18 Basic data for calculating the life of cylinder crack positions during hot start transient process

[0665] Serial number project Data Value 1 <![CDATA[The maximum stress σ at the cylinder crack location under warm start transient conditions maxh / MPa]]> 237.736 2 <![CDATA[Low cycle fatigue crack growth test constant m of cylinder material 0 > 3.15 3 <![CDATA[Low cycle fatigue crack growth test constant C of cylinder material 0 > <![CDATA[4.2×10 -12 ]]>

[0666] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the No. 1 low-pressure inner cylinder of nuclear power steam turbine A is as follows:

[0667]

[0668]

[0669]

[0670]

[0671]

[0672]

[0673] For example, continuing to take the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B in the above embodiment as an example, the crack extension category of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B is the first crack extension category, and the basic data for calculating the life of the cylinder crack position in the cold start transient process, the basic data for calculating the life of the cylinder crack position in the warm start transient process, and the basic data for calculating the life of the cylinder crack position in the hot start transient process of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B are shown in Tables 16, 17, and 18, respectively.

[0674] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the No. 2 low-pressure inner cylinder of nuclear power steam turbine B is as follows:

[0675]

[0676]

[0677]

[0678]

[0679]

[0680]

[0681] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C in the above embodiment as an example, the crack extension category of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C is the first crack extension category, and the basic data for calculating the life of the cylinder crack position in the cold start transient process, the basic data for calculating the life of the cylinder crack position in the warm start transient process, and the basic data for calculating the life of the cylinder crack position in the hot start transient process of the nuclear power steam turbine C are shown in Tables 16, 17, and 18, respectively.

[0682] The calculation process of the low-cycle fatigue crack growth life of the first crack growth category of the No. 1 low-pressure inner cylinder of nuclear power steam turbine C is as follows:

[0683]

[0684]

[0685]

[0686]

[0687]

[0688]

[0689] For example, continuing to take the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D in the above embodiment as an example, the crack extension category of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D is the second crack extension category, and the basic data for calculating the life of the cylinder crack position in the cold start transient process, the basic data for calculating the life of the cylinder crack position in the warm start transient process, and the basic data for calculating the life of the cylinder crack position in the hot start transient process of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D are shown in Tables 16, 17, and 18, respectively.

[0690] The calculation process of the low-cycle fatigue crack growth life under the second crack growth category of the No. 2 low-pressure inner cylinder of nuclear power steam turbine D is as follows:

[0691]

[0692]

[0693]

[0694] Therefore, in this method, if the target monitoring component is a cylinder, the crack shape parameters of the cylinder, the low-cycle fatigue crack growth test constants of the cylinder material, the maximum stress at the cylinder crack site, and the crack growth size set of the cylinder can be comprehensively considered to obtain the low-cycle fatigue crack growth life under different crack growth categories.

[0695] On the basis of any of the above embodiments, the fatigue crack growth life includes the high-cycle fatigue crack growth life, and the high-cycle fatigue crack growth life is obtained based on the crack growth size set, including the third parameter of the target monitoring component, the high-cycle fatigue critical crack size, the crack shape parameter of the target monitoring component, the high-cycle fatigue crack growth test constant of the material of the target monitoring component, and the high-cycle fatigue stress range of the crack part of the target monitoring component under the steady-state condition of nuclear power steam turbine under load operation, so as to obtain the high fatigue crack growth life. Among them, the third parameter is the phased array detection crack depth of the target monitoring component or the high-cycle fatigue crack growth size threshold value. Therefore, the method can comprehensively consider the third parameter of the target monitoring component, the high-cycle fatigue critical crack size, the crack shape parameter of the target monitoring component, the high-cycle fatigue crack growth test constant of the material of the target monitoring component, and the high-cycle fatigue stress range of the crack part of the target monitoring component under the steady-state condition of nuclear power steam turbine under load operation, and obtain the high fatigue crack growth life.

[0696] The following takes the rotor as an example of the target monitoring component to describe how to obtain the high cycle fatigue crack growth life of the rotor.

[0697] Based on any of the above embodiments, Fig.14 As shown, the high cycle fatigue crack growth life of the rotor is obtained, including:

[0698] S1401, obtaining basic data for stress calculation and basic data for material testing of a nuclear power steam turbine rotor.

[0699] S1402: Determine the threshold value of high cycle fatigue crack growth size of the rotor based on stress calculation basic data and material test basic data.

[0700] S1403, determine the high cycle fatigue critical crack size of the rotor based on the basic data of stress calculation and basic data of material testing.

[0701] For the relevant contents of steps S1401 - S1403 , please refer to the above embodiments and will not be described again here.

[0702] S1404, based on the high cycle fatigue crack growth size threshold value, high cycle fatigue critical crack size, crack shape parameters of the rotor, high cycle fatigue crack growth test constants of rotor materials, and high cycle fatigue stress range of the rotor under steady-state conditions of nuclear power steam turbine under load operation, the high cycle fatigue crack growth life is obtained.

[0703] In one embodiment, the high cycle fatigue crack growth life is calculated as follows:

[0704]

[0705] For example, continuing to take the welded low-pressure rotor of a certain model of 1200MW nuclear power steam turbine in the above embodiment as an example, the basic data for high-cycle fatigue life damage design monitoring of the welded low-pressure rotor is shown in Table 19.

[0706] Table 19 Basic data for high cycle fatigue life damage design monitoring of welded low pressure rotor

[0707]

[0708] The calculation process of high cycle fatigue crack growth life of welded low pressure rotor is as follows:

[0709]

[0710] Therefore, if the target monitored component in this method is the rotor, the high-cycle fatigue crack growth size threshold value, the high-cycle fatigue critical crack size, the crack shape parameters of the rotor, the high-cycle fatigue crack growth test constants of the rotor material, and the high-cycle fatigue stress range of the rotor under steady-state conditions of nuclear power steam turbine load operation can be comprehensively considered to obtain the high-cycle fatigue crack growth life.

[0711] The following takes the rotor blade root slot as an example of the target monitoring component to describe how to obtain the high cycle fatigue crack growth life of the rotor blade root slot.

[0712] Based on any of the above embodiments, if the target monitoring component is a rotor blade root slot, such as Fig.15 As shown, the high cycle fatigue crack growth life under different crack growth categories is obtained, including:

[0713] S1501, based on the high cycle fatigue crack growth size threshold value, the high cycle fatigue critical crack size, the crack shape parameters of the rotor blade root slot, the rotor material high cycle fatigue crack growth test constants, and the high cycle fatigue stress range of the rotor blade root slot under the steady-state condition of nuclear power steam turbine under load operation, obtain the high cycle fatigue crack growth life under any one of the first crack growth category, the second crack growth category and the third crack growth category.

[0714] S1502, based on the crack depth detected by phased array, the critical crack size of high-cycle fatigue, the crack shape parameters of the rotor blade root slot, the high-cycle fatigue crack growth test constants of the rotor material, and the high-cycle fatigue stress range of the rotor blade root slot under the steady-state condition of nuclear power steam turbine under load operation, the high-cycle fatigue crack growth life under the fourth crack growth category is obtained.

[0715] In one embodiment, the calculation process of the high cycle fatigue crack growth life under any one of the first crack growth category, the second crack growth category and the third crack growth category is as follows:

[0716]

[0717] Among them, C 0H 、m 0H These are all constants of high cycle fatigue crack growth test of rotor materials.

[0718] Among them, N fH1 is the high cycle fatigue crack growth life under the first crack growth category, N fH2 is the high cycle fatigue crack growth life under the second crack growth category, N fH3 It is the high cycle fatigue crack growth life under the third crack growth category.

[0719] In one embodiment, the high cycle fatigue crack growth life N under the fourth crack growth category fH4 The calculation process is as follows:

[0720]

[0721] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is the first crack extension category, and the high-cycle fatigue stress and material test basic data of the No. 1 low-pressure rotor of the nuclear power steam turbine A are shown in Table 20.

[0722] Table 20 Basic data of high cycle fatigue stress and material test of low pressure rotor of nuclear power steam turbine

[0723] Serial number project Data Value 1 <![CDATA[High-cycle fatigue stress range Δσ at the crack location of the rotor blade root H / MPa]]> 3.078 2 <![CDATA[High cycle fatigue crack growth test constant m of rotor material 0H > 2.889 3 <![CDATA[High-cycle fatigue crack growth test constant C of rotor material 0H > <![CDATA[6.859×10 —12 ]]> 4 Crack shape parameter Q 0.99976

[0724] The high cycle fatigue crack growth life N of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 1 low pressure rotor of nuclear power steam turbine A fH1 The calculation process is as follows:

[0725]

[0726] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B is the first crack extension category, and the high-cycle fatigue stress and material test basic data of the No. 2 low-pressure rotor of the nuclear power steam turbine B are shown in Table 19.

[0727] The high cycle fatigue crack growth life N of the first crack growth category of the inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B in the fifth stage fH1 The calculation process is as follows:

[0728]

[0729] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is the second crack extension category, and the high-cycle fatigue stress and material test basic data of the No. 3 low-pressure rotor of the nuclear power steam turbine C are shown in Table 19.

[0730] The high cycle fatigue crack growth life N of the 5th stage inverted T-shaped blade root groove of No. 3 low pressure rotor of nuclear power steam turbine C under the second crack growth category fH2 The calculation process is as follows:

[0731]

[0732] Therefore, in this method, if the target monitoring component is the rotor blade root slot, the high-cycle fatigue crack growth size threshold value, the high-cycle fatigue critical crack size, the crack shape parameters of the rotor blade root slot, the high-cycle fatigue crack growth test constants of the rotor material, and the high-cycle fatigue stress range of the rotor blade root slot under the steady-state condition of nuclear power steam turbine under load can be comprehensively considered to obtain the high-cycle fatigue crack growth life under any crack growth category of the first crack growth category, the second crack growth category, and the third crack growth category, and the phased array detection crack depth, the high-cycle fatigue critical crack size, the crack shape parameters of the rotor blade root slot, the high-cycle fatigue crack growth test constants of the rotor material, and the high-cycle fatigue stress range of the rotor blade root slot under the steady-state condition of nuclear power steam turbine under load can be comprehensively considered to obtain the high-cycle fatigue crack growth life under the fourth crack growth category.

[0733] Fig.16 The present invention is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine throughout its entire life cycle according to another embodiment of the present invention.

[0734] like Fig.16 As shown, the stress corrosion and fatigue long-life monitoring method for a nuclear power steam turbine during its entire life cycle according to an embodiment of the present disclosure includes:

[0735] S1601: Determine one or more target monitoring components from the components to be monitored.

[0736] S1602, determining the long-life monitoring data required for the target monitoring component, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life.

[0737] For the relevant contents of steps S1601-S1602, please refer to the above embodiment and will not be repeated here.

[0738] S1603, based on the long-life monitoring data required by the target monitoring component, obtain the crack growth calendar life of the target monitoring component.

[0739] In one embodiment, based on the long-life monitoring data required for the target monitoring component, the crack growth calendar life of the target monitoring component is obtained, including if the target monitoring component is a rotor blade root slot, based on the stress corrosion crack growth life, low cycle fatigue crack growth life and high cycle fatigue crack growth life under the crack growth category of the rotor blade root slot, to obtain the crack growth calendar life of the rotor blade root slot.

[0740] In one embodiment, the crack growth calendar life of the target monitored component is obtained based on the long-life monitoring data required for the target monitored component, including if the target monitored component is a cylinder, the crack growth calendar life of the cylinder is obtained based on the stress corrosion crack growth life and low cycle fatigue crack growth life under the crack growth category of the cylinder.

[0741] In one embodiment, based on the long-life monitoring data required for the target monitoring component, the crack growth calendar life of the target monitoring component is obtained, including if the target monitoring component is a rotor, based on the stress corrosion crack growth life, low cycle fatigue crack growth life and high cycle fatigue crack growth life under the crack growth category of the rotor, to obtain the crack growth calendar life of the rotor.

[0742] In one embodiment, based on the long-life monitoring data required by the target monitoring component, the crack growth calendar life of the target monitoring component is obtained, including obtaining the multi-stage calendar life of the target monitoring component based on the long-life monitoring data required by the target monitoring component, and obtaining the crack growth calendar life based on the multi-stage calendar life of the target monitoring component. It should be noted that the stage refers to the crack growth stage of the target monitoring component, the number of stages is multiple, and different phased array detection crack depths and different crack growth size sets of the target monitoring component can correspond to different categories and different stages.

[0743] In some examples, the crack growth calendar life is obtained based on the multi-stage calendar life of the target monitoring component, including determining the sum of the multi-stage calendar life of the target monitoring component as the crack growth calendar life.

[0744] S1604: Based on the crack propagation calendar life, crack propagation life safety monitoring is performed on the target monitoring component.

[0745] In one embodiment, based on the crack propagation calendar life, crack propagation life safety monitoring is performed on the target monitoring component, including obtaining the monitoring criterion value of the target monitoring component, if the crack propagation calendar life is greater than or equal to the monitoring criterion value, it is determined that no safety abnormality occurs in the target monitoring component, and if the crack propagation calendar life is less than the monitoring criterion value, it is determined that a safety abnormality occurs in the target monitoring component.

[0746] In some examples, a mapping relationship between the model of the target monitoring component and the monitoring criterion value can be established in advance to obtain the monitoring criterion value of the target monitoring component, including querying the monitoring criterion value in the above mapping relationship based on the model of the target monitoring component, and determining the queried monitoring criterion value as the monitoring criterion value of the target monitoring component.

[0747] In summary, according to the stress corrosion and fatigue long-life monitoring method for the whole life of a nuclear power steam turbine of the embodiment of the present disclosure, the crack propagation calendar life of the target monitoring component is obtained based on the long-life monitoring data required by the target monitoring component, and the crack propagation life safety monitoring of the target monitoring component is performed based on the crack propagation calendar life. Thus, the influence of stress corrosion and fatigue on the life of the target monitoring component can be comprehensively considered to perform crack propagation life safety monitoring on the target monitoring component, so as to ensure the long-life safe operation of the nuclear power steam turbine throughout its whole life.

[0748] The following takes the rotor as an example of the target monitoring component to describe how to obtain the crack growth calendar life of the rotor.

[0749] In one embodiment, the calendar life of the first stage is obtained based on the low-cycle fatigue crack growth life of the first stage of the normal shutdown transient condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the first stage of the 110% overspeed test transient condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the first stage of the 120% overspeed operation transient condition of the nuclear power steam turbine, the average annual number of normal shutdowns of the nuclear power steam turbine, the average annual number of 110% overspeed tests and the average annual number of 120% overspeed operations.

[0750] In one embodiment, the calendar life of the second stage is obtained based on the high-cycle fatigue crack growth life, the low-cycle fatigue crack growth life of the second stage of the normal shutdown transient condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the second stage of the 110% overspeed test transient condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the second stage of the 120% overspeed operation transient condition of the nuclear power steam turbine, the average annual normal shutdown times of the nuclear power steam turbine, the average annual 110% overspeed test times, the average annual 120% overspeed operation times and the average annual fatigue times of the rotor.

[0751] In one embodiment, it also includes the calendar life of the third stage based on the stress corrosion crack growth life, the high cycle fatigue crack growth life, the low cycle fatigue crack growth life of the third stage of the normal shutdown transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the third stage of the 110% overspeed test transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the third stage of the 120% overspeed operation transient condition of the nuclear power steam turbine, the average annual normal shutdown times of the nuclear power steam turbine, the average annual 110% overspeed test times, the average annual 120% overspeed operation times and the average annual fatigue times of the rotor.

[0752] In one embodiment, the method further includes obtaining a crack growth calendar life based on the calendar life of the first stage, the calendar life of the second stage, and the calendar life of the third stage. For example, obtaining a crack growth calendar life based on the calendar life of the first stage, the calendar life of the second stage, and the calendar life of the third stage includes determining the sum of the calendar life of the first stage, the calendar life of the second stage, and the calendar life of the third stage as the crack growth calendar life.

[0753] In some examples, the crack growth calendar life τ CL The calculation process is as follows:

[0754]

[0755]

[0756]

[0757] τ CL =τ CL1 +τ CL2 +τ CL3

[0758] Among them, τ CL1 is the calendar life of the first stage, τ CL2 is the calendar life of the second stage, τ CL3 is the calendar life of the third stage, y n is the annual average number of normal shutdowns of nuclear power steam turbines, y 110% is the annual average number of 110% overspeed tests, y 120% is the annual average of 120% overspeed operation times, y H is the annual average high cycle fatigue number of the rotor.

[0759] In some examples, the average annual operating hours of nuclear power turbines can be based on t y and the operating speed n of the nuclear power steam turbine 0 , the annual average high cycle fatigue number of the rotor y is obtained H For example, this can be achieved by the following formula:

[0760]

[0761] For example, continuing to take the welded low-pressure rotor of a certain model of 1200MW nuclear power steam turbine in the above embodiment as an example, the calendar design monitoring basic data of the welded low-pressure rotor is shown in Table 21.

[0762] Table 21 Calendar design monitoring basic data for welded low-pressure rotor

[0763] Serial number project Data Value 1 <![CDATA[Average annual normal shutdown times y n / time]]> 99 2 <![CDATA[Number of times of 110% overspeed test per year y 110% / time]]> 1 3 <![CDATA[Number of times of running at 120% over speed per year y 120% / time]]> 0.2 4 <![CDATA[Annual average operating hours t y / h]]> 7000 5 <![CDATA[Operating speed n 0 / r / min]]> 1500 6 <![CDATA[Crack growth life safety monitoring criterion value τ 0 / year]]> 60

[0764] The calculation process of the annual average high-cycle fatigue number of welded low-pressure rotors is as follows:

[0765]

[0766] The calculation process of the crack growth calendar life of the welded low-pressure rotor is as follows:

[0767]

[0768]

[0769]

[0770] τ CL =τ CL1 +τ CL2 +τ CL3 =133.54+11.37+17.78=162.69 years

[0771] The following takes the rotor blade root slot as an example of the target monitoring component to describe how to obtain the crack growth calendar life of the rotor blade root slot.

[0772] like Fig.17 As shown, if the target monitoring component is a rotor blade root slot, the crack growth calendar life of the rotor blade root slot is obtained, including:

[0773] S1701, based on the stress corrosion crack growth life under the first crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, the crack growth calendar life under the first crack growth category is obtained.

[0774] In one embodiment, based on the stress corrosion crack growth life under the first crack growth category, the low cycle fatigue crack growth life of multiple stages, and the high cycle fatigue crack growth life, the crack growth calendar life under the first crack growth category is obtained, including obtaining the calendar life of each stage of the first crack growth category based on the stress corrosion crack growth life under the first crack growth category, the low cycle fatigue crack growth life of multiple stages, and the high cycle fatigue crack growth life, and obtaining the crack growth calendar life under the first crack growth category based on the calendar life of each stage of the first crack growth category.

[0775] In some examples, the calendar life of the first stage of the first crack growth category is obtained based on the low-cycle fatigue crack growth life of the first stage of the first crack growth category under the transient operating condition of the normal shutdown of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the first stage of the first crack growth category under the transient operating condition of the 110% overspeed test of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the first stage of the first crack growth category under the transient operating condition of the 120% overspeed test of the nuclear power steam turbine, the average annual number of normal shutdowns of the nuclear power steam turbine, the average annual number of 110% overspeed tests and the average annual number of 120% overspeed operations.

[0776] In some examples, the calendar life of the second stage of the first crack growth category is obtained based on the stress corrosion crack growth life under the first crack growth category, the low cycle fatigue crack growth life of the second stage of the first crack growth category under the transient condition of normal shutdown of nuclear power steam turbine, the low cycle fatigue crack growth life of the second stage of the first crack growth category under the transient condition of 110% overspeed test of nuclear power steam turbine, the low cycle fatigue crack growth life of the second stage of the first crack growth category under the transient condition of 120% overspeed test of nuclear power steam turbine, the average annual normal shutdown times, the average annual 110% overspeed test times and the average annual 120% overspeed operation times of nuclear power steam turbine.

[0777] In some examples, the calendar life of the third stage of the first crack growth category is obtained based on the stress corrosion crack growth life under the first crack growth category, the high cycle fatigue crack growth life under the first crack growth category, the low cycle fatigue crack growth life of the third stage of the first crack growth category under the normal shutdown transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the third stage of the first crack growth category under the 110% overspeed test transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the third stage of the first crack growth category under the 120% overspeed test transient condition of the nuclear power steam turbine, the average annual normal shutdown times of the nuclear power steam turbine, the average annual 110% overspeed test times, the average annual 120% overspeed operation times and the average annual high cycle fatigue times of the rotor blade root slot.

[0778] The crack extension calendar life under the first crack extension category is obtained based on the calendar life of the first stage of the first crack extension category, the calendar life of the second stage of the first crack extension category, and the calendar life of the third stage of the first crack extension category.

[0779] In some examples, the crack growth calendar life τ under the first crack growth category is CL1 The calculation process is as follows:

[0780]

[0781]

[0782]

[0783] τ CL1 =τ CL1,1 +τ CL1,2 +τ CL1,3

[0784] Among them, τ CL1,1 is the calendar life of the first stage of the first crack growth category, τ CL1,2 is the calendar life of the second stage of the first crack growth category, τ CL1,3 is the calendar life of the third stage of the first crack growth category, y n is the annual average number of normal shutdowns of nuclear power steam turbines, y 110% is the annual average number of 110% overspeed tests of nuclear power steam turbines, y 120% is the annual average 120% overspeed operation times of nuclear power steam turbines, y H is the annual average high cycle fatigue number of the rotor blade root slot.

[0785] In some examples, the average annual operating hours of nuclear power steam turbines can be calculated based on the average annual operating hours of nuclear power turbines. y and nuclear power steam turbine operating speed n 0 , and the annual average high cycle fatigue number y of the rotor blade root slot is obtained H For example, this can be achieved by the following formula:

[0786]

[0787] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is the first crack extension category, and the calendar design monitoring basic data of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is shown in Table 22.

[0788] Table 22 Basic data for monitoring calendar design of nuclear power steam turbine rotor blade root slot

[0789] Serial number project Data Value 1 <![CDATA[Annual average normal shutdown times y n / times]]> 99 2 <![CDATA[Number of times of 110% overspeed test per year y 110% / time]]> 1 3 <![CDATA[Annual average number of times of running at 120% over speed y 120% / times]]> 0.2 4 <![CDATA[Annual average operating hours t y / h]]> 7000 5 <![CDATA[Operating speed n 0 / r / min]]> 1500 6 <![CDATA[Crack growth life safety monitoring criterion value τ 0 / year]]> 60 7 <![CDATA[τ for the planned overhaul interval of nuclear power steam turbines m / year]]> 10

[0790] The calculation process of the annual average high-cycle fatigue number of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of nuclear power steam turbine A is as follows:

[0791]

[0792] The crack growth calendar life τ of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of nuclear power steam turbine A CL1 The calculation process is as follows:

[0793]

[0794] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B is the first crack extension category, and the calendar design monitoring basic data of the fifth-stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of the nuclear power steam turbine B is shown in Table 22.

[0795] The calculation process of the annual average high cycle fatigue number of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B is as follows:

[0796]

[0797] The crack growth calendar life τ of the first crack growth category of the inverted T-shaped blade root groove of the 5th stage of the No. 2 low-pressure rotor of nuclear power steam turbine B CL1 The calculation process is as follows:

[0798]

[0799] S1702, based on the stress corrosion crack growth life under the second crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, the crack growth calendar life under the second crack growth category is obtained.

[0800] In one embodiment, based on the stress corrosion crack growth life under the second crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, the crack growth calendar life under the second crack growth category is obtained, including obtaining the calendar life of each stage of the second crack growth category based on the stress corrosion crack growth life under the second crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, and obtaining the crack growth calendar life under the second crack growth category based on the calendar life of each stage of the second crack growth category.

[0801] In some examples, the calendar life of the first stage of the second crack growth category is obtained based on the stress corrosion crack growth life under the second crack growth category, the low cycle fatigue crack growth life of the first stage of the second crack growth category under the normal shutdown transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the first stage of the second crack growth category under the 110% overspeed test transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the first stage of the second crack growth category under the 120% overspeed test transient condition of the nuclear power steam turbine, the average annual normal shutdown times, the average annual 110% overspeed test times and the average annual 120% overspeed operation times of the nuclear power steam turbine.

[0802] In some examples, the stress corrosion crack growth life under the first crack growth category, the high cycle fatigue crack growth life under the second crack growth category, the low cycle fatigue crack growth life of the second crack growth category of the second stage of the normal shutdown transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the second crack growth category of the second stage of the 110% overspeed test transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the second crack growth category of the second stage of the 120% overspeed test transient condition of the nuclear power steam turbine, the annual average number of normal shutdowns of the nuclear power steam turbine, and the annual average number of 110% overspeed tests 110% , the annual average 120% overspeed operation times and the annual average high cycle fatigue times of the rotor blade root slot, and the calendar life of the second stage of the second crack growth category is obtained.

[0803] In some examples, the method further includes obtaining a crack growth calendar life for the second crack growth category based on the calendar life for the first stage of the second crack growth category and the calendar life for the second stage of the second crack growth category.

[0804] In some examples, the crack growth calendar life τ for the second crack growth category is CL2 The calculation process is as follows:

[0805]

[0806]

[0807] τ CL2 =τ CL2,1 +τ CL2,2

[0808] Among them, τ CL2,1 is the calendar life of the first stage of the second crack growth category, τ CL2,2 Calendar life of the second stage of the second crack growth category.

[0809] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is the second crack extension category, and the calendar design monitoring basic data of the fifth-stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is shown in Table 22.

[0810] The calculation process of the annual average high cycle fatigue number of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of nuclear power steam turbine C is as follows:

[0811]

[0812] The crack growth calendar life τ of the 5th stage inverted T-shaped blade root groove of No. 3 low-pressure rotor of nuclear power steam turbine C under the second crack growth categoryCL2 The calculation process is as follows:

[0813]

[0814] S1703, based on the stress corrosion crack growth life under the third crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, the crack growth calendar life under the third crack growth category is obtained.

[0815] In one embodiment, based on the stress corrosion crack growth life under the third crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, the crack growth calendar life under the third crack growth category is obtained, including obtaining the calendar life of each stage of the third crack growth category based on the stress corrosion crack growth life under the third crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, and obtaining the crack growth calendar life under the third crack growth category based on the calendar life of each stage of the third crack growth category.

[0816] In some examples, the calendar life of the first stage of the third crack growth category is obtained based on the low-cycle fatigue crack growth life of the first stage of the third crack growth category under the normal shutdown transient condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the first stage of the third crack growth category under the 110% overspeed test transient condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the first stage of the third crack growth category under the 120% overspeed test transient condition of the nuclear power steam turbine, the average annual normal shutdown times of the nuclear power steam turbine, the average annual 110% overspeed test times and the average annual 120% overspeed operation times.

[0817] In some examples, the calendar life of the second stage of the third crack growth category is obtained based on the high cycle fatigue crack growth life under the third crack growth category, the low cycle fatigue crack growth life of the second stage of the third crack growth category under the normal shutdown transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the second stage of the third crack growth category under the 110% overspeed test transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the second stage of the third crack growth category under the 120% overspeed test transient condition of the nuclear power steam turbine, the average annual normal shutdown times of the nuclear power steam turbine, the average annual 110% overspeed test times, the average annual 120% overspeed operation times and the average annual high cycle fatigue times of the rotor blade root slot.

[0818] In some examples, the calendar life of the third crack growth category in the third stage is obtained based on the stress corrosion crack growth life under the third crack growth category, the high cycle fatigue crack growth life under the third crack growth category, the low cycle fatigue crack growth life of the third crack growth category in the third stage of the normal shutdown transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the third crack growth category in the third stage of the 110% overspeed test transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the third crack growth category in the third stage of the 120% overspeed test transient condition of the nuclear power steam turbine, the average annual normal shutdown times of the nuclear power steam turbine, the average annual 110% overspeed test times, the average annual 120% overspeed operation times and the average annual high cycle fatigue times of the rotor blade root slot.

[0819] In some examples, the method further includes obtaining a crack extension calendar life for a third crack extension category based on the calendar life for a first stage of the third crack extension category, the calendar life for a second stage of the third crack extension category, and the calendar life for a third stage of the third crack extension category.

[0820] In some examples, the crack growth calendar life τ for the third crack growth category is CL3 The calculation process is as follows:

[0821]

[0822]

[0823]

[0824] τ CL3 =τ CL3,1 +τ CL3,2 +τ CL3,3

[0825] Among them, τ CL3,1 is the calendar life of the first stage of the third crack growth category, τ CL3,2 is the calendar life of the second stage of the third crack growth category, τ CL3,3 It is the calendar life of the third stage of the third crack growth category.

[0826] S1704, based on the stress corrosion crack growth life under the fourth crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, the crack growth calendar life under the fourth crack growth category is obtained.

[0827] In one embodiment, based on the stress corrosion crack growth life under the fourth crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, the crack growth calendar life under the fourth crack growth category is obtained, including obtaining the calendar life of each stage of the fourth crack growth category based on the stress corrosion crack growth life under the fourth crack growth category, the low cycle fatigue crack growth life of multiple stages and the high cycle fatigue crack growth life, and obtaining the crack growth calendar life under the fourth crack growth category based on the calendar life of each stage of the fourth crack growth category.

[0828] In some examples, the calendar life of the first stage of the fourth crack growth category is obtained based on the high cycle fatigue crack growth life under the fourth crack growth category, the low cycle fatigue crack growth life of the first stage of the fourth crack growth category of the normal shutdown transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the first stage of the fourth crack growth category of the 110% overspeed test transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the first stage of the fourth crack growth category of the 120% overspeed test transient condition of the nuclear power steam turbine, the annual average normal shutdown times of the nuclear power steam turbine, the annual average 110% overspeed test times, the annual average 120% overspeed operation times and the annual average high cycle fatigue times of the rotor blade root slot;

[0829] In some examples, the calendar life of the second stage of the fourth crack growth category is obtained based on the stress corrosion crack growth life under the first crack growth category, the high cycle fatigue crack growth life under the fourth crack growth category, the low cycle fatigue crack growth life of the second stage of the fourth crack growth category under the normal shutdown transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the second stage of the fourth crack growth category under the 110% overspeed test transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the second stage of the fourth crack growth category under the 120% overspeed test transient condition of the nuclear power steam turbine, the average annual normal shutdown times of the nuclear power steam turbine, the average annual 110% overspeed test times, the average annual 120% overspeed operation times and the average annual high cycle fatigue times of the rotor blade root slot.

[0830] In some examples, the method further includes obtaining a crack growth calendar life for a fourth crack growth category based on the calendar life for a first stage of the fourth crack growth category and the calendar life for a second stage of the fourth crack growth category.

[0831] In some examples, the crack growth calendar life τ for the fourth crack growth category is CL4 The calculation process is as follows:

[0832]

[0833]

[0834] τCL4 =τ CL4,1 +τ CL4,2

[0835] Among them, τ CL4,1 is the calendar life of the first stage of the fourth crack growth category, τ CL4,2 Calendar life of the second stage of the fourth crack growth category.

[0836] Therefore, in this method, if the target monitoring component is the rotor blade root slot, the average annual normal shutdown times of the nuclear power steam turbine, the average annual 110% overspeed test times, the average annual 120% overspeed operation times, the average annual high-cycle fatigue times of the rotor blade root slot, the stress corrosion crack growth life under a certain crack growth category of the rotor blade root slot, the low-cycle fatigue crack growth life in multiple stages, and the high-cycle fatigue crack growth life can be comprehensively considered to obtain the crack growth calendar life under the crack growth category.

[0837] The following takes the target monitoring component as a cylinder as an example to describe how to obtain the crack growth calendar life of the cylinder.

[0838] In one embodiment, it also includes the low-cycle fatigue crack growth life of the first stage of the nuclear power steam turbine cold start transient condition, the low-cycle fatigue crack growth life of the first stage of the nuclear power steam turbine warm start transient condition, the low-cycle fatigue crack growth life of the first stage of the nuclear power steam turbine hot start transient condition, the average annual number of cold starts, the average annual number of warm starts and the average annual number of hot starts of the nuclear power steam turbine, to obtain the calendar life of the first stage.

[0839] In one embodiment, it also includes obtaining the calendar life of the second stage based on the target stress corrosion crack growth life, the low-cycle fatigue crack growth life of the second stage of the cold start transient condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the second stage of the warm start transient condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the second stage of the hot start transient condition of the nuclear power steam turbine, the average annual number of cold starts, the average annual number of warm starts and the average annual number of hot starts of the nuclear power steam turbine.

[0840] In one embodiment, the method further includes obtaining a crack growth calendar life based on the calendar life of the first stage and the calendar life of the second stage. For example, obtaining a crack growth calendar life based on the calendar life of the first stage and the calendar life of the second stage includes determining the sum of the calendar life of the first stage and the calendar life of the second stage as the crack growth calendar life.

[0841] In some examples, the crack growth calendar life τ CL The calculation process is as follows:

[0842]

[0843]

[0844] τ CL =τ CL1 +τ CL2

[0845] Among them, τ CL1 is the calendar life of the first stage, τ CL2 is the calendar life of the second stage, y c is the annual average number of cold starts of nuclear power steam turbines, y w is the annual average number of warm-state starts, y h is the average number of hot starts per year.

[0846] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E in the above embodiment as an example, the calendar design monitoring basic data of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E is shown in Table 23.

[0847] Table 23 Calendar design monitoring basic data of low pressure inner cylinder

[0848] Serial number project Data Value 1 <![CDATA[Average annual cold start times y c / times]]> 4 2 <![CDATA[Annual average temperature state start-up times y w / times]]> 20 3 <![CDATA[Annual average number of hot start-ups y h / times]]> 75 4 <![CDATA[Crack growth life safety monitoring criterion value τ 0 / year]]> 60

[0849] The calculation process of the crack growth calendar life of the No. 1 low-pressure inner cylinder of nuclear power steam turbine E is as follows:

[0850]

[0851]

[0852] τ CL =τ CL1 +τ CL2 =45.13+8.81=53.94 years

[0853] The following takes the target monitoring component as a cylinder as an example to describe how to obtain the crack growth calendar life of the cylinder.

[0854] like Fig.18 As shown, if the target monitored component is a cylinder, the crack growth calendar life of the cylinder is obtained, including:

[0855] S1801, based on the stress corrosion crack growth life under the first crack growth category and the multi-stage low cycle fatigue crack growth life, obtain the crack growth calendar life under the first crack growth category.

[0856] In some examples, the calendar life of the first stage of the first crack growth category is obtained based on the low-cycle fatigue crack growth life of the first stage of the first crack growth category under the transient operating condition of cold start of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the first stage of the first crack growth category under the transient operating condition of warm start of the nuclear power steam turbine, the low-cycle fatigue crack growth life of the first stage of the first crack growth category under the transient operating condition of hot start of the nuclear power steam turbine, the average annual number of cold starts, the average annual number of warm starts and the average annual number of hot starts of the nuclear power steam turbine.

[0857] In some examples, the calendar life of the second stage of the first crack growth category is obtained based on the stress corrosion crack growth life under the first crack growth category, the low cycle fatigue crack growth life of the second stage of the first crack growth category under the cold start transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the second stage of the first crack growth category under the warm start transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the second stage of the first crack growth category under the hot start transient condition of the nuclear power steam turbine, the average annual number of cold starts, the average annual number of warm starts and the average annual number of hot starts of the nuclear power steam turbine.

[0858] In some examples, the method further includes obtaining a crack growth calendar life for the first crack growth category based on the calendar life for the first stage of the first crack growth category and the calendar life for the second stage of the first crack growth category.

[0859] In some examples, the crack growth calendar life τ under the first crack growth category is CL1 The calculation process is as follows:

[0860]

[0861]

[0862] τ CL1 =τ CL1,1 +τ CL1,2

[0863] Among them, τ CL1,1 is the calendar life of the first stage of the first crack growth category, τ CL1,2 is the calendar life of the second stage of the first crack growth category, y c is the annual average number of cold starts of nuclear power steam turbines, y w is the annual average number of warm-state starts of nuclear power steam turbines, y h is the average annual number of hot starts of nuclear power steam turbines.

[0864] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power turbine A in the above embodiment as an example, the crack extension category of the No. 1 low-pressure inner cylinder of the nuclear power turbine A is the first crack extension category, and the calendar design monitoring basic data of the No. 1 low-pressure inner cylinder of the nuclear power turbine A is shown in Table 24.

[0865] Table 24 Calendar design monitoring basic data of low pressure inner cylinder

[0866] Serial number project Data Value 1 <![CDATA[Average annual cold start times y c / times]]> 4 2 <![CDATA[Annual average temperature state starting times y w / times]]> 20 3 <![CDATA[Annual average number of hot starts y h / times]]> 75 4 <![CDATA[Crack propagation life safety monitoring criterion value τ 0 / year]]> 60

[0867] Crack growth calendar life τ of the first crack growth category of the No. 1 low-pressure inner cylinder of nuclear power steam turbine A CL1 The calculation process is as follows:

[0868]

[0869] For example, continuing to take the No. 2 low-pressure inner cylinder of the nuclear power turbine B in the above embodiment as an example, the crack extension category of the No. 2 low-pressure inner cylinder of the nuclear power turbine B is the first crack extension category, and the calendar design monitoring basic data of the No. 2 low-pressure inner cylinder of the nuclear power turbine B is shown in Table 24.

[0870] Crack growth calendar life τ of the No. 2 low-pressure inner cylinder of nuclear power steam turbine B under the first crack growth category CL1 The calculation process is as follows:

[0871]

[0872] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power turbine C in the above embodiment as an example, the crack extension category of the No. 1 low-pressure inner cylinder of the nuclear power turbine C is the first crack extension category, and the calendar design monitoring basic data of the No. 1 low-pressure inner cylinder of the nuclear power turbine C is shown in Table 25.

[0873] Table 25 Calendar design monitoring basic data of low pressure inner cylinder

[0874] Serial number project Data Value 1 <![CDATA[Annual average cold start times y c / times]]> 4 2 <![CDATA[Average annual temperature state start-up times y w / times]]> 20 3 <![CDATA[Annual average number of hot start-ups y h / times]]> 75 4 <![CDATA[The planned overhaul interval τ of a nuclear power steam turbine m / year]]> 10

[0875] Crack growth calendar life τ of the first crack growth category of the No. 1 low-pressure inner cylinder of nuclear power steam turbine C CL1 The calculation process is as follows:

[0876]

[0877] S1802, based on the stress corrosion crack growth life under the second crack growth category and the multi-stage low cycle fatigue crack growth life, obtain the crack growth calendar life under the second crack growth category.

[0878] In some examples, the calendar life of the first stage of the second crack growth category is obtained based on the stress corrosion crack growth life under the second crack growth category, the low cycle fatigue crack growth life of the first stage of the second crack growth category under the cold start transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the first stage of the second crack growth category under the warm start transient condition of the nuclear power steam turbine, the low cycle fatigue crack growth life of the first stage of the second crack growth category under the hot start transient condition of the nuclear power steam turbine, the average annual number of cold starts, the average annual number of warm starts and the average annual number of hot starts of the nuclear power steam turbine.

[0879] In some examples, the method further includes obtaining a crack growth calendar life based on the calendar life of the first stage of the second crack growth category.

[0880] In some examples, the crack growth calendar life τ for the second crack growth category is CL2 The calculation process is as follows:

[0881]

[0882] Among them, τ CL2,1 Calendar life of the first stage of the second crack growth category.

[0883] For example, continuing to take the No. 2 low-pressure inner cylinder of the nuclear power turbine D in the above embodiment as an example, the crack extension category of the No. 2 low-pressure inner cylinder of the nuclear power turbine D is the second crack extension category, and the calendar design monitoring basic data of the No. 2 low-pressure inner cylinder of the nuclear power turbine D is shown in Table 25.

[0884] Crack growth calendar life τ of the No. 2 low-pressure inner cylinder of nuclear power steam turbine D under the second crack growth category CL2 The calculation process is as follows:

[0885]

[0886] Therefore, if the target monitored component in this method is a cylinder, the annual average number of cold starts, annual average number of warm starts and annual average number of hot starts of the nuclear power steam turbine, the stress corrosion crack growth life under the crack growth category of the cylinder and the multi-stage low-cycle fatigue crack growth life can be comprehensively considered to obtain the crack growth calendar life of the cylinder.

[0887] Fig.19 The present invention is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine throughout its entire life cycle according to another embodiment of the present invention.

[0888] like Fig.19 As shown, the stress corrosion and fatigue long-life monitoring method for a nuclear power steam turbine during its entire life cycle according to an embodiment of the present disclosure includes:

[0889] S1901, determining one or more target monitoring components from the components to be monitored.

[0890] S1902, determining the long-life monitoring data required for the target monitoring component, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life.

[0891] For the relevant contents of steps S1901-S1902, please refer to the above embodiments and will not be repeated here.

[0892] S1903: If the nuclear power steam turbine is in the design stage, obtain the crack growth life safety monitoring criterion value of the target monitoring component.

[0893] S1904: If the crack growth calendar life is less than the crack growth life safety monitoring criterion value, it is determined that the crack growth calendar life does not meet the first monitoring qualification condition.

[0894] S1905, if the crack growth calendar life is greater than or equal to the crack growth life safety monitoring criterion value, it is determined that the crack growth calendar life meets the first monitoring qualification condition.

[0895] For example, taking the welded low-pressure rotor of a certain type of 1200MW nuclear power steam turbine in the above embodiment as an example, the crack propagation calendar life τ of the welded low-pressure rotor is CL The crack growth life safety monitoring criterion value τ of the welded low-pressure rotor is 162.69 years. 0 As shown in Table 21, τ 0 = 60 years, then τ CL >τ 0 , it can be judged that the crack propagation calendar life meets the first monitoring qualification condition.

[0896] For example, taking the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E in the above embodiment as an example, the crack growth calendar life τ of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E is CL =53.94 years, the crack growth life safety monitoring criterion value τ of the No. 1 low-pressure inner cylinder of nuclear power steam turbine E 0 As shown in Table 23, τ 0 = 60 years, then τ CL <τ 0 , it can be judged that the crack propagation calendar life does not meet the first monitoring qualification condition.

[0897] S1906: If the crack propagation calendar life does not meet the first monitoring qualification condition, obtain abnormal data of the target monitoring component in the design stage.

[0898] S1907, optimizing and improving the abnormal data of the target monitoring component in the design phase, and returning to execute the process of obtaining the crack growth calendar life, until the obtained crack growth calendar life meets the first monitoring qualification condition.

[0899] The following describes the optimization and improvement of the rotor by taking the rotor as an example of the monitoring component.

[0900] It should be noted that there are not too many restrictions on the abnormal data of the rotor in the design stage. For example, it may include the design process parameters of the rotor, the basic data for stress calculation of the rotor in the design stage, the basic data for rotor material testing, etc.

[0901] In one embodiment, the abnormal data of the rotor in the design stage is optimized and improved, including selecting materials with good stress corrosion resistance; selecting materials with good fatigue performance; adopting a welded rotor structure; adopting a whole rotor structure; avoiding structures that cause stress concentration in high stress areas; increasing the fillet radius of the rotor blade root slot structure to reduce the stress concentration coefficient; changing the axial key of the set impeller to a radial key; increasing the assembly gap between the set rotor key and the keyway; optimizing the starting parameter change curve of the nuclear power steam turbine to reduce the rotor thermal stress under the starting transient condition; optimizing the normal shutdown parameter change curve of the nuclear power steam turbine to reduce the rotor thermal stress under the shutdown transient condition; optimizing the load change parameter change curve of the nuclear power steam turbine to reduce the rotor thermal stress under the starting transient condition; using heat treatment technology to improve material toughness; improving processing accuracy and eliminating machining stress concentration; using heat treatment technology to reduce residual tensile stress; rolling the impeller surface to form surface compressive stress; shot peening the blade root slot to improve fatigue performance, etc.

[0902] The following takes the cylinder as an example of the monitored component to describe the optimization and improvement of the cylinder.

[0903] It should be noted that there are not too many restrictions on the abnormal data of the cylinder in the design stage. For example, it may include the design process parameters of the cylinder, the basic data of the stress calculation of the cylinder in the design stage, the basic data of the cylinder material test, etc.

[0904] In one embodiment, the abnormal data of the cylinder in the design stage is optimized and improved, including selecting materials with good stress corrosion resistance; selecting materials with good low-cycle fatigue performance; avoiding structures that cause stress concentration in high stress areas; adopting structural fillet transition at the structural discontinuity of the connection between the turbine steam inlet pipe and the cylinder; adopting structural fillet transition at the structural discontinuity of the connection between the turbine steam extraction pipe and the cylinder; increasing the fillet radius of the connection between the cylinder and the steam extraction pipe to reduce the stress concentration coefficient; designing the cylinder weld to be away from the stress concentration; optimizing the nuclear power steam turbine starting parameter change curve to reduce the cylinder thermal stress under the starting transient working condition; optimizing the nuclear power steam turbine load change parameter change curve to reduce the cylinder thermal stress under the starting transient working condition; using heat treatment technology to improve material toughness; improving processing accuracy to eliminate machining stress concentration; using heat treatment technology to reduce welding residual tensile stress; rolling the cylinder surface to form surface compressive stress; shot peening the cylinder surface to improve fatigue performance, etc.

[0905] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E in the above embodiment as an example, the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E has weak lifespan, namely, the connection between the inner cylinder and the second-stage steam extraction pipe, and the structural transition fillet radius of the structural discontinuity at the connection between the second-stage steam extraction pipe and the low-pressure inner cylinder is increased from the original design 5mm to 20mm, and the structure of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E is optimized and improved.

[0906] A model of the optimized structure of the No. 1 low-pressure inner cylinder of nuclear power steam turbine E is established, and the temperature field and stress field calculations are performed. The basic data for stress calculation and material testing of the No. 1 low-pressure inner cylinder of nuclear power steam turbine E are updated. The specific data are shown in Table 26.

[0907] Table 26 Basic data for design and monitoring of low-pressure inner cylinder

[0908]

[0909] Using the updated stress calculation basic data and material test basic data of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E shown in Table 26, the crack growth size set, stress corrosion crack growth life, multi-stage low-cycle fatigue crack growth life, multi-stage calendar life and crack growth calendar life of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E are recalculated. The specific data are shown in Tables 27, 28, 29 and 30.

[0910] Table 27 Crack extension size collection of low pressure inner cylinder

[0911]

[0912]

[0913] Table 28 Stress corrosion crack growth life and target stress corrosion crack growth life of various types of low-pressure inner cylinders

[0914] Serial number project Data Value 1 <![CDATA[The first stress corrosion crack growth life N fSCC1 / year]]> 22.741 2 <![CDATA[The second stress corrosion crack growth life N fSCC2 / year]]> 19.832 3 <![CDATA[The third stress corrosion crack growth life N fSCC3 / year]]> 26.477 4 <![CDATA[Stress corrosion crack growth life N fSCC / year]]> 19.832

[0915] Table 29 Multi-stage low-cycle fatigue crack growth life of low-pressure inner cylinder

[0916]

[0917] Table 30 Multi-stage calendar life and crack growth calendar life of low-pressure inner cylinder

[0918] Serial number project Data Value 1 <![CDATA[Calendar life τ of the first stage CL1 / year]]> 123.73 2 <![CDATA[Calendar life τ of the second stage CL1 / year]]> 14.96 3 <![CDATA[Crack growth calendar life τ CL / year]]> 138.69

[0919] It can be seen from Table 30 that after the structural optimization and improvement of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E, the crack growth calendar life τ of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine E CL =138.69 years, which is greater than the crack growth life safety monitoring criterion value τ of nuclear power steam turbine 0 =60 years, the crack propagation calendar life of the low-pressure inner cylinder meets the first monitoring qualification condition, and the crack propagation life safety monitoring of the low-pressure inner cylinder is ended.

[0920] In summary, according to the stress corrosion and fatigue long-life monitoring method for the entire life cycle of a nuclear power steam turbine according to an embodiment of the present disclosure, if the nuclear power steam turbine is in the design stage, the crack propagation life safety monitoring criterion value of the target monitoring component is obtained, and based on the size relationship between the crack propagation calendar life and the crack propagation life safety monitoring criterion value, it is judged whether the crack propagation calendar life meets the first monitoring qualification condition, if the crack propagation calendar life does not meet the first monitoring qualification condition, the abnormal data of the target monitoring component in the design stage is obtained, the abnormal data of the target monitoring component in the design stage is optimized and improved, and the process of obtaining the crack propagation calendar life is returned to execute until the obtained crack propagation calendar life meets the first monitoring qualification condition, which helps to improve the safety of the target monitoring component in the design stage and is suitable for monitoring the target monitoring component in the design stage of the nuclear power steam turbine.

[0921] Fig. 20 The present invention is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine throughout its entire life cycle according to another embodiment of the present invention.

[0922] like Fig. 20 As shown, the stress corrosion and fatigue long-life monitoring method for a nuclear power steam turbine during its entire life cycle according to an embodiment of the present disclosure includes:

[0923] S2001, determining one or more target monitoring components from the components to be monitored.

[0924] S2002, determining the long-life monitoring data required for the target monitoring component, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life.

[0925] For the relevant contents of steps S2001-S2002, please refer to the above embodiment and will not be repeated here.

[0926] S2003, if the nuclear power steam turbine is in the manufacturing stage, a safety factor is obtained based on the crack growth calendar life and the crack growth life safety monitoring criterion value of the target monitoring component.

[0927] S2004, determine whether the safety factor meets the second monitoring qualification condition.

[0928] In one embodiment, a safety factor is obtained based on the crack growth calendar life and the crack growth life safety monitoring criterion value of the target monitoring component, including determining the ratio or difference between the crack growth calendar life and the crack growth life safety monitoring criterion value as the safety factor.

[0929] In one embodiment, the safety factor is positively correlated with the crack growth calendar life and negatively correlated with the crack growth life safety monitoring criterion value.

[0930] It should be noted that the second monitoring qualified condition is not too limited, for example, the safety factor can be greater than the first set threshold value, which is determined as the second monitoring qualified condition. The first set threshold is not too limited, for example, it can be 1.

[0931] The following describes the crack propagation life safety monitoring of the rotor blade root slot by taking the rotor blade root slot as an example of the target monitoring component.

[0932] For example, continuing to take the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A in the above embodiment as an example, the crack extension category of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is the first crack extension category, and the crack extension life safety monitoring criterion value of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A is shown in Table 22, and the crack extension calendar life τ of the fifth-stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of the nuclear power steam turbine A under the first crack extension category CL1 is 71.39 years, τ 0 = 60 years, then the safety factor S F The calculation process is as follows:

[0933]

[0934] It can be seen that the safety factor S of the fifth stage inverted T-shaped blade root groove of the No. 1 low-pressure rotor of nuclear power steam turbine A is F =1.19>1, determine the safety factor S F The second monitoring qualification condition is met.

[0935] The following takes the target monitoring component as an example of a cylinder to describe the crack propagation life safety monitoring of the cylinder.

[0936] For example, continuing to take the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A in the above embodiment as an example, the crack extension category of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A is the first crack extension category, and the crack extension life safety monitoring criterion value of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A is shown in Table 24, and the crack extension calendar life τ of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine A under the first crack extension category is CL1 is 138.69 years, τ 0 = 60 years, then the safety factor S F The calculation process is as follows:

[0937]

[0938] It can be known that the safety factor S of the No. 1 low-pressure inner cylinder of nuclear power steam turbine A is F =2.31>1, determine the safety factor S F The second monitoring qualification condition is met.

[0939] For example, continuing to take the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B in the above embodiment as an example, the crack extension category of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B is the first crack extension category, and the crack extension life safety monitoring criterion value of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B is shown in Table 24, and the crack extension calendar life τ of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B under the first crack extension category is CL1 is 47.83 years, τ 0 = 60 years, then the safety factor S F The calculation process is as follows:

[0940]

[0941] It can be known that the safety factor S of the No. 2 low-pressure inner cylinder of nuclear power steam turbine B is F =0.79<1, determine the safety factor S F The second monitoring eligibility condition is not met.

[0942] S2005: If the safety factor does not meet the second monitoring qualification condition, obtain abnormal data of the target monitoring component during the manufacturing stage.

[0943] S2006, optimizing and improving the abnormal data of the target monitoring component in the manufacturing stage, and returning to execute the process of obtaining the safety factor until the obtained safety factor meets the second monitoring qualification condition.

[0944] The following describes the optimization and improvement of the rotor blade root slot by taking the rotor blade root slot as an example of the target monitoring component.

[0945] It should be noted that there are not too many restrictions on the abnormal data of the rotor blade root slot during the manufacturing stage. For example, it may include the manufacturing process parameters of the rotor blade root slot, the basic data for stress calculation of the rotor blade root slot during the manufacturing stage, and the basic data for rotor material testing of nuclear power turbines during the manufacturing stage.

[0946] In some examples, the abnormal data of the rotor blade root slot during the manufacturing stage are optimized and improved, including turning or grinding the rotor blade root slot cracks; turning to increase the fillet radius of the rotor blade root slot without affecting the structural strength of the rotor blade root slot; local repair welding; using local heat treatment process to eliminate welding residual stress; finishing and polishing the repair welding area; improving processing accuracy and eliminating machining stress concentration; performing phased array non-destructive monitoring again to determine the depth of the blade root slot cracks; shot peening the blade root slot to improve fatigue performance, etc.

[0947] The following takes the cylinder as an example of the target monitoring component to describe the optimization and improvement of the cylinder.

[0948] It should be noted that there are not too many restrictions on the abnormal data of the cylinder during the manufacturing stage. For example, it may include the manufacturing process parameters of the cylinder, the basic data for stress calculation of the cylinder during the manufacturing stage, and the basic data for material testing of the nuclear power turbine during the manufacturing stage.

[0949] In one embodiment, the abnormal data of the cylinder in the manufacturing stage is optimized and improved, including turning or grinding the nuclear power turbine cylinder cracks; turning to increase the fillet radius of the nuclear power turbine cylinder without affecting the structural strength of the nuclear power turbine cylinder; local repair welding; using local heat treatment process to eliminate welding residual stress; fine machining and polishing of the repair welding area; improving machining accuracy and eliminating machining stress concentration; performing phased array non-destructive monitoring again to determine the depth of the cylinder crack; and shot peening the cylinder to improve fatigue performance.

[0950] For example, taking the No. 2 low-pressure inner cylinder of the nuclear power steam turbine B in the above embodiment as an example, the safety factor S FIf the second monitoring qualification condition is not met, the abnormal data of the No. 2 low-pressure inner cylinder of nuclear power steam turbine B in the manufacturing stage can be optimized and improved. For example, a combination of partial optimization and improvement strategies can be used to turn or grind the nuclear power steam turbine cylinder cracks, locally repair welding, use local heat treatment processes to eliminate welding residual stress, and fine-process and polish the repair welding parts. The No. 2 low-pressure inner cylinder of nuclear power steam turbine B after optimization and improvement is subjected to phased array nondestructive testing again, and no cracks are found. In the case that no cracks are found in the phased array nondestructive testing, the crack depth a of the connection between the No. 2 low-pressure inner cylinder of nuclear power steam turbine B and the second-stage steam extraction pipeline is given. i =2mm=0.002m.

[0951] The crack growth life safety monitoring under the combined action of stress corrosion cracking and low cycle fatigue damage is carried out again, and the crack growth calendar life of the No. 2 low pressure inner cylinder of nuclear power steam turbine B is recalculated. If the recalculated crack growth calendar life is the crack growth calendar life τ under the first crack growth category CL1 is 138.69 years, τ 0 = 60 years, then the safety factor S F The calculation process is as follows:

[0952]

[0953] It can be known that the safety factor S of the No. 2 low-pressure inner cylinder of nuclear power steam turbine B is F =2.31>1, determine the safety factor S F The second monitoring qualification condition is met, and the crack extension life safety monitoring of the No. 2 low-pressure inner cylinder of nuclear power turbine B is ended.

[0954] In summary, according to the stress corrosion and fatigue long-life monitoring method for the entire life cycle of a nuclear power steam turbine according to an embodiment of the present disclosure, if the nuclear power steam turbine is in the manufacturing stage, a safety factor is obtained based on the crack propagation calendar life and the crack propagation life safety monitoring criterion value of the target monitoring component, and it is determined whether the safety factor meets the second monitoring qualification condition. If the safety factor does not meet the second monitoring qualification condition, the abnormal data of the target monitoring component in the manufacturing stage is obtained, the abnormal data of the target monitoring component in the manufacturing stage is optimized and improved, and the process of obtaining the safety factor is returned until the obtained safety factor meets the second monitoring qualification condition. This helps to improve the safety of the target monitoring component in the manufacturing stage, and is suitable for monitoring the target monitoring component in the manufacturing stage of the nuclear power steam turbine.

[0955] Fig.21 The present invention is a flow chart of a method for monitoring stress corrosion and fatigue of a nuclear power steam turbine throughout its entire life cycle according to another embodiment of the present invention.

[0956] like Fig.21As shown, the stress corrosion and fatigue long-life monitoring method for a nuclear power steam turbine during its entire life cycle according to an embodiment of the present disclosure includes:

[0957] S2101, determining one or more target monitoring components from the components to be monitored.

[0958] S2102, determining the long-life monitoring data required for the target monitoring component, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life.

[0959] For the relevant contents of steps S2101-S2102, please refer to the above embodiment and will not be repeated here.

[0960] S2103, if the nuclear power steam turbine is in use, obtain the safety factor based on the crack growth calendar life and the planned overhaul interval of the nuclear power steam turbine.

[0961] S2104, determine whether the safety ratio meets the third monitoring qualification condition.

[0962] In one embodiment, a safety factor is obtained based on the crack growth calendar life and the planned overhaul interval of the nuclear power steam turbine, including determining the ratio or difference between the crack growth calendar life and the planned overhaul interval as the safety factor.

[0963] In one embodiment, the safety factor is positively correlated with the crack growth calendar life and negatively correlated with the planned overhaul interval.

[0964] It should be noted that the third monitoring qualified condition is not too limited, for example, the safety multiple can be greater than the second set threshold value, which is determined as the third monitoring qualified condition. The second set threshold is not too limited, for example, it can be 2.

[0965] The following describes the crack propagation life safety monitoring of the rotor blade root slot by taking the rotor blade root slot as an example of the target monitoring component.

[0966] For example, taking the fifth stage inverted T-shaped blade root groove of the second low-pressure rotor of the nuclear power steam turbine B in the above embodiment as an example, the crack propagation category of the fifth stage inverted T-shaped blade root groove of the second low-pressure rotor of the nuclear power steam turbine B is the first crack propagation category, and the planned overhaul interval τ of the nuclear power steam turbine B is m As shown in Table 22, the crack growth calendar life τ of the first crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B is CL1 is 31.29 years, τ m = 10 years, then the safety factor S R The calculation process is as follows:

[0967]

[0968] It can be seen that the safety factor S of the 5th stage inverted T-shaped blade root groove of the No. 2 low-pressure rotor of nuclear power steam turbine B is R =3.13>2, determine the safety factor S R The third monitoring qualification condition is met.

[0969] Continuing to take the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment as an example, the crack growth category of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is the second crack growth category, and the planned overhaul interval τ of the nuclear power steam turbine C is m As shown in Table 22, the crack growth calendar life τ of the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of nuclear power steam turbine C under the second crack growth category CL2 is 12.93 years, τ m = 10 years, then the safety factor S R The calculation process is as follows:

[0970]

[0971] It can be seen that the safety factor S of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of nuclear power steam turbine C is R =1.29<2, determine the safety factor S R The third monitoring qualification condition is not met.

[0972] The following takes the target monitoring component as an example of a cylinder to describe the crack propagation life safety monitoring of the cylinder.

[0973] For example, taking the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C in the above embodiment as an example, the crack growth category of the No. 1 low-pressure inner cylinder of the nuclear power steam turbine C is the first crack growth category, and the planned overhaul interval τ of the nuclear power steam turbine C is m As shown in Table 25, the crack growth calendar life τ of the first crack growth category of the No. 1 low-pressure inner cylinder of nuclear power steam turbine C is CL1 is 47.83 years, τ m = 10 years, then the safety factor S R The calculation process is as follows:

[0974]

[0975] It can be seen that the safety factor S of the No. 1 low-pressure inner cylinder of nuclear power steam turbine C is R =4.78>2, determine the safety factor S R The third monitoring qualification condition is met.

[0976] For example, taking the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D in the above embodiment as an example, the crack growth category of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D is the second crack growth category, and the planned overhaul interval τ of the nuclear power steam turbine D is m As shown in Table 25, the crack growth calendar life τ of the second crack growth category of the No. 2 low-pressure inner cylinder of nuclear power steam turbine D is CL2 is 13.65 years, τ m = 10 years, then the safety factor S R The calculation process is as follows:

[0977]

[0978] It can be seen that the safety factor S of the No. 2 low-pressure inner cylinder of nuclear power steam turbine D is R =1.37<2, determine the safety factor S R The third monitoring qualification condition is not met.

[0979] S2105: If the safety multiple does not meet the third monitoring qualification condition, obtain abnormal data of the target monitoring component during the use phase.

[0980] S2106, optimizing and improving the abnormal data of the target monitoring component during the use phase, and returning to execute the process of obtaining the safety multiple until the obtained safety multiple meets the third monitoring qualification condition.

[0981] The following describes the optimization and improvement of the rotor blade root slot by taking the rotor blade root slot as an example of the target monitoring component.

[0982] It should be noted that there are not too many restrictions on the abnormal data of the rotor blade root slot during the use stage. For example, it may include the use process parameters of the rotor blade root slot, the basic data for stress calculation of the rotor blade root slot during the use stage, and the basic data for rotor material testing of nuclear power turbines during the use stage.

[0983] In some examples, the abnormal data of the rotor blade root slot during the use stage are optimized and improved, including turning or grinding the cracks in the rotor blade root slot; turning to increase the fillet radius of the rotor blade root slot without affecting the structural strength of the rotor blade root slot; local repair welding; using local heat treatment process to eliminate welding residual stress; finishing and polishing the repair welding area; improving processing accuracy and eliminating machining stress concentration; performing phased array non-destructive monitoring again to determine the crack depth of the blade root slot; shot peening the blade root slot to improve fatigue performance, etc.

[0984] Continuing with the example of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C in the above embodiment, its safety factor S RThe third monitoring qualification condition is not met. The abnormal data of the inverted T-shaped blade root groove of the 5th stage of the No. 3 low-pressure rotor of the nuclear power steam turbine C during the use stage can be optimized and improved. The phased array nondestructive monitoring of the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C after optimization and improvement is performed again. No cracks are found. Given the crack depth a i =2mm=0.002m.

[0985] The crack growth life safety monitoring under the combined effects of stress corrosion cracking, high cycle fatigue damage and low cycle fatigue damage is conducted again, and the crack growth calendar life of the fifth stage inverted T-shaped blade root groove of the No. 3 low pressure rotor of nuclear power steam turbine C is recalculated. If the recalculated crack growth calendar life is the crack growth calendar life τ under the first crack growth category CL1 is 71.39 years, τ m = 10 years, then the safety factor S R The calculation process is as follows:

[0986]

[0987] It can be seen that the safety factor S of the fifth stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of nuclear power steam turbine C is R =7.14>2, determine the safety factor S R The third monitoring qualification condition is met, and the crack extension life safety monitoring of the 5th stage inverted T-shaped blade root groove of the No. 3 low-pressure rotor of the nuclear power steam turbine C is completed.

[0988] The following takes the cylinder as an example of the target monitoring component to describe the optimization and improvement of the cylinder.

[0989] It should be noted that there are not too many restrictions on the abnormal data of the cylinder during the use stage. For example, it may include the cylinder's operating process parameters, the basic data for stress calculation of the cylinder during the use stage, the basic data for material testing of the nuclear power turbine during the use stage, etc.

[0990] In one embodiment, the abnormal data of the cylinder during the use stage is optimized and improved, including turning or grinding the nuclear power turbine cylinder cracks; turning to increase the fillet radius of the nuclear power turbine cylinder without affecting the structural strength of the nuclear power turbine cylinder; local repair welding; using local heat treatment process to eliminate welding residual stress; fine machining and polishing the repair welding part; improving machining accuracy and eliminating machining stress concentration; performing phased array non-destructive monitoring again to determine the depth of the cylinder crack; cylinder shot peening to improve fatigue performance; optimizing the cold start parameter change curve of the nuclear power turbine to reduce the cylinder thermal stress under cold start transient conditions; optimizing the warm start parameter change curve of the nuclear power turbine to reduce the cylinder thermal stress under warm start transient conditions; optimizing the hot start parameter change curve of the nuclear power turbine to reduce the cylinder thermal stress under hot start transient conditions; strengthening the technical supervision of chemical water to ensure that the water quality of condensate meets the requirements; timely blocking the pipes after the condenser tube bundle leaks to prevent a large amount of circulating water from leaking into the condensate, etc.

[0991] For example, taking the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D in the above embodiment as an example, the safety factor S R If the third monitoring qualification condition is not met, the abnormal data of the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D during the use phase can be optimized and improved. For example, turning or grinding the nuclear power steam turbine cylinder cracks, local repair welding, local heat treatment process and elimination of welding residual stress, fine machining and polishing of the repair welding part, improving machining accuracy, and eliminating the machining stress concentration part of the optimization and improvement strategy combination, and the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D after optimization and improvement is again subjected to phased array nondestructive testing, and no cracks are found. In the case that no cracks are found in the phased array nondestructive testing, the crack depth a of the connection between the No. 2 low-pressure inner cylinder of the nuclear power steam turbine D and the second-stage steam extraction pipeline is given. i =2mm=0.002m.

[0992] The crack growth life safety monitoring under the combined action of stress corrosion cracking and low cycle fatigue damage is carried out again, and the crack growth calendar life of the No. 2 low pressure inner cylinder of nuclear power steam turbine D is recalculated. If the recalculated crack growth calendar life is the crack growth calendar life τ under the first crack growth category CL1 is 138.69 years, τ m = 10 years, then the safety factor S R The calculation process is as follows:

[0993]

[0994] It can be seen that the safety factor S of the No. 2 low-pressure inner cylinder of nuclear power steam turbine D is R =13.87>2, determine the safety factor S R The third monitoring qualification condition is met, and the crack extension life safety monitoring of the No. 2 low-pressure inner cylinder of the nuclear power turbine D is completed.

[0995] In summary, according to the long-life monitoring method for stress corrosion and fatigue of a nuclear power steam turbine throughout its life cycle in an embodiment of the present disclosure, if the nuclear power steam turbine is in the use stage, a safety factor is obtained based on the crack propagation calendar life and the planned overhaul interval of the nuclear power steam turbine, and it is determined whether the safety factor satisfies the third monitoring qualified condition. If the safety factor does not meet the third monitoring qualified condition, the abnormal data of the target monitoring component in the use stage is obtained, the abnormal data of the target monitoring component in the use stage is optimized and improved, and the process of obtaining the safety factor is returned until the obtained safety factor meets the third monitoring qualified condition. This helps to improve the safety of the target monitoring component in the use stage and is suitable for monitoring the target monitoring component in the use stage of the nuclear power steam turbine.

[0996] In order to realize the above-mentioned embodiments, the present disclosure also proposes a stress corrosion and fatigue long-life monitoring device for a nuclear power steam turbine during its entire life cycle.

[0997] Fig. 22 The present invention is a schematic structural diagram of a device for monitoring stress corrosion and fatigue over the entire life of a nuclear power steam turbine according to an embodiment of the present invention.

[0998] like Fig. 22 As shown, the stress corrosion and fatigue long-life monitoring device 100 for a nuclear power steam turbine during its entire life cycle according to an embodiment of the present disclosure includes: a first determination module 110 , a second determination module 120 and a monitoring module 130 .

[0999] A first determining module 110 is used to determine one or more target monitoring components from the components to be monitored;

[1000] A second determination module 120, configured to determine the long-life monitoring data required for the target monitoring component, wherein the long-life monitoring data includes a stress corrosion crack growth life and a fatigue crack growth life, and the fatigue crack growth life includes at least one of a low-cycle fatigue crack growth life and a high-cycle fatigue crack growth life;

[1001] The monitoring module 130 is used to perform crack propagation life safety monitoring on the target monitoring component based on the long life monitoring data required by the target monitoring component.

[1002] In one embodiment of the present disclosure, the second determination module 120 is further used to: obtain a mapping relationship between the target monitoring component and the long-life monitoring data; and determine the long-life monitoring data required by the target monitoring component based on the mapping relationship.

[1003] In one embodiment of the present disclosure, the second determination module 120 is further used to: if the target monitoring component is a rotor blade root slot or a rotor, determine that the long-life monitoring data required for the target monitoring component includes the stress corrosion crack growth life, the low-cycle fatigue crack growth life and the high-cycle fatigue crack growth life; if the target monitoring component is a cylinder, determine that the long-life monitoring data required for the target monitoring component includes the stress corrosion crack growth life and the low-cycle fatigue crack growth life.

[1004] In one embodiment of the present disclosure, the first determination module 110 is further used to: obtain a crack extension life safety monitoring instruction; extract an identifier of the target monitoring component from the crack extension life safety monitoring instruction; and determine one or more target monitoring components from the components to be monitored based on the identifier of the target monitoring component.

[1005] In one embodiment of the present disclosure, the first determination module 110 is further used to: obtain a crack extension life safety monitoring instruction sent by a remote client; and determine the component to be monitored associated with the remote client as the target monitoring component.

[1006] In one embodiment of the present disclosure, the second determination module 120 is further used to: obtain a crack extension size set of the target monitoring component; and determine the long-life monitoring data required for the target monitoring component based on the crack extension size set.

[1007] In one embodiment of the present disclosure, the second determination module 120 is further used to: obtain stress calculation basic data of the target monitoring component; obtain material test basic data of the target monitoring component; and determine the crack extension size set based on the stress calculation basic data and the material test basic data.

[1008] In one embodiment of the present disclosure, the second determining module 120 is further configured to:

[1009] Determine a stress corrosion crack extension size threshold value of the target monitoring component based on the crack shape parameters of the target monitoring component, the stress corrosion fracture toughness of the material of the target monitoring component, and the maximum stress at the crack site of the target monitoring component under the steady-state condition of the nuclear power steam turbine under load operation;

[1010] Based on the crack shape parameters of the target monitoring component, the fracture toughness of the material of the target monitoring component and the maximum stress at the crack site of the target monitoring component under the set operating condition of the nuclear power turbine, the low-cycle fatigue critical crack size of the target monitoring component under the set operating condition of the nuclear power turbine is determined.

[1011] In one embodiment of the present disclosure, the second determining module 120 is further configured to:

[1012] Determine the high cycle fatigue crack extension size threshold value of the target monitoring component based on the crack shape parameters of the target monitoring component, the test value of the high cycle fatigue crack extension threshold value of the material of the target monitoring component, and the high cycle fatigue stress range of the crack position of the target monitoring component under the steady-state condition of the nuclear power steam turbine under load operation;

[1013] Based on the crack shape parameters of the target monitored component, the fracture toughness of the material of the target monitored component, and the maximum stress at the crack site of the target monitored component under steady-state conditions of load operation of the nuclear power turbine, the high-cycle fatigue critical crack size of the target monitored component is determined.

[1014] In one embodiment of the present disclosure, the second determination module 120 is further used to obtain the stress corrosion crack growth life based on the first parameter of the target monitoring component, the annual average stress corrosion crack growth rate test value of the material of the target monitoring component, and the low-cycle fatigue critical crack size of the target monitoring component under the set operating conditions of the nuclear power steam turbine; wherein the first parameter is the phased array detection crack depth of the target monitoring component or the stress corrosion crack growth size threshold value.

[1015] In one embodiment of the present disclosure, the second determination module 120 is also used to obtain the low-cycle fatigue crack growth life of at least one stage of the set operating condition of the nuclear power steam turbine based on the second parameter of the target monitoring component, the crack shape parameter of the target monitoring component, the material low-cycle fatigue crack growth test constant of the target monitoring component, and the maximum stress at the crack site of the target monitoring component under the set operating condition of the nuclear power steam turbine; wherein the second parameter is any one of the phased array detection crack depth, initial crack size, and the crack growth size set of the target monitoring component.

[1016] In one embodiment of the present disclosure, the second determination module 120 is further used to obtain the high fatigue crack growth life based on the third parameter of the target monitoring component, the high cycle fatigue critical crack size, the crack shape parameter of the target monitoring component, the material high cycle fatigue crack growth test constant of the target monitoring component, and the high cycle fatigue stress range of the crack site of the target monitoring component under the steady-state condition of load operation of the nuclear power steam turbine; wherein the third parameter is the phased array detection crack depth of the target monitoring component or the high cycle fatigue crack growth size threshold value.

[1017] In one embodiment of the present disclosure, the monitoring module 130 is further used to: obtain the crack propagation calendar life of the target monitoring component based on the long-life monitoring data required by the target monitoring component; and perform crack propagation life safety monitoring of the target monitoring component based on the crack propagation calendar life.

[1018] In one embodiment of the present disclosure, the monitoring module 130 is further used to: obtain the multi-stage calendar life of the target monitoring component based on the long-life monitoring data required by the target monitoring component; and obtain the crack extension calendar life based on the multi-stage calendar life of the target monitoring component.

[1019] In one embodiment of the present disclosure, the monitoring module 130 is also used for: if the nuclear power steam turbine is in the design stage, obtaining the crack propagation life safety monitoring criterion value of the target monitoring component; if the crack propagation calendar life is less than the crack propagation life safety monitoring criterion value, judging that the crack propagation calendar life does not meet the first monitoring qualification condition, so as to perform crack propagation life safety monitoring on the target monitoring component; or, if the crack propagation calendar life is greater than or equal to the crack propagation life safety monitoring criterion value, judging that the crack propagation calendar life meets the first monitoring qualification condition, so as to perform crack propagation life safety monitoring on the target monitoring component.

[1020] In one embodiment of the present disclosure, the monitoring module 130 is also used to: if the crack propagation calendar life does not meet the first monitoring qualification condition, obtain abnormal data of the target monitoring component in the design stage; optimize and improve the abnormal data of the target monitoring component in the design stage, and return to execute the process of obtaining the crack propagation calendar life until the crack propagation calendar life obtained meets the first monitoring qualification condition.

[1021] In one embodiment of the present disclosure, the monitoring module 130 is also used to: if the nuclear power steam turbine is in the manufacturing stage, obtain a safety factor based on the crack propagation calendar life and the crack propagation life safety monitoring criterion value of the target monitoring component; determine whether the safety factor meets the second monitoring qualification condition to perform crack propagation life safety monitoring on the target monitoring component.

[1022] In one embodiment of the present disclosure, the monitoring module 130 is also used to: if the safety factor does not meet the second monitoring qualification condition, obtain abnormal data of the target monitoring component in the manufacturing stage; optimize and improve the abnormal data of the target monitoring component in the manufacturing stage, and return to execute the process of obtaining the safety factor until the obtained safety factor meets the second monitoring qualification condition.

[1023] In one embodiment of the present disclosure, the monitoring module 130 is also used to: if the nuclear power steam turbine is in use, obtain a safety factor based on the crack propagation calendar life and the planned overhaul interval of the nuclear power steam turbine; determine whether the safety factor meets the third monitoring qualification condition to perform crack propagation life safety monitoring on the target monitoring component.

[1024] In one embodiment of the present disclosure, the monitoring module 130 is also used to: if the safety ratio does not meet the third monitoring qualification condition, obtain abnormal data of the target monitoring component during the use phase; optimize and improve the abnormal data of the target monitoring component during the use phase, and return to execute the process of obtaining the safety ratio until the obtained safety ratio meets the third monitoring qualification condition.

[1025] It should be noted that for details not disclosed in the stress corrosion and fatigue long-life monitoring device for the entire life cycle of a nuclear power steam turbine in the embodiment of the present disclosure, please refer to the details disclosed in the stress corrosion and fatigue long-life monitoring method for the entire life cycle of a nuclear power steam turbine in the embodiment of the present disclosure, and they will not be repeated here.

[1026] In summary, the stress corrosion and fatigue long-life monitoring device for the whole life of a nuclear power steam turbine of the disclosed embodiment determines one or more target monitoring components from the components to be monitored, and determines the long-life monitoring data required for the target monitoring components, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life. Based on the long-life monitoring data required by the target monitoring component, the target monitoring component is subjected to crack growth life safety monitoring. Thus, the target monitoring component can be subjected to cra...

Claims

1. A method for monitoring stress corrosion and fatigue of a nuclear power steam turbine during its entire life cycle, characterized in that: include: Determine one or more target monitoring components from the components to be monitored; Determine the long-life monitoring data required for the target monitoring component, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life, wherein the stress corrosion crack growth life is obtained based on the phased array detection crack depth or stress corrosion crack growth size threshold value of the target monitoring component, the annual average stress corrosion crack growth rate test value of the material of the target monitoring component, and the low-cycle fatigue critical crack size of the target monitoring component under the set working condition of the nuclear power steam turbine; Based on the long-life monitoring data required by the target monitoring component, crack propagation life safety monitoring is performed on the target monitoring component.

2. The method according to claim 1, characterized in that The determining of the long-life monitoring data required for the target monitoring component includes: Acquire a mapping relationship between the target monitoring component and the long-life monitoring data; Based on the mapping relationship, the long-life monitoring data required by the target monitoring component is determined.

3. The method according to claim 1, characterized in that: The determining of the long-life monitoring data required for the target monitoring component includes: If the target monitoring component is a rotor blade root slot or a rotor, determining that the long-life monitoring data required for the target monitoring component includes the stress corrosion crack growth life, the low-cycle fatigue crack growth life, and the high-cycle fatigue crack growth life; If the target monitoring component is a cylinder, it is determined that the long-life monitoring data required for the target monitoring component includes the stress corrosion crack growth life and the low cycle fatigue crack growth life.

4. The method according to claim 1, characterized in that: The step of determining one or more target monitoring components from the components to be monitored includes: Obtain crack growth life safety monitoring instructions; Extracting the identification of the target monitoring component from the crack growth life safety monitoring instruction; Based on the identification of the target monitoring component, one or more target monitoring components are determined from the components to be monitored.

5. The method according to claim 1, characterized in that The step of determining one or more target monitoring components from the components to be monitored further includes: Obtain crack extension life safety monitoring instructions sent by the remote client; The component to be monitored associated with the remote client is determined as the target monitoring component.

6. The method according to claim 1, characterized in that The determining of the long-life monitoring data required for the target monitoring component includes: Acquire a set of crack extension sizes of the target monitoring component; Based on the crack growth size set, long-life monitoring data required for the target monitoring component is determined.

7. The method according to claim 6, characterized in that The step of obtaining a set of crack extension sizes of the target monitoring component includes: Acquiring basic data for stress calculation of the target monitoring component; Acquiring basic material test data of the target monitoring component; The crack extension size set is determined based on the stress calculation basic data and the material experiment basic data.

8. The method according to claim 7, characterized in that The step of determining the crack extension size set based on the stress calculation basic data and the material experiment basic data includes: Determine a stress corrosion crack extension size threshold value of the target monitoring component based on the crack shape parameters of the target monitoring component, the stress corrosion fracture toughness of the material of the target monitoring component, and the maximum stress at the crack site of the target monitoring component under the steady-state condition of the nuclear power steam turbine under load operation; Based on the crack shape parameters of the target monitoring component, the fracture toughness of the material of the target monitoring component and the maximum stress at the crack site of the target monitoring component under the set operating condition of the nuclear power turbine, the low-cycle fatigue critical crack size of the target monitoring component under the set operating condition of the nuclear power turbine is determined.

9. The method according to claim 7, characterized in that: The step of determining the crack extension size set based on the stress calculation basic data and the material experiment basic data includes: Determine the high cycle fatigue crack extension size threshold value of the target monitoring component based on the crack shape parameters of the target monitoring component, the test value of the high cycle fatigue crack extension threshold value of the material of the target monitoring component, and the high cycle fatigue stress range of the crack position of the target monitoring component under the steady-state condition of the nuclear power steam turbine under load operation; Based on the crack shape parameters of the target monitored component, the fracture toughness of the material of the target monitored component, and the maximum stress at the crack site of the target monitored component under steady-state conditions of load operation of the nuclear power turbine, the high-cycle fatigue critical crack size of the target monitored component is determined.

10. The method according to claim 8, characterized in that Based on the crack extension size set, obtaining the stress corrosion crack extension life includes: The stress corrosion crack growth life is obtained based on the first parameter of the target monitoring component, the annual average stress corrosion crack growth rate test value of the material of the target monitoring component, and the low cycle fatigue critical crack size of the target monitoring component under the set working condition of the nuclear power steam turbine; wherein, The first parameter is the phased array detection crack depth of the target monitoring component or the stress corrosion crack extension size threshold value.

11. The method according to claim 8, characterized in that The fatigue crack growth life includes a low cycle fatigue crack growth life, and based on the crack growth size set, obtaining the low cycle fatigue crack growth life includes: Based on the second parameter of the target monitoring component, the crack shape parameter of the target monitoring component, the low-cycle fatigue crack growth test constant of the material of the target monitoring component, and the maximum stress at the crack site of the target monitoring component under the set working condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of at least one stage of the set working condition of the nuclear power steam turbine is obtained; wherein, The second parameter is any one parameter of the phased array detection crack depth, initial crack size, and crack extension size set of the target monitoring component.

12. The method according to claim 9, characterized in that The fatigue crack growth life includes a high cycle fatigue crack growth life, and based on the crack growth size set, obtaining the high cycle fatigue crack growth life includes: Based on the third parameter of the target monitoring component, the high cycle fatigue critical crack size, the crack shape parameter of the target monitoring component, the material high cycle fatigue crack growth test constant of the target monitoring component, and the high cycle fatigue stress range of the crack part of the target monitoring component under the steady-state condition of the nuclear power steam turbine under load operation, the high cycle fatigue crack growth life is obtained; wherein, The third parameter is the phased array detection crack depth of the target monitoring component or the high cycle fatigue crack extension size threshold value.

13. The method according to any one of claims 1 to 12, characterized in that The method of performing crack propagation life safety monitoring on the target monitoring component based on the long life monitoring data required by the target monitoring component comprises: Based on the long-life monitoring data required by the target monitoring component, obtaining the crack growth calendar life of the target monitoring component; Based on the crack growth calendar life, the target monitoring component is subjected to crack growth life safety monitoring.

14. The method according to claim 13, characterized in that The step of obtaining the crack growth calendar life of the target monitoring component based on the long-life monitoring data required by the target monitoring component comprises: Based on the long-life monitoring data required by the target monitoring component, obtaining the multi-stage calendar life of the target monitoring component; The crack growth calendar life is obtained based on the multi-stage calendar life of the target monitoring component.

15. The method according to claim 13, characterized in that The step of performing crack growth life safety monitoring on the target monitoring component based on the crack growth calendar life includes: If the nuclear power steam turbine is in the design stage, obtaining a crack growth life safety monitoring criterion value of the target monitoring component; If the crack growth calendar life is less than the crack growth life safety monitoring criterion value, it is determined that the crack growth calendar life does not meet the first monitoring qualification condition, so as to perform crack growth life safety monitoring on the target monitoring component; or, If the crack growth calendar life is greater than or equal to the crack growth life safety monitoring criterion value, it is determined that the crack growth calendar life meets the first monitoring qualification condition, so as to perform crack growth life safety monitoring on the target monitoring component.

16. The method according to claim 15, characterized in that The method further comprises: If the crack growth calendar life does not meet the first monitoring qualification condition, obtaining abnormal data of the target monitoring component in the design stage; The abnormal data of the target monitoring component in the design phase is optimized and improved, and the process of obtaining the crack propagation calendar life is returned to be executed until the obtained crack propagation calendar life meets the first monitoring qualification condition.

17. The method according to claim 13, characterized in that The step of performing crack growth life safety monitoring on the target monitoring component based on the crack growth calendar life includes: If the nuclear power steam turbine is in the manufacturing stage, a safety factor is obtained based on the crack growth calendar life and the crack growth life safety monitoring criterion value of the target monitoring component; It is determined whether the safety factor satisfies a second monitoring qualification condition so as to perform crack propagation life safety monitoring on the target monitoring component.

18. The method according to claim 17, characterized in that The method further comprises: If the safety factor does not meet the second monitoring qualification condition, obtaining abnormal data of the target monitoring component in the manufacturing stage; The abnormal data of the target monitoring component in the manufacturing stage is optimized and improved, and the process of obtaining the safety factor is returned to be executed until the safety factor obtained meets the second monitoring qualification condition.

19. The method according to claim 13, characterized in that The step of performing crack growth life safety monitoring on the target monitoring component based on the crack growth calendar life includes: If the nuclear power steam turbine is in use, a safety multiple is obtained based on the crack growth calendar life and the planned overhaul interval of the nuclear power steam turbine; It is determined whether the safety multiple satisfies a third monitoring qualification condition so as to perform crack propagation life safety monitoring on the target monitoring component.

20. The method according to claim 19, characterized in that The method further comprises: If the safety multiple does not meet the third monitoring qualification condition, obtaining abnormal data of the target monitoring component during the use phase; The abnormal data of the target monitoring component during the use phase is optimized and improved, and the process of obtaining the safety multiple is returned to execute until the obtained safety multiple meets the third monitoring qualification condition.

21. A stress corrosion and fatigue long-life monitoring device for a nuclear power steam turbine during its entire life cycle, characterized in that: include: A first determination module, used to determine one or more target monitoring components from the components to be monitored; A second determination module is used to determine the long-life monitoring data required for the target monitoring component, wherein the long-life monitoring data includes stress corrosion crack growth life and fatigue crack growth life, and the fatigue crack growth life includes at least one of low-cycle fatigue crack growth life and high-cycle fatigue crack growth life, and the stress corrosion crack growth life is obtained based on the phased array detection crack depth or stress corrosion crack growth size threshold value of the target monitoring component, the material annual average stress corrosion crack growth rate test value of the target monitoring component, and the low-cycle fatigue critical crack size of the target monitoring component under the set working condition of the nuclear power steam turbine; A monitoring module is used to perform crack propagation life safety monitoring on the target monitoring component based on the long-life monitoring data required by the target monitoring component.

22. The device according to claim 21, characterized in that The second determining module is further used for: Acquire a mapping relationship between the target monitoring component and the long-life monitoring data; Based on the mapping relationship, the long-life monitoring data required by the target monitoring component is determined.

23. The device according to claim 21, characterized in that The second determining module is further used for: If the target monitoring component is a rotor blade root slot or a rotor, determining that the long-life monitoring data required for the target monitoring component includes the stress corrosion crack growth life, the low-cycle fatigue crack growth life, and the high-cycle fatigue crack growth life; If the target monitoring component is a cylinder, it is determined that the long-life monitoring data required for the target monitoring component includes the stress corrosion crack growth life and the low cycle fatigue crack growth life.

24. The device according to claim 21, characterized in that The first determining module is further used for: Obtain crack growth life safety monitoring instructions; Extracting the identification of the target monitoring component from the crack growth life safety monitoring instruction; Based on the identification of the target monitoring component, one or more target monitoring components are determined from the components to be monitored.

25. The device according to claim 21, characterized in that The first determining module is further used for: Obtain crack extension life safety monitoring instructions sent by the remote client; The component to be monitored associated with the remote client is determined as the target monitoring component.

26. The device according to claim 21, characterized in that The second determining module is further used for: Acquire a set of crack extension sizes of the target monitoring component; Based on the crack growth size set, long-life monitoring data required for the target monitoring component is determined.

27. The device according to claim 26, characterized in that The second determining module is further used for: Acquiring basic data for stress calculation of the target monitoring component; Acquiring basic material test data of the target monitoring component; The crack extension size set is determined based on the stress calculation basic data and the material experiment basic data.

28. The device according to claim 27, characterized in that The second determining module is further used for: Determine a stress corrosion crack extension size threshold value of the target monitoring component based on the crack shape parameters of the target monitoring component, the stress corrosion fracture toughness of the material of the target monitoring component, and the maximum stress at the crack site of the target monitoring component under the steady-state condition of the nuclear power steam turbine under load operation; Based on the crack shape parameters of the target monitoring component, the fracture toughness of the material of the target monitoring component and the maximum stress at the crack site of the target monitoring component under the set operating condition of the nuclear power turbine, the low-cycle fatigue critical crack size of the target monitoring component under the set operating condition of the nuclear power turbine is determined.

29. The device according to claim 27, characterized in that The second determining module is further used for: Determine the high cycle fatigue crack extension size threshold value of the target monitoring component based on the crack shape parameters of the target monitoring component, the test value of the high cycle fatigue crack extension threshold value of the material of the target monitoring component, and the high cycle fatigue stress range of the crack position of the target monitoring component under the steady-state condition of the nuclear power steam turbine under load operation; Based on the crack shape parameters of the target monitored component, the fracture toughness of the material of the target monitored component, and the maximum stress at the crack site of the target monitored component under steady-state conditions of load operation of the nuclear power turbine, the high-cycle fatigue critical crack size of the target monitored component is determined.

30. The device according to claim 28, characterized in that The second determining module is further used for: The stress corrosion crack growth life is obtained based on the first parameter of the target monitoring component, the annual average stress corrosion crack growth rate test value of the material of the target monitoring component, and the low cycle fatigue critical crack size of the target monitoring component under the set working condition of the nuclear power steam turbine; wherein, The first parameter is the phased array detection crack depth of the target monitoring component or the stress corrosion crack extension size threshold value.

31. The device according to claim 28, characterized in that The second determining module is further used for: Based on the second parameter of the target monitoring component, the crack shape parameter of the target monitoring component, the low-cycle fatigue crack growth test constant of the material of the target monitoring component, and the maximum stress at the crack site of the target monitoring component under the set working condition of the nuclear power steam turbine, the low-cycle fatigue crack growth life of at least one stage of the set working condition of the nuclear power steam turbine is obtained; wherein, The second parameter is any one parameter of the phased array detection crack depth, initial crack size, and crack extension size set of the target monitoring component.

32. The device according to claim 29, characterized in that The second determining module is further used for: Based on the third parameter of the target monitoring component, the high cycle fatigue critical crack size, the crack shape parameter of the target monitoring component, the material high cycle fatigue crack growth test constant of the target monitoring component, and the high cycle fatigue stress range of the crack part of the target monitoring component under the steady-state condition of the nuclear power steam turbine under load operation, the high cycle fatigue crack growth life is obtained; wherein, The third parameter is the phased array detection crack depth of the target monitoring component or the high cycle fatigue crack extension size threshold value.

33. The device according to any one of claims 21 to 32, characterized in that The monitoring module is also used for: Based on the long-life monitoring data required by the target monitoring component, obtaining the crack growth calendar life of the target monitoring component; Based on the crack growth calendar life, the target monitoring component is subjected to crack growth life safety monitoring.

34. The device according to claim 33, characterized in that The monitoring module is also used for: Based on the long-life monitoring data required by the target monitoring component, obtaining the multi-stage calendar life of the target monitoring component; The crack growth calendar life is obtained based on the multi-stage calendar life of the target monitoring component.

35. The device according to claim 33, characterized in that The monitoring module is also used for: If the nuclear power steam turbine is in the design stage, obtaining a crack growth life safety monitoring criterion value of the target monitoring component; If the crack growth calendar life is less than the crack growth life safety monitoring criterion value, it is determined that the crack growth calendar life does not meet the first monitoring qualification condition, so as to perform crack growth life safety monitoring on the target monitoring component; or, If the crack growth calendar life is greater than or equal to the crack growth life safety monitoring criterion value, it is determined that the crack growth calendar life meets the first monitoring qualification condition, so as to perform crack growth life safety monitoring on the target monitoring component.

36. The device according to claim 35, characterized in that The monitoring module is also used for: If the crack growth calendar life does not meet the first monitoring qualification condition, obtaining abnormal data of the target monitoring component in the design stage; The abnormal data of the target monitoring component in the design phase is optimized and improved, and the process of obtaining the crack propagation calendar life is returned to be executed until the obtained crack propagation calendar life meets the first monitoring qualification condition.

37. The device according to claim 33, characterized in that The monitoring module is also used for: If the nuclear power steam turbine is in the manufacturing stage, a safety factor is obtained based on the crack growth calendar life and the crack growth life safety monitoring criterion value of the target monitoring component; It is determined whether the safety factor satisfies a second monitoring qualification condition so as to perform crack propagation life safety monitoring on the target monitoring component.

38. The device according to claim 37, characterized in that The monitoring module is also used for: If the safety factor does not meet the second monitoring qualification condition, obtaining abnormal data of the target monitoring component in the manufacturing stage; The abnormal data of the target monitoring component in the manufacturing stage is optimized and improved, and the process of obtaining the safety factor is returned to be executed until the safety factor obtained meets the second monitoring qualification condition.

39. The device according to claim 33, characterized in that The monitoring module is also used for: If the nuclear power steam turbine is in use, a safety multiple is obtained based on the crack growth calendar life and the planned overhaul interval of the nuclear power steam turbine; It is determined whether the safety multiple satisfies a third monitoring qualification condition so as to perform crack propagation life safety monitoring on the target monitoring component.

40. The device according to claim 39, characterized in that The monitoring module is also used for: If the safety multiple does not meet the third monitoring qualification condition, obtaining abnormal data of the target monitoring component during the use phase; The abnormal data of the target monitoring component during the use phase is optimized and improved, and the process of obtaining the safety multiple is returned to execute until the obtained safety multiple meets the third monitoring qualification condition.

41. An electronic device, characterized in that: include: A memory, a processor, and a computer program stored in the memory and executable on the processor, wherein when the processor executes the program, a method for monitoring stress corrosion and fatigue long life of a nuclear power steam turbine throughout its life cycle is implemented as described in any one of claims 1 to 20.

42. The electronic device according to claim 41, characterized in that Also includes: A wireless communication component is connected to the nuclear power steam turbine, and data is transmitted between the electronic device and the nuclear power steam turbine via the wireless communication component.

43. The electronic device according to claim 41, characterized in that The memory is used to store the long-life monitoring data required by the monitoring components of the nuclear power steam turbine; The processor is used to obtain a crack propagation life safety monitoring instruction, obtain long-life monitoring data required by a target monitoring component of the nuclear power steam turbine to be monitored from the memory based on the crack propagation life safety monitoring instruction, and perform crack propagation life safety monitoring on the target monitoring component based on the long-life monitoring data required by the target monitoring component.

44. The electronic device according to claim 43, characterized in that Also includes: a remote client, the remote client being connected to the processor; The remote client is used to send the crack extension life safety monitoring instruction to the processor and receive the monitoring result fed back by the processor.

45. The electronic device according to claim 44, characterized in that The remote client is also used to obtain control information of a user who controls the remote client, and generate the crack extension life safety monitoring instruction based on the control information.

46. ​​The electronic device according to claim 44, characterized in that The processor is also used to determine the monitoring component of the nuclear power steam turbine associated with the remote client as the target monitoring component.

47. A computer-readable storage medium having a computer program stored thereon, characterized in that: When the program is executed by a processor, the method for monitoring stress corrosion and fatigue long life of a nuclear power steam turbine throughout its entire life cycle as described in any one of claims 1 to 20 is implemented.

48. A monitoring platform suitable for nuclear power steam turbines, characterized in that: include: The stress corrosion and fatigue long-life monitoring device for a nuclear power steam turbine throughout its life cycle as claimed in any one of claims 21 to 40; Or an electronic device as described in any one of claims 41-46; or a computer-readable storage medium as described in claim 47.

Citation Information

Patent Citations

  • Monitoring method of crack propagation life of low-cycle fatigue and high-cycle fatigue of steam turbine rotor

    CN104481601A

  • Method for designing and monitoring service life of steam turbine rotor under action low-cycle and high-cycle fatigue

    CN112668111A

  • Rotor outer surface manufacturing defect monitoring method, device, equipment, system and medium

    CN112748124A

  • Method and system for predicting creep-fatigue life of steam turbine rotor

    CN113722946A

  • Joint monitoring platform of nuclear turbine

    CN114398751A