A halide solid electrolyte and a battery using the same
By using a halide solid electrolyte with a specific chemical composition and structure, combined with a high-energy ball mill grinding process, the problems of low ionic conductivity and complex preparation of solid electrolyte materials are solved, and high ionic conductivity and high voltage stability are achieved, which is suitable for battery applications. Large-scale production.
Patent Information
- Application Number
- CN202310779841.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-06-28
AI Technical Summary
Existing solid electrolyte materials, especially polymer and oxide electrolytes, have low ionic conductivity, resulting in high battery interface impedance, making it difficult to apply on a large scale, and the preparation process is complex to meet high environmental and equipment requirements.
A halide solid electrolyte with a chemical composition of (2+n)LiCl·(1-n)ZrCl4·nM is used, in which M contains Fe element. The characteristic diffraction peak intensity ratio of the X-ray diffraction pattern conforms to I2/I1=0.45~3. The structure of I2/I3=0.6~2.6, combined with the high-energy ball mill grinding process, simplifies the preparation process.
It significantly improves the ionic conductivity and high voltage stability of the solid electrolyte, simplifies the preparation process, and is suitable for large-scale production.
Smart Images

Figure CN116779952B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrolyte materials, and specifically relates to a halide solid electrolyte and a battery using the same. Background Art
[0002] Compared with traditional liquid lithium-ion batteries, solid-state lithium-ion batteries have the advantages of high energy density, small volume, high safety, and flexibility and deformability, so they have attracted much attention. Solid electrolytes are the core components of solid-state batteries. They replace the separator and electrolyte in liquid lithium-ion batteries and play the role of transmitting lithium ions while isolating the positive and negative electrodes.
[0003] Currently, the commonly used solid electrolytes are mainly divided into polymer electrolytes, sulfide electrolytes, and oxide electrolytes. Polymer solid electrolytes are currently the mainstream choice of solid electrolytes. However, they have the technical problem of low ionic conductivity. Oxide solid electrolytes also have the problem of low ionic conductivity. The high Young's modulus of the particles of this type of solid electrolyte leads to a large final battery interface impedance, making it difficult to be applied on a large scale. Compared with general liquid electrolytes, the ionic conductivities of the above two types of solid electrolytes are significantly lower. Among the above three mainstream solid electrolytes, sulfide is the only solid electrolyte material that is close to or even exceeds liquid electrolytes. However, the preparation of this type of solid electrolyte is complex, and the production process, environment, and equipment for preparing this type of solid electrolyte all require high requirements. Summary of the Invention
[0004] In order to improve the ionic conductivity of solid electrolytes, the present invention provides a halide solid electrolyte and a battery using the same.
[0005] According to one aspect of the present invention, a halide solid electrolyte is provided: the chemical composition of the halide solid electrolyte satisfies the general formula (2 + n)LiCl·(1 - n)ZrCl4·nM. In the general formula, the chemical composition of M contains Fe element, and the value of n satisfies 0 < n < 1; in the X-ray diffraction pattern of the halide solid electrolyte: the diffraction intensity corresponding to 2Θ = 30° is used as the first characteristic diffraction peak intensity, denoted as I1; the diffraction intensity corresponding to 2Θ = 32.8° is used as the second characteristic diffraction peak intensity, denoted as I2; the diffraction intensity corresponding to 2Θ = 34° is used as the third characteristic diffraction peak intensity, denoted as I3; the structure of the halide solid electrolyte satisfies I2 / I1 = 0.45 - 3, and I2 / I3 = 0.6 - 2.6. The above-mentioned halide solid electrolyte provided by the present invention has excellent ionic conductivity and high high-voltage stability. Brief Description of the Drawings
[0006] Figure 1 XRD pattern of the all-solid electrolyte prepared in Example 2;
[0007] Figure 2 XRD pattern of the all-solid-state electrolyte prepared in Comparative Example 3. Detailed implementation manners
[0008] According to one aspect of the present invention, a halide solid electrolyte is provided: the chemical composition of the halide solid electrolyte satisfies the general formula (2 + n)LiCl·(1 - n)ZrCl4·nM, in the general formula, the chemical composition of M contains Fe element, and the value of n satisfies 0 < n < 1; in the X-ray diffraction pattern of the halide solid electrolyte: the diffraction intensity corresponding to 2Θ = 30° is used as the first characteristic diffraction peak intensity, denoted as I1; the diffraction intensity corresponding to 2Θ = 32.8° is used as the second characteristic diffraction peak intensity, denoted as I2; the diffraction intensity corresponding to 2Θ = 34° is used as the third characteristic diffraction peak intensity, denoted as I3; the structure of the halide solid electrolyte satisfies that I2 / I1 = 0.45 to 3, and I2 / I3 = 0.6 to 2.6. The above-mentioned halide solid electrolyte provided by the present invention has excellent ionic conductivity and high high-voltage stability.
[0009] Preferably, in the general formula, the value of n satisfies that the equivalent ratio of each element in the halide solid electrolyte reaches Li element: Zr element: Fe element = 2.1 to 2.25: 0.75 to 0.9: 0.1 to 0.25.
[0010] Preferably, in the general formula, the value of n satisfies that the equivalent ratio of each element in the halide solid electrolyte reaches Li element: Zr element: Fe element = 2.15: 0.85: 0.15.
[0011] Preferably, in the general formula, the chemical composition of M includes a halide containing iron element.
[0012] Preferably, in the general formula, the chemical composition of M includes at least one of FeCl2 and FeCl3.
[0013] Preferably, the particle size D of the halide solid electrolyte 50 is 1 to 5 μm.
[0014] Preferably, the preparation method of the halide solid electrolyte includes the following operations: material preparation step: weigh LiCl, ZrCl4 and the iron source material for providing M in the general formula according to the chemical composition of the halide solid electrolyte; prepare the first precursor: mix LiCl and ZrCl4, and the mixture obtained is the first precursor; prepare the second precursor: mix the iron source material and the first precursor, and the mixture obtained is the second precursor; prepare the halide solid electrolyte: grind the second precursor using a high-energy ball mill, the ball-to-material ratio is 20 to 50:1, the ball milling speed is 500 to 800 rpm, the ball milling time is not less than 10 hours, and the halide solid electrolyte is obtained after the ball milling. The above-mentioned high ionic conductivity solid electrolyte material involved in the present invention can be prepared by a simple ball milling process, without cumbersome synthesis operations and harsh reaction conditions, which is conducive to subsequent large-scale production.
[0015] Preferably, the specific operation of preparing the first precursor includes: mixing LiCl and ZrCl4, and then stirring and dispersing the mixture formed thereby, with a stirring speed of 3000 to 30000 rpm and a stirring time of not less than 0.5 hour, thereby obtaining the first precursor.
[0016] Preferably, the specific operation of preparing the second precursor includes: mixing the iron source material and the first precursor, and then stirring and dispersing the resulting mixture at a stirring speed of 3000 to 35000 rpm for a stirring time of not less than 0.5 hour, thereby obtaining the second precursor.
[0017] Preferably, the ion conductivity of the halide solid electrolyte is 0.01 to 1.5 mS / cm.
[0018] According to a second aspect of the present invention, a battery is provided, comprising the halide solid electrolyte as described above. Based on the excellent ionic conductivity and high high voltage stability of the halide solid electrolyte, the battery has good compatibility with high voltage positive electrode materials and exhibits excellent electrical performance.
[0019] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.
[0020] Example 1
[0021] In this embodiment, the 2.1LiCl·0.9ZrCl4·0.1FeCl3 all-solid electrolyte was prepared according to the following steps.
[0022] S1. Preparation: Weigh 1.1305 g of LiCl powder, 2.6635 g of ZrCl4 powder and 0.206 g of FeCl3 powder.
[0023] S2. Preparation of the first precursor: First, LiCl powder and ZrCl4 powder are premixed using a mechanical pulverizer. During the premixing process, the speed of the mechanical pulverizer is 3000 rpm and the premixing time is 30 minutes. The resulting mixture is used as the first precursor.
[0024] S3. Prepare the second precursor: Then add FeCl3 powder to the above-mentioned first precursor and premix it using a mechanical pulverizer. During the premixing process, the speed of the mechanical pulverizer is 30000 rpm and the premixing time is 30 minutes. The resulting mixture is used as the second precursor.
[0025] S4. Preparation of halide solid electrolyte: The second precursor is ground by a high-energy ball mill to further crush and mix the second precursor. During the grinding process, the ball-to-material ratio of the high-energy ball mill is 20:1, the ball milling speed is 500 rpm, and the ball milling time is 10 hours to obtain a halide solid electrolyte. The powder product after ball milling contains a fully solid electrolyte with a chemical composition of 2.1LiCl·0.9ZrCl4·0.1FeCl3.
[0026] Example 2
[0027] This embodiment uses the method for preparing an all-solid electrolyte in accordance with Embodiment 1 to prepare a 2.15LiCl·0.85ZrCl4·0.15FeCl3 all-solid electrolyte. The difference from Embodiment 1 is that in this embodiment, the amount of each raw material is 2.3254g of LiCl powder, 5.0538g of ZrCl4 powder, and 0.6208g of FeCl3 powder. In addition to the above differences, the other operations for preparing an all-solid electrolyte in this embodiment are strictly consistent with those in Embodiment 1, thereby obtaining an all-solid electrolyte with a chemical composition of 2.15LiCl·0.85ZrCl4·0.15FeCl3.
[0028] Example 3
[0029] This embodiment refers to the method for preparing an all-solid electrolyte in Example 1 to complete the preparation of a 2.25LiCl·0.75ZrCl4·0.25FeCl3 all-solid electrolyte. The difference from Example 1 is that in this embodiment, the amount of each raw material is 1.228g of LiCl powder, 2.25g of ZrCl4 powder and 0.522g of FeCl3 powder. Except for the above differences, the other operations for preparing the all-solid electrolyte in this embodiment are strictly consistent with those in Example 1, thereby obtaining an all-solid electrolyte with a chemical composition of 2.25LiCl·0.75ZrCl4·0.25FeCl3.
[0030] Example 4
[0031] This embodiment uses the method for preparing an all-solid electrolyte in accordance with Embodiment 1 to prepare a 2.5LiCl·0.5ZrCl4·0.5FeCl3 all-solid electrolyte. The difference from Embodiment 1 is that in this embodiment, the amount of each raw material is 1.364g of LiCl powder, 1.496g of ZrCl4 powder, and 1.043g of FeCl3 powder. In addition to the above differences, the other operations for preparing an all-solid electrolyte in this embodiment are strictly consistent with those in Embodiment 1, thereby obtaining an all-solid electrolyte with a chemical composition of 2.5LiCl·0.5ZrCl4·0.5FeCl3.
[0032] Example 5
[0033] This embodiment uses the method for preparing an all-solid electrolyte in accordance with Embodiment 1 to prepare a 2.9LiCl·0.1ZrCl4·0.9FeCl3 all-solid electrolyte. The difference from Embodiment 1 is that in this embodiment, the amount of each raw material is 1.583g of LiCl powder, 0.299g of ZrCl4 powder, and 1.878g of FeCl3 powder. Except for the above differences, the other operations for preparing an all-solid electrolyte in this embodiment are strictly consistent with those in Embodiment 1, thereby obtaining an all-solid electrolyte with a chemical composition of 2.9LiCl·0.1ZrCl4·0.9FeCl3.
[0034] Example 6
[0035] In this embodiment, the 2.15LiCl·0.85ZrCl4·0.15FeCl2 all-solid electrolyte was prepared according to the following steps.
[0036] S1. Preparation: Weigh 2.3254 g of LiCl powder, 5.0538 g of ZrCl4 powder and 0.4852 g of FeCl2 powder.
[0037] S2. Preparation of the first precursor: First, LiCl powder and ZrCl4 powder are premixed using a mechanical pulverizer. During the premixing process, the speed of the mechanical pulverizer is 3000 rpm, and the premixing time is 1 hour. The resulting mixture is used as the first precursor.
[0038] S3. Prepare the second precursor: Then add FeCl2 powder to the above-mentioned first precursor and use a mechanical pulverizer for premixing. During the premixing process, the speed of the mechanical pulverizer is 35000 rpm and the premixing time is 2 hours. The resulting mixture is used as the second precursor.
[0039] S4. Preparation of halide solid electrolyte: The second precursor is ground by a high-energy ball mill to further crush and mix the second precursor. During the grinding process, the ball-to-material ratio of the high-energy ball mill is 50:1, the ball milling speed is 800 rpm, and the ball milling time is 24 hours. The powder product after the ball milling contains a halide solid electrolyte with a chemical composition of 2.15LiCl·0.85ZrCl4·0.15FeCl2.
[0040] Example 7
[0041] In this embodiment, the 2.15LiCl·0.85ZrCl4·0.15FeBr3 all-solid electrolyte was prepared according to the following steps.
[0042] S1. Preparation: Weigh 2.3254 g of LiCl powder, 5.0538 g of ZrCl4 powder and 1.1308 g of FeBr3 powder.
[0043] S2. Preparation of the first precursor: First, LiCl powder and ZrCl4 powder are premixed using a mechanical pulverizer. During the premixing process, the speed of the mechanical pulverizer is 1000 rpm and the premixing time is 15 minutes. The resulting mixture is used as the first precursor.
[0044] S3. Prepare the second precursor: Then add FeBr3 powder to the above-mentioned first precursor and use a mechanical pulverizer for premixing. During the premixing process, the speed of the mechanical pulverizer is 20000 rpm and the premixing time is 15 minutes. The resulting mixture is used as the second precursor.
[0045] S4. Preparation of halide solid electrolyte: The second precursor is ground by a high-energy ball mill to further crush and mix the second precursor. During the grinding process, the ball-to-material ratio of the high-energy ball mill is 50:1, the ball milling speed is 800 rpm, and the ball milling time is 24 hours. The powder product after the ball milling contains a halide solid electrolyte with a chemical composition of 2.15LiCl·0.85ZrCl4·0.15FeBr3.
[0046] Example 8
[0047] In this embodiment, the 2.15LiCl·0.85ZrCl4·0.15Fe2(SO4)3 all-solid electrolyte is prepared according to the following steps.
[0048] S1. Preparation: Weigh 2.3254 g of LiCl powder, 5.0538 g of ZrCl4 powder and 1.5281 g of Fe2(SO4)3 powder.
[0049] S2. Preparation of the first precursor: First, LiCl powder and ZrCl4 powder are premixed using a mechanical pulverizer. During the premixing process, the speed of the mechanical pulverizer is 4000 rpm, and the premixing time is 45 minutes. The resulting mixture is used as the first precursor.
[0050] S3. Prepare the second precursor: Then add Fe2(SO4)3 powder to the above-mentioned first precursor and use a mechanical pulverizer for premixing. During the premixing process, the speed of the mechanical pulverizer is 38000 rpm and the premixing time is 45 minutes. The resulting mixture is used as the second precursor.
[0051] S4. Preparation of halide solid electrolyte: The second precursor is ground using a high-energy ball mill to further crush and mix the second precursor. During the grinding process, the ball-to-material ratio of the high-energy ball mill is 50:1, the ball milling speed is 800 rpm, and the ball milling time is 24 hours. The powder product after the ball milling contains a halide solid electrolyte with a chemical composition of 2.15LiCl·0.85ZrCl4·0.15Fe2(SO4)3.
[0052] Comparative Example 1
[0053] This comparative example refers to the method for preparing a solid-state electrolyte in Example 2 to complete the preparation of a 2LiCl·ZrCl4 solid-state electrolyte. The difference from Example 2 is that this comparative example does not use FeCl3 to prepare a solid-state electrolyte. In this comparative example, the amount of each raw material is 2.1632g of LiCl powder and 5.9456g of ZrCl4 powder. Accordingly, the step of adding FeCl3 and the step of ball milling are omitted in the process of preparing the solid-state electrolyte. In addition to the above differences, the other operations used in this comparative example to prepare the solid-state electrolyte are strictly consistent with those in Example 2.
[0054] The specific steps for preparing 2LiCl·ZrCl4 all-solid electrolyte in this comparative example are as follows:
[0055] S1. Preparation: Weigh 2.1632 g of LiCl powder and 5.9456 g of ZrCl4 powder.
[0056] S2. Preparation of the first precursor: First, LiCl powder and ZrCl4 powder are premixed using a mechanical pulverizer. During the premixing process, the speed of the mechanical pulverizer is 3000 rpm, and the premixing time is 0.5 hour. The resulting mixture is used as the first precursor.
[0057] S3. Preparation of halide solid electrolyte: The first precursor is ground by a high-energy ball mill to further crush and mix the first precursor. During the grinding process, the ball-to-material ratio of the high-energy ball mill is 20:1, the ball milling speed is 500 rpm, and the ball milling time is 10 hours to obtain a halide solid electrolyte. The powder product after the ball milling contains a fully solid electrolyte with a chemical composition of 2LiCl·ZrCl4.
[0058] Comparative Example 2
[0059] This comparative example completes the preparation of the all-solid electrolyte with reference to the method for preparing the all-solid electrolyte in Example 2. The difference from Example 2 is that in the premixing process of preparing S2 for the all-solid electrolyte, the speed of the mechanical pulverizer is adjusted to 800 rpm, and the premixing time is adjusted to 15 minutes; in the premixing process of preparing S3 for the all-solid electrolyte, the speed of the mechanical pulverizer is adjusted to 18000 rpm, and the premixing time is adjusted to 15 minutes. In addition to the above differences, the other operations used in this comparative example to prepare the all-solid electrolyte are strictly consistent with Example 2.
[0060] Comparative Example 3
[0061] This comparative example prepares the all-solid electrolyte with reference to the method for preparing the all-solid electrolyte in Example 2. The difference from Example 2 is that the steps of preparing the first precursor and the second precursor are omitted, and the LiCl powder, ZrCl4 powder and FeCl3 powder are directly put into a high-energy ball mill for mixing. Except for the above differences, the other operations for preparing the all-solid electrolyte in this comparative example are strictly consistent with those in Example 2.
[0062] The specific steps for preparing the all-solid electrolyte in this comparative example are as follows:
[0063] S1. Preparation: Weigh 1.1305 g of LiCl powder, 2.6635 g of ZrCl4 powder and 0.206 g of FeCl3 powder.
[0064] S2. Mix LiCl powder, ZrCl4 powder and FeCl3 powder and add them into a high-energy ball mill, grind the above materials, crush and mix the above materials. During the grinding process, the ball-to-material ratio of the high-energy ball mill is 20:1, the ball milling speed is 500 rpm, and the ball milling time is 10 hours to obtain a halide solid electrolyte. The powder product after the ball milling contains a fully solid electrolyte.
[0065] Test Case
[0066] 1. Test subjects
[0067] The all-solid electrolytes provided in Examples 1 to 8 and Comparative Examples 1 to 3.
[0068] 2. Test items
[0069] (1) XRD spectrum test method
[0070] A D / Max 2500 x-ray instrument was used, a Cu target was used as a radiation source, a scanning speed of 6° / min, a tube current of 100 mA, a tube voltage of 40 kV, and a scanning angle of 10° to 80°. XRD tests were performed on the all-solid electrolytes provided in Examples 1 to 8 and Comparative Examples 1 to 3, respectively. In the measured spectra: the diffraction peak at 2θ=30° was taken as the first characteristic diffraction peak, and the intensity of the first characteristic diffraction peak was read, marked as I1; the diffraction peak at 2θ=32.8° was taken as the second characteristic diffraction peak, and the intensity of the second characteristic diffraction peak was read, marked as I2; the diffraction peak at 2θ=34° was taken as the third characteristic diffraction peak, and the intensity of the third characteristic diffraction peak was read, marked as I3.
[0071] (2) Ionic conductivity of all-solid-state electrolytes
[0072] 200 mg of all-solid electrolyte was pressed into a small disc sample with a diameter of 13 mm. The upper and lower surfaces of the all-solid electrolyte disc were gold-sprayed and assembled into a button battery. The test was carried out at a temperature of 25 and a test frequency of 0.1 to 1 MHz. The conductivity was calculated using the formula: L / (R*A), where A represents the sample area, L represents the sample thickness, and R represents the resistance.
[0073] 3. Test results
[0074] The raw materials used to prepare the solid electrolytes in Examples 1 to 8 and Comparative Examples 2 to 3 all include LiCl, ZrCl4 and iron salts. In the all-solid electrolytes prepared in the above Examples and Comparative Examples, the XRD spectra of the test objects provided in Examples 1 to 8 respectively show obvious characteristic diffraction peaks at 2θ=32.8°. For example, the XRD spectra of the all-solid electrolyte provided in Example 2 are as follows: Figure 1 As shown, the XRD patterns of the all-solid electrolytes provided in Examples 1, 3 to 8 are Figure 1The results show that the XRD patterns of the test objects provided in Comparative Example 2 have similar characteristics; although a certain diffraction intensity is also measured at 2θ=32.8° in the XRD pattern of the test object provided in Comparative Example 2, the diffraction intensity at 2θ=32.8° in the XRD pattern of the test object provided in Comparative Example 2 is significantly lower than that of the XRD patterns of the test objects provided in Examples 1 to 8; and no characteristic diffraction peak that can be clearly distinguished from the baseline appears at 2θ=32.8° in the XRD pattern of the test object provided in Comparative Example 3. In the process of preparing the all-solid electrolyte in Examples 1 to 8, the raw materials are ground step by step to promote the good compounding of different salts in the raw materials, and the XRD patterns corresponding to the products thus formed all show characteristic absorption peaks with peaks located near 2θ=32.8°, while in Comparative Examples 2 and 3, due to insufficient grinding of the raw materials, after completing all operations in the preparation process, the composite effect of different salts provided by the raw materials is not good, which is manifested as the XRD patterns corresponding to the products thus formed, which are located near 2θ=32.8°, and the characteristic diffraction peaks are low or do not appear. In general, the XRD pattern characteristics of the all-solid electrolytes provided by Examples 1 to 8 simultaneously meet the characteristics of I2 / I1=0.45~3 and I2 / I3=0.6~2.6, but the XRD patterns corresponding to the all-solid electrolytes provided by Comparative Examples 2 and 3 cannot simultaneously meet the above characteristics. The ionic conductivity test results of the all-solid electrolytes of the above-mentioned embodiments and comparative examples are further compared. As shown in Table 2, the ionic conductivity measured by the test objects provided by Examples 1 to 8 is significantly higher than the ionic conductivity measured by the test objects provided by Comparative Examples 2 to 3. Although the XRD spectrum corresponding to the all-solid electrolyte prepared in Comparative Example 1 can also simultaneously meet the characteristics of I2 / I1=0.45-3 and I2 / I3=0.6-2.6, however, the raw materials included in the preparation of the all-solid electrolyte in Comparative Example 1 do not include iron salts. Therefore, even if its corresponding XRD spectrum has similar structural characteristics to the XRD spectrum corresponding to the all-solid electrolytes prepared in Examples 1 to 8, the all-solid electrolyte of Comparative Example 1 still presents a significant disadvantage in the comparison of the ionic conductivity test results.
[0075] In Examples 1 to 8, the main difference between Example 1, Example 6, Example 7, and Example 8 in the process of preparing the all-solid-state electrolyte is that the types of iron source materials used in the raw materials are different. By comparison, the all-solid-state electrolytes prepared using different iron source materials show certain differences in ionic conductivity. In the above embodiments, the all-solid-state electrolyte prepared using FeCl3 as the iron source material in the raw material has the highest ionic conductivity.
[0076] While Examples 1 to 5 use the same types of raw materials for preparing all-solid-state electrolytes, the main difference lies in the ratio of each material (reflected in the change of n value). As the proportion of iron source materials in the raw materials increases, the corresponding measured ionic conductivity of the prepared all-solid-state electrolyte shows a trend of first increasing and then decreasing. In these examples, the all-solid-state electrolyte prepared in Example 2 has the highest ionic conductivity.
[0077] Table 1. Structural composition of the test objects
[0078] Group <![CDATA[I2 / I1]]> <![CDATA[I2 / I3]]> n value Types of M Example 1 0.47 0.64 0.1 <![CDATA[FeCl3]]> Example 2 1.63 1.70 0.15 <![CDATA[FeCl3]]> Example 3 2.76 2.87 0.25 <![CDATA[FeCl3]]> Example 4 2.45 1.82 0.5 <![CDATA[FeCl3 <!-- 6 -->]]> Example 5 2.97 2.51 0.9 <![CDATA[FeCl3]]> Example 6 1.12 0.98 0.15 <![CDATA[FeCl2]]> Example 7 2.34 2.49 0.15 <![CDATA[FeBr3]]> Example 8 2.28 2.31 0.15 <![CDATA[Fe2(SO4)3]]> Comparative Example 1 1.73 1.45 - - Comparative Example 2 3.05 2.64 0.15 <![CDATA[FeCl3]]> Comparative Example 3 0.12 0.19 0.15 <![CDATA[FeCl3]]> LiCl none none - - <![CDATA[ZrCl4]]> none none - - <![CDATA[FeCl3]]> none none - - <![CDATA[FeCl2]]> none none - - <![CDATA[FeBr3]]> none none - - <![CDATA[Fe2(SO4)3]]> none none - -
[0079] Table 2. Performance of the test objects
[0080]
[0081]
[0082] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.
Claims
1. A halide solid electrolyte, Features: The chemical composition of the halide solid electrolyte satisfies the general formula (2+n)LiCl·(1-n)ZrCl 4 nM, in the general formula, the chemical composition of M contains Fe element, and the value of n satisfies 0 <n<1; In the X-ray diffraction spectrum of the halide solid electrolyte: the diffraction intensity corresponding to 2θ=30° is taken as the first characteristic diffraction peak intensity, marked as I 1 ; The diffraction intensity corresponding to 2θ = 32.8° is taken as the second characteristic diffraction peak intensity, marked as I 2 ; The diffraction intensity corresponding to 2θ = 34° is taken as the third characteristic diffraction peak intensity, marked as I 3 ; The structure of the halide solid electrolyte satisfies: 2 / I 1 =0.45~3, and, I 2 / I 3 =0.6~2.
6.
2. The halide solid electrolyte according to claim 1, Features: In the general formula, the value of n satisfies the requirement that the equivalent ratio of each element in the halide solid electrolyte reaches Li element: Zr element: Fe element = 2.1-2.25: 0.75-0.9: 0.1-0.
25.
3. The halide solid electrolyte according to claim 2, Features: In the general formula, the value of n satisfies the requirement that the equivalent ratio of each element in the halide solid electrolyte reaches Li element: Zr element: Fe element=2.15:0.85:0.
15.
4. The halide solid electrolyte according to claim 1, Features: In the general formula, the chemical composition of M includes a halide containing an iron element.
5. The halide solid electrolyte according to claim 4, Features: In the general formula, the chemical composition of M includes FeCl 2 、FeCl 3 At least one of .
6. The halide solid electrolyte according to claim 1, Features: The particle size D of the halide solid electrolyte 50 1~5μm.
7. The halide solid electrolyte according to claim 1, It is characterized in that The preparation method of the halide solid electrolyte comprises the following operations: Preparation steps: weigh LiCl, ZrCl according to the chemical composition of the halide solid electrolyte 4 and an iron source material for providing M in the general formula; Prepare the first precursor: LiCl and ZrCl 4 Mixing, the resulting mixture is the first precursor; Preparing a second precursor: mixing the iron source material and the first precursor, and the resulting mixture is the second precursor; Preparation of the halide solid electrolyte: grinding the second precursor using a high-energy ball mill, with a ball-to-material ratio of 20 to 50:1, a ball milling speed of 500 to 800 rpm, and a ball milling time of not less than 10 hours, to obtain the halide solid electrolyte after the ball milling is completed.
8. The halide solid electrolyte according to claim 7, It is characterized in that The specific operation of preparing the first precursor includes: LiCl and ZrCl 4 The mixture is then stirred and dispersed at a stirring speed of 3000 to 30000 rpm for a stirring time of not less than 0.5 hour, thereby obtaining the first precursor.
9. The halide solid electrolyte according to claim 7, It is characterized in that The specific operation of preparing the second precursor includes: mixing the iron source material and the first precursor, and then stirring and dispersing the resulting mixture at a stirring speed of 3000 to 35000 rpm for a stirring time of not less than 0.5 hours, thereby obtaining the second precursor.
10. The halide solid electrolyte according to any one of claims 1 to 9, Features: The ion conductivity of the halide solid electrolyte is 0.01 to 1.5 mS / cm.
11. A battery, Features: It comprises the halide solid electrolyte as claimed in any one of claims 1 to 10.
