Composite solid electrolyte and preparation method therefor, and lithium metal battery
By using composite solid electrolytes in lithium metal batteries, combined with polyvinylidene fluoride, lithium salts, organic solvents and complexing agents, the problems of interfacial side reactions and short cycle life of liquid electrolytes in lithium metal batteries are solved, achieving higher The ionic conductivity and interface stability extend the service life of the battery.
Patent Information
- Application Number
- PCT/CN2023/125094
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-10-18
- Publication Date
- 2024-10-03
AI Technical Summary
The liquid electrolyte of existing lithium metal batteries has serious interface side reactions and short cycle life, leading to problems such as lithium dendrite growth, internal short circuits and thermal runaway of the battery, and the ion transport capacity of PVDF-based solid electrolytes under high-voltage cathode materials such as NCM811 insufficient.
A composite solid electrolyte is used, including polyvinylidene fluoride, lithium salt, organic solvent and complexing agent. The lithium ion coordination ability of the complexing agent is weaker than that of the organic solvent. The solvation structure is controlled through the combination of the complexing agent and the organic solvent to improve the Lithium ion conductivity and interface stability, using fast ion conductors to further improve conductivity.
It significantly improves the ion conductivity and interface stability of lithium metal batteries, extends the cycle life of the battery, enhances the ability to operate at high rates, and reduces capacity fading.
Smart Images

Figure CN2023125094_03102024_PF_FP_ABST
Abstract
Description
Composite solid electrolyte, preparation method thereof and lithium metal battery Technical Field
[0001] The present application relates to the technical field of lithium metal batteries, and in particular to a composite solid electrolyte, a preparation method thereof, and a lithium metal battery. Background Art
[0002] At present, lithium metal batteries (LMBs) have the advantages of high energy density and long cycle life and are widely used in many fields. In order to meet the development needs of new energy industries such as portable electronic products and electric vehicles (EVs), lithium metal batteries (LMBs) are developing towards high energy density, long cycle life and high safety. The theoretical capacity of lithium metal is as high as 3860mA hg –1 , is considered to be one of the most promising negative electrode materials for achieving high energy density, with a theoretical capacity of NCM811 exceeding 200 mA h g –1 , is considered one of the most promising cathode materials for achieving high energy density. However, liquid lithium metal batteries formed by the assembly of lithium metal and NCM811 have many disadvantages such as severe interfacial side reactions and short cycle life, which limit their practical application. For example, lithium dendrite growth leads to internal short circuits, thermal runaway, and even explosion in the battery, and severe interfacial side reactions lead to rapid capacity decay. Solid-state lithium metal batteries (ASSLBs) with high energy density and safety are the most promising alternatives to liquid lithium metal batteries.
[0003] Solid polymer electrolytes (SPEs) have the advantages of high elasticity and plasticity, good electrode affinity, and easy preparation. They are one of the most studied solid electrolytes. However, there are still many problems that limit their practical use. For example, polymers such as polyethylene oxide (PEO) cannot promote the dissociation of ion pairs, and their high crystallinity leads to low room temperature ionic conductivity, which cannot meet the needs of daily use. At the same time, PEO has a low oxidation resistance window and cannot match high-voltage positive electrodes represented by NCM811. Compared with PEO-based electrolytes, solid electrolytes based on polyvinylidene fluoride (PVDF) have higher oxidation resistance and thermal stability, which gives them broader application prospects. However, pure PVDF is a good insulator, and lithium ions cannot be transported in pure, solvent-free PVDF-based membranes. By adding the organic solvent N,N-dimethylformamide (DMF) to PVDF, the ionic conductivity of PVDF solid electrolytes can be improved, and matching full batteries can show better electrochemical performance. However, due to the instability of DMF, the solid electrolyte causes the capacity of the lithium metal battery to seriously decay during the continuous reaction on the electrode surface, which cannot meet the ion transport capacity required for high-rate operation of the lithium metal battery.
[0004] Summary of the Invention
[0005] In view of this, the present application provides a composite solid electrolyte, a preparation method thereof, and a lithium metal battery.
[0006] To achieve the above-mentioned objectives, the present application provides a composite solid electrolyte comprising polyvinylidene fluoride, a lithium salt, an organic solvent and a ligand, wherein the ligand has a weaker coordination ability with the lithium ions in the lithium salt than the coordination ability of the organic solvent with the lithium ions, and the ligand comprises at least one of trifluoroacetamide, N-methyltrifluoroacetamide or N,N-dimethyltrifluoroacetamide.
[0007] In some possible implementations, the organic solvent includes one of N,N-dimethylformamide, acetamide, or dimethyl sulfoxide.
[0008] In some possible implementations, the composite solid electrolyte further includes a fast ion conductor, and the fast ion conductor includes Li 1.4 Al 0.4 Ti 1.6 (PO4)3、Li7La3Zr2O 12 or Li 0.34 La 0.5 1TiO 2.94 One of them.
[0009] In some possible implementations, the molar ratio of the organic solvent to the complexing agent is 5:(1-5).
[0010] The present application also provides a method for preparing a composite solid electrolyte, which comprises: mixing polyvinylidene fluoride and a lithium salt, and dissolving the mixture in an organic solvent to obtain a first solution; adding a ligand to the first solution, stirring the mixture evenly, and obtaining a second solution, wherein the ligand has a weaker coordination ability with the lithium ions in the lithium salt than the coordination ability of the organic solvent with the lithium ions, and the ligand comprises at least one of trifluoroacetamide, N-methyltrifluoroacetamide, or N,N-dimethyltrifluoroacetamide; and drying the second solution to obtain a composite solid electrolyte.
[0011] In some possible implementations, the molar ratio of the organic solvent to the complexing agent is 5:(1-5).
[0012] In some possible implementations, the organic solvent includes one of N,N-dimethylformamide, acetamide, or dimethyl sulfoxide.
[0013] In some possible implementations, a fast ion conductor is further added to the second solution, and the fast ion conductor includes Li 1.4 Al 0.4 Ti 1.6 (PO4)3、Li7La3Zr2O 12 or Li0.34 La 0.5 1TiO 2.94 One of them.
[0014] In some possible implementations, the fast ion conductor accounts for 5-20% by mass of the polyvinylidene fluoride.
[0015] The present application also provides a lithium metal battery comprising the composite solid electrolyte.
[0016] The composite solid electrolyte provided by the present application includes polyvinylidene fluoride, a lithium salt, an organic solvent and a ligand, and the polyvinylidene fluoride and the lithium salt are dissolved together in the ligand and the organic solvent. The introduction of the ligand can regulate the solvation structure of the composite solid electrolyte, and the organic solvent and the ligand form a large number of ion cluster solvation structures with the lithium salt, and interact with the polyvinylidene fluoride, thereby realizing lithium ion conduction. In the above-mentioned composite solid-state electrolyte, the ligand is chemically stable, and the coordination ability of the ligand with the lithium ions in the lithium salt is weaker than the coordination ability of the organic solvent with the lithium ions, and the interaction force between the ligand and the polyvinylidene fluoride is weak. Compared with a single organic solvent, the combination of the ligand and the organic solvent can weaken the binding force to lithium ions, and at the same time weaken the interaction force between the solvation structure and polyvinylidene fluoride in the composite solid-state electrolyte, thereby improving the ion conduction of lithium ions in the composite solid-state electrolyte, so that the composite solid-state electrolyte has better ion conduction ability and interface stability, thereby improving the interaction force between the single organic solvent and polyvinylidene fluoride in the composite solid-state electrolyte, which leads to severe capacity decay of the lithium metal battery during the continuous reaction process. At the same time, the ligand provided by the present application has excellent oxidation resistance, and has a small binding energy with lithium ions, small interface side effects with lithium metal, high stability, and can improve the ion transport capacity required for high-rate operation of lithium metal batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In Figure 1, (a) is an atomic force microscope image of the PVDF solid electrolyte, and (b) is a nano-infrared microscope image of (a).
[0018] FIG2 is a thermogravimetric test curve of the Li-DMF-PVDF solid electrolyte of the present application.
[0019] Figure 3 is an infrared test graph of 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte.
[0020] In Figure 4, (a) is a schematic diagram of the solvation structure of 8M Li-DMF solution, and (b) is an analysis diagram of the Raman test results of 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte.
[0021] Figure 5 is based on Li +Calculate FSI for coordinate center - , DMF, and PVDF radial distribution function diagrams.
[0022] FIG6 is an oxidation potential test graph of a button cell prepared with 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte.
[0023] In Figure 7, (a) is a test graph of the lithium ion migration number of a button cell prepared with 8M Li-DMF solution; (b) is a test graph of the lithium ion migration number of a button cell prepared with Li-DMF-PVDF solid electrolyte; and (c) is a graph of the ion migration activation energy of the Li-DMF-PVDF solid electrolyte.
[0024] In Figure 8, (a) is a diagram showing the theoretical calculation results of the molecular orbital energy levels of TFA and DMF; (b) is a performance comparison analysis diagram of TFA and DMF;
[0025] In Figure 9, (a) is an oxidation potential test diagram of an 8M Li-DMF solution [marked as Li-DMF (1:2) in (a)] and a solution of LiFSI dissolved in TFA with the same molar ratio [marked as Li-TFA (1:2) in (a)]; (b) is an oxidation-reduction test diagram of a half-cell assembled with a Li-DMF (1:2) solution; and (c) is an oxidation-reduction test diagram of a half-cell assembled with a Li-TFA (1:2) solution.
[0026] In Figure 10, (a) is a vertical graph showing the calculated binding energies of TFA solvent and DMF solvent for lithium ions; (b) is a graph showing the lithium element ( 7 Li) liquid NMR images, (c) are the fluorine elements of Li-TFA (1:2), Li-TFA (1:4), Li-DMF (1:2) and Li-DMF (1:4) ( 19 F) Liquid NMR image; (d) is a vertical graph showing the calculated interaction forces between TFA solvent and DMF solvent and PVDF respectively.
[0027] Figure 11 is Li prepared in Example 1 1.4 Al 0.4 Ti 1.6 X-ray diffraction pattern of (PO4)3 nanowires.
[0028] FIG12 is an X-ray diffraction pattern of the composite solid electrolyte prepared in Example 1.
[0029] FIG13 is an X-ray diffraction pattern of the composite solid electrolyte prepared in Comparative Example 2.
[0030] In Figure 14, (a) is a scanning electron microscope image of the composite solid electrolyte prepared in Example 1; (b) is a cross-sectional electron microscope image of the composite solid electrolyte prepared in Example 1.
[0031] In Figure 15, (a) is an ion migration activation energy diagram of the composite solid electrolytes prepared in Example 1 and Comparative Example 2; (b) is an oxidation potential test diagram of the composite solid electrolytes prepared in Example 1 and Comparative Example 2; and (c) is a lithium ion migration number test diagram of the composite solid electrolyte assembled by the composite solid electrolyte prepared in Example 1.
[0032] FIG16 is a cycle performance test graph of the lithium metal batteries assembled in Example 1 and Comparative Example 2 at 25° C. and 2C rate after 4900 cycles.
[0033] FIG17 is a cycle performance test graph of the lithium metal batteries assembled in Example 1 and Comparative Example 2 at 45° C. and 2C rate for 1000 cycles.
[0034] FIG18 is a cycle performance test graph of the lithium metal batteries assembled in Example 1 and Comparative Example 2 at -20° C. and 0.1C rate after 200 cycles.
[0035] FIG19 is a cycle performance test chart of a soft-pack battery assembled with the composite solid electrolyte prepared in Example 1 and cycled 300 times at 25° C. and 0.5C rate. DETAILED DESCRIPTION
[0036] The embodiments of the present invention are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.
[0037] Throughout this specification, reference to terms such as "one embodiment," "some embodiments," "examples," "specific examples," or "some examples" means that a specific feature, structure, material, or characteristic described in conjunction with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, schematic representations of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.
[0038] The present application provides a method for preparing a composite electrolyte, the preparation method comprising:
[0039] S1. Mix polyvinylidene fluoride and lithium salt, and dissolve them in an organic solvent to obtain a first solution.
[0040] In some embodiments, the lithium salt includes at least one of lithium bis(fluorosulfonyl)imide (LIFSI), lithium bis(trifluorosulfonyl)imide, or lithium difluorooxalatoborate.
[0041] In some embodiments, the organic solvent comprises one of N,N-dimethylformamide (DMF), acetamide, or dimethyl sulfoxide.
[0042] In this step, the mass ratio of polyvinylidene fluoride (PVDF) to lithium salt is (1-3):1, and the mass ratio can be 1:1, 2:1, or 3:1. The polyvinylidene fluoride and lithium salt are added to an organic solvent and stirred for 2-4 hours to completely dissolve the polyvinylidene fluoride and lithium salt in the organic solvent, forming a uniform, transparent first solution.
[0043] S2. Add a ligand to the first solution and stir evenly to obtain a second solution, wherein the coordination ability of the ligand with the lithium ions in the lithium salt is weaker than the coordination ability of the organic solvent with the lithium ions, and the ligand includes at least one of trifluoroacetamide (TFA), N-methyltrifluoroacetamide (NMTFA) or N,N-dimethyltrifluoroacetamide (FDMA).
[0044] In this step, polyvinylidene fluoride and lithium salt are dissolved together in an organic solvent and a ligand. Compared with a solid electrolyte composed of a single organic solvent, polyvinylidene fluoride and a lithium salt, the addition of a ligand can regulate the solvation structure of the subsequently formed composite solid electrolyte. Due to the stable chemical properties of the ligand, the ligand has a weaker coordination ability with lithium ions than the organic solvent, and its interaction with polyvinylidene fluoride is weak. Compared with a single organic solvent, the combination of the ligand and the organic solvent can weaken the binding force to lithium ions, and at the same time, it can also weaken the interaction between the solvation structure and polyvinylidene fluoride in the composite solid electrolyte, thereby improving the ion conduction of lithium ions in the composite solid electrolyte, so that the composite solid electrolyte has better ion conduction ability and interface stability, thereby improving the phenomenon that the interaction between the single organic solvent and polyvinylidene fluoride in the composite solid electrolyte is large, resulting in severe capacity decay of the lithium metal battery during the continuous reaction process.
[0045] For example, taking the organic solvent DMF as an example, the coordination agent TFA is used as an example for explanation. Compared with the case where the solid electrolyte only contains DMF, lithium salt and PVDF, the TFA contained in the composite solid electrolyte in this application has high chemical stability and high oxidation resistance compared to DMF, thereby being able to broaden the charge and discharge voltage range of the lithium metal battery and improve the interface stability of the lithium metal battery. In the composite solid electrolyte of this application, DMF and TFA form a large number of ion cluster solvation structures with lithium ions and interact with PVDF to achieve lithium ion conduction.
[0046] By calculating the binding energy of DMF and TFA to lithium ions respectively, it was found that the binding energy of TFA to lithium ions is much weaker than that of DMF to lithium ions, which can enhance the interaction between lithium ions and anions, facilitate the anions in the lithium salt to enter the solvation structure, form contact ion pairs and ion aggregates, promote the reduction and decomposition of anions at the interface to generate rich inorganic components (such as Li2O, LiF, Li3N, Li2S) and form a chemically stable solid electrolyte interface film (SEI), which is conducive to the stable operation of the battery. At the same time, the interaction forces between DMF and TFA and PVDF were also calculated. After calculation, it was found that the force between TFA and PVDF is weaker than the force between DMF and PVDF. The introduction of TFA weakened the force with the solvent and PVDF, and improved the ion conductivity of the electrolyte. This also shows that the introduction of TFA regulates the solvation structure in the composite solid electrolyte.
[0047] The above-mentioned ligand provided in the present application has high stability, higher oxidation resistance than organic solvents, is not easy to react on the electrode surface, has little chemical reaction with lithium metal, and weakens interfacial side reactions; and compared with organic solvents, the above-mentioned ligand can also provide a weak coordination environment for lithium ions and PVDF, thereby improving the ion conductivity and interface stability of the composite solid electrolyte.
[0048] In order to further study the mechanism of action of the composite solid electrolyte in this application, this application also conducted an atomic force microscopy test on the PVDF electrolyte formed by the combination of PVDF and DMF. Referring to Figure 1, (a) is an atomic force microscope image of the PVDF solid electrolyte, and (b) is a nano-infrared microscope image of (a). As can be seen from Figure 1, (a) shows that the PVDF electrolyte is a non-dense porous structure, and the PVDF is in the form of spherical grains and there are pores between adjacent spherical grains [the black part in (a)]; (b) shows that the DMF solvent is mainly distributed inside the spherical crystals of PVDF rather than in the pores [the white part in (b)].
[0049] In order to further analyze the interactions and characteristics between substances in the electrolyte, this application takes a solid electrolyte composed of LIFSI, DMF and PVDF (labeled as Li-DMF-PVDF solid electrolyte) as an example for analysis. Thermogravimetric analysis of the Li-DMF-PVDF solid electrolyte was performed under nitrogen, as shown in Figure 2. It can be calculated from Figure 2 that the Li-DMF-PVDF solid electrolyte contains 18.87wt% of residual DMF solvent. Based on this data, according to the mass of LIFSI in the original Li-DMF-PVDF solid electrolyte, the Li-DMF-PVDF solid electrolyte containing 18.87wt% of residual DMF solvent contains 8M LiFSI. Based on this, this application takes a DMF solution of high concentration 8M LiFSI (labeled as 8M Li-DMF solution) as an example, and analyzes the intrinsic differences between the Li-DMF-PVDF solid electrolyte and the 8M Li-DMF solution as electrolytes and the interactions between their respective substances. Infrared testing and Raman testing were performed on the 8M Li-DMF solution and the Li-DMF-PVDF solid electrolyte, respectively. Referring to Figure 3, the infrared test images of the 8M Li-DMF solution and the Li-DMF-PVDF solid electrolyte show that the -CH3 peak in the Li-DMF-PVDF solid electrolyte exhibits a significant shift (to the right) compared to the 8M Li-DMF solution, while the other peaks do not. This is due to the interaction between the -CH3 and PVDF segments in DMF, which causes the -CH3 peak to shift. The absence of other peaks also indicates that the interaction between the lithium salt anion and PVDF is very weak, and that the 8M Li-DMF solution and the Li-DMF-PVDF solid electrolyte have very similar solvation coordination structures.
[0050] Refer to Figure 4, (a) is a schematic diagram of the solvation structure of 8M Li-DMF solution, and (b) is an analysis diagram of the Raman test results of 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte. (a) shows all the solvation types in 8M Li-DMF solution. (b) analyzes the proportion of various types of solvation structures in 8M Li-DMF solution in (a). From (a), it can be seen that 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte have very similar solvation structures. Combined with theoretical calculations, Li + Calculate FSI for coordinate center - , DMF, PVDF radial distribution function, the results analysis is shown in Figure 5, in the first solvent sheath A sharp peak appeared near the + The closest distance, due to DMF and Li + With strong coordination effect, Li-N(FSI -) shows no peak in the first solvent sheath, indicating that the probability of lithium salt anions entering the first solvent sheath is very low. Li-F(PVDF) also shows no peak, indicating that the PVDF polymer does not participate in the solvation structure, as shown in Figure 4(a). Therefore, for PVDF electrolytes, the solvation structure, rather than the polymer itself, plays a key role and determines both the ionic conductivity and interfacial stability of the solid electrolyte.
[0051] This application also conducted electrochemical stability window tests on 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte. Referring to Figure 6, under identical conditions, the decomposition voltages of 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte were 3.62V and 4.25V, respectively. This indicates that the fundamental cause of instability in the DMF-containing PVDF electrolyte is the inherent instability of 8M Li-DMF, which causes the PVDF electrolyte to decompose easily during the continuous reaction process on the electrode surface.
[0052] Furthermore, the lithium ion migration numbers of 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte were tested. Specifically, two lithium sheets were selected and assembled into button cells with the above electrolyte / solid electrolyte. Impedance testing was performed using an electrochemical workstation at 25°C, and the lithium ion migration numbers of the above electrolytes were calculated and evaluated. Referring to Figure 7, (a) is a test graph of the lithium ion migration number of the button cell prepared with 8M Li-DMF solution; (b) is a test graph of the lithium ion migration number of the button cell prepared with Li-DMF-PVDF solid electrolyte; and (c) is a graph of the ion migration activation energy of the Li-DMF-PVDF solid electrolyte. From the results in Figure 7, it can be seen that the lithium ion migration number (t) of 8M Li-DMF solution and Li-DMF-PVDF solid electrolyte is very low, and the lithium ion migration number of 8M Li-DMF and Li-DMF-PVDF solid electrolyte is similar, and the ion migration activation energy of Li-DMF-PVDF solid electrolyte is higher, which is due to the strong interaction between DMF and lithium ions and PVDF segments.
[0053] The present application has found through calculation that the coordination agent provided by the present application is more stable than DMF. Referring to Figure 8, (a) is a diagram showing the theoretical calculation results of the molecular orbital energy levels of TFA and DMF, and (b) is a performance comparison analysis diagram of TFA and DMF. The present application uses the coordination agent TFA as an example and conducts a comparative analysis with DMF. From (a) and (b) in Figure 8, it is found that TFA has excellent high-pressure stability and interfacial stability with lithium metal, and has a weak interaction force with PVDF and a lower binding energy with lithium ions.
[0054] Figure 9 (a) shows the oxidation potential of an 8M Li-DMF solution (labeled as Li-DMF(1:2) in (a)) and a solution of LiFSI dissolved in TFA at the same molar ratio (labeled as Li-TFA(1:2) in (a)). (b) shows the redox potential of a half-cell assembled with the Li-DMF(1:2) solution. (c) shows the redox potential of a half-cell assembled with the Li-TFA(1:2) solution. As can be seen in (a), the oxidation potential of Li-DMF(1:2) is 3.62V, which is lower than that of Li-TFA(1:2) (4.81V). (b) shows that the interfacial side reactions between Li-DMF(1:2) and lithium metal are intense, preventing lithium ions from effectively intercalating and deintercalating lithium. (c) demonstrates that Li-TFA(1:2) forms a solid electrolyte interphase (SEI) in the first cycle, with minimal interfacial side reactions with lithium metal.
[0055] The present application also calculates the binding energy of different solvents to lithium ions. Referring to Figure 10, (a) is a vertical graph showing the binding energy of TFA and DMF solvents to lithium ions, and it is found that the binding energy of TFA to lithium ions is much weaker than that of DMF. Figure 10 (b) shows the lithium element ( 7 Li) liquid NMR images, (c) are the fluorine elements of Li-TFA (1:2), Li-TFA (1:4), Li-DMF (1:2) and Li-DMF (1:4) ( 19 F) Liquid NMR images, from Figure 10 (b) and (c), it can be further explained that at the same molar ratio, the Li-TFA solution 7 Li and 19 F all appear in high-field chemical shifts, indicating that TFA's binding energy to lithium ions is much weaker than DMF's. Furthermore, calculations show that the binding force between TFA and PVDF is weaker than that between DMF and TFA, as shown in Figure 10 (d). (D) is a vertical graph showing the calculated interaction forces between TFA and DMF solvents and PVDF, respectively.
[0056] In some embodiments, the molar ratio of the organic solvent to the ligand is 5:(1-5), such as 5:1, 5:2, 5:3, or 5:5. If the molar ratio is greater than 5:1, the ligand has little effect on regulating the solvation of the composite solid electrolyte. If the molar ratio is less than 5:5, the ligand is present in an excessive amount, resulting in undissociated lithium salts and reduced ion conductivity of the composite solid electrolyte.
[0057] In some embodiments, a fast ion conductor is further added to the second solution, and the fast ion conductor includes Li 1.4 Al0.4 Ti 1.6 (PO4)3、Li7La3Zr2O 12 or Li 0.34 La 0.5 1TiO 2.94 Fast ion conductors have high ionic conductivity and high specific surface area. The addition of fast ion conductors can further improve the ionic conductivity of the composite solid electrolyte, while also helping to increase the densification and stability of the composite solid electrolyte.
[0058] The fast ion conductor and the ligand can be added to the first solution simultaneously, or the ligand can be added first and then the fast ion conductor. After the ligand and fast ion conductor are added to the first solution, stirring is required for 24-48 hours to obtain a uniform suspension. In other embodiments, PVDF, lithium salt, organic solvent, ligand, and fast ion conductor can be mixed simultaneously to obtain a mixed solution.
[0059] In some embodiments, the fast ion conductor accounts for 5-20% by weight of the polyvinylidene fluoride. For example, the weight percentage can be 5%, 7%, 10%, 15%, or 20%. If a large amount of fast ion conductor is added, the fast ion conductor may agglomerate, thereby reducing the ion conductivity of the composite solid electrolyte.
[0060] S3. Drying the second solution to obtain a composite solid electrolyte.
[0061] In some embodiments, the second solution is transferred to a glass petri dish and placed in a forced air oven at 60-80°C to dry the resulting composite solid electrolyte. To facilitate subsequent application in lithium metal batteries, the composite solid electrolyte is in the form of a film, which is punched to a predetermined size and stored dry in an inert atmosphere.
[0062] The present application also provides a composite solid electrolyte, which includes polyvinylidene fluoride, a lithium salt, an organic solvent and a ligand. The coordination ability of the ligand with the lithium ions in the lithium salt is weaker than the coordination ability of the organic solvent with the lithium ions. The ligand includes at least one of trifluoroacetamide, N-methyltrifluoroacetamide or N,N-dimethyltrifluoroacetamide.
[0063] In the above-mentioned composite solid-state electrolyte, the ligand has stable chemical properties, and its coordination ability with lithium ions is weaker than that of organic solvents, and its interaction with polyvinylidene fluoride is weaker. Compared with a single organic solvent, the combination of the ligand and the organic solvent can weaken the binding force to lithium ions. At the same time, it can also weaken the interaction force between the solvation structure and polyvinylidene fluoride in the composite solid-state electrolyte, thereby improving the ion conduction of lithium ions in the composite solid-state electrolyte, so that the composite solid-state electrolyte has better ion conduction ability and interface stability, thereby improving the phenomenon that the interaction force between the single organic solvent and polyvinylidene fluoride in the composite solid-state electrolyte is large, resulting in severe capacity decay of the lithium metal battery during continuous reaction.
[0064] The present application also provides a lithium metal battery, comprising a composite solid electrolyte, a lithium sheet, and a positive electrode sheet, wherein the composite solid electrolyte is disposed between the lithium sheet and the positive electrode sheet. The active material in the positive electrode sheet comprises one of lithium cobalt oxide, a ternary positive electrode material, and lithium manganese oxide.
[0065] The present invention will be explained below with reference to the embodiments. Those skilled in the art will appreciate that the following examples are intended only to illustrate the present invention and are not to be construed as limiting the present invention. Unless otherwise indicated, the reagents, software, and instruments not specifically described in the following examples are all conventional commercially available products or open source.
[0066] Example 1
[0067] This implementation is based on Li 1.4 Al 0.4 Ti 1.6 Taking the preparation method of (PO4)3[LATP] as an example, the preparation method includes:
[0068] (1) 0.1448 g of LiNO3 (lithium nitrate), 0.2251 g of Al(NO3)3·9H2O (aluminum nitrate nonahydrate), 0.8168 g of Ti(OC4H9)4 (tetrabutyl titanate), 0.7114 g of C6H7O3P (phenylphosphonic acid), 0.8646 g of a complexing agent (C6H8O7, citric acid), and 1.75 g of a binder (PVP, polyvinylpyrrolidone) were dissolved in 15 mL of DMF (N,N-dimethylformamide) to prepare a precursor solution. The precursor solution was stirred at room temperature for at least 24 h to obtain a homogeneous, transparent solution.
[0069] (2) The precursor solution stirred evenly in step (1) is placed in a syringe and assembled into an electrospinning machine. The syringe is pushed at a pushing speed of 1.0 mL / h. The electrospinning voltage is set to a high voltage of 20 kV and a low voltage of -1 kV. The receiving distance is set to 15 cm. At the same time, the air humidity is ensured to be less than 30%. Electrospinning is performed to obtain a spinning membrane.
[0070] (3) Dry the spun membrane obtained in step (2) in an oven at 80° C. for more than 12 hours to remove excess solvent.
[0071] (4) Cut the spun membrane dried in step (3) into the size of a crucible and stack them in the crucible in sequence, placing a layer of carbon paper between each layer. Place the membrane in a muffle furnace and heat it to 280°C at a heating rate of 1°C / min. Keep the temperature for 2 hours for pre-oxidation, then cool it in the furnace and remove it.
[0072] (5) Remove the carbon paper from the crucible of step (4), continue to place the spinning membrane in the crucible, and put it into a muffle furnace, heat it to 800℃ at a heating rate of 5℃ / min, keep it warm for 6h, and sinter it to obtain Li 1.4 Al 0.4 Ti 1.6 (PO4)3 nanowires.
[0073] A method for preparing a composite solid electrolyte and a lithium metal battery, comprising:
[0074] Step 1: First, weigh 100 mg of PVDF (binder) and place it in a stirring bottle. Add 1 mL of NMP (N-methylpyrrolidone) and stir on a small stirrer for 1 hour until the PVDF is completely dissolved. Then, add 100 mg of Super P (conductive carbon black) and 1 mL of NMP and stir at room temperature for 1 hour. Then, add 800 mg of NCM811 active material and 1.5 mL of NMP and stir at room temperature for more than 6 hours to obtain the positive electrode slurry.
[0075] Step 2: The positive electrode slurry obtained in step 1 is coated on aluminum foil, dried at 80° C. for more than 6 hours, cut into appropriate sizes to obtain NCM811 positive electrode sheets, and placed in a vacuum oven for drying and storage.
[0076] Step 3: Under an inert atmosphere, weigh 267 mg of LiFSI and place it in a stirring bottle. Add 15 mL of DMF and 400 mg (equivalent to 6.25 mmol of PVDF) of PVDF and stir on a stirrer. Stir at room temperature for more than 2 hours until LiFSI and PVDF are completely dissolved to obtain a uniform transparent solution, i.e., the first solution is obtained.
[0077] Step 4: Add 60 mg of LATP nanowires to the first solution obtained in step 3, and stir at room temperature for more than 24 hours to obtain a uniform white suspension.
[0078] Step 5: Add 500 mg (equivalent to 4.42 mmol TFA solvent) of TFA solvent to the white suspension obtained in step 4, and stir at room temperature for more than 24 hours to obtain a uniform white suspension.
[0079] Step 6: Pour the white suspension obtained in step 5 into a glass culture dish and place it in a 55°C forced air oven to dry for 23 hours to obtain a composite solid electrolyte (abbreviated as PDTL) membrane, which is punched into a suitable size and stored dry in an inert atmosphere for use.
[0080] Step seven, assembling the NCM811 positive electrode sheet prepared in step two, the composite solid electrolyte membrane prepared in step six, and lithium metal to obtain a lithium metal button battery.
[0081] Example 2
[0082] The difference between Example 2 and Example 1 is that the NCM811 positive electrode active material is replaced by Ni90 positive electrode active material, and the remaining steps are the same as Example 1.
[0083] Example 3
[0084] The difference between Example 3 and Example 1 is that the NCM811 positive electrode active material is replaced by LiCoO2 active material, and the remaining steps are the same as Example 1.
[0085] Example 4
[0086] The difference between Example 4 and Example 1 is that the NCM811 positive electrode active material is replaced by LiCoO2 active material, and the TFA solvent is replaced by N-methyltrifluoroacetamide (NMFA). The remaining steps are the same as Example 1.
[0087] Example 5
[0088] The difference between Example 5 and Example 1 is that the NCM811 positive electrode active material is replaced by LiCoO2 active material, and the TFA solvent is replaced by N,N-dimethyltrifluoroacetamide (FDMA). The remaining steps are the same as Example 1.
[0089] Comparative Example 1
[0090] The difference between Comparative Example 1 and Example 1 is that LATP nanowires and TFA solvent are not added to the prepared composite solid electrolyte, and the remaining steps are the same as those in Example 1.
[0091] Comparative Example 2
[0092] The difference between Comparative Example 2 and Example 1 is that TFA solvent is not added to the prepared composite solid electrolyte, and the remaining steps are the same as those in Example 1.
[0093] This application also studies the Li prepared in Example 1 1.4 Al 0.4 Ti 1.6(PO4)3 nanowires and composite solid electrolyte membranes, as well as the composite solid electrolyte membrane prepared in Comparative Example 2, were subjected to X-ray diffraction tests. Referring to FIG11 , the characteristic peaks shown in FIG11 are consistent with those in PDF#35-0754, indicating that the Li 1.4 Al 0.4 Ti 1.6 (PO4)3 nanowires.
[0094] Refer to Figures 12 and 13. It can be seen from Figures 12 and 13 that Li 1.4 Al 0.4 Ti 1.6 The XRD peak position of (PO4)3 nanowires corresponds to that of the standard card, indicating that LATP nanowires can maintain phase stability in the composite solid electrolyte.
[0095] This application also conducted scanning electron microscopy testing on the composite solid electrolyte prepared in Example 1. Referring to Figure 14 , (a) is a scanning electron micrograph of the composite solid electrolyte prepared in Example 1, and (b) is a cross-sectional electron micrograph of the composite solid electrolyte prepared in Example 1. As can be seen in (a) and (b), both the surface and cross-section of the composite solid electrolyte are relatively dense.
[0096] The present application also conducted electrochemical performance tests on the composite solid electrolytes prepared in Example 1 and Comparative Example 2. Referring to Figure 15, Figure 15 (a) is a graph showing the ion migration activation energy of the composite solid electrolytes prepared in Example 1 and Comparative Example 2. As can be seen from (a), the addition of the TFA ligand reduces the ion migration activation energy in the composite electrolyte from 0.268 eV to 0.140 eV. Figure 15 (b) is a graph showing the oxidation potential of the composite solid electrolytes prepared in Example 1 and Comparative Example 2. As can be seen from (b), the TFA ligand introduced into the composite solid electrolyte increases the oxidation potential from 4.48 V to 4.77 V, thereby improving the electrochemical window of the composite solid electrolyte. Figure 15 (c) is a graph showing the lithium ion migration number of a button cell assembled with the composite solid electrolyte prepared in Example 1. As can be seen from (c), the lithium ion migration number reaches 0.67, which further demonstrates that the introduction of the ligand into the composite solid electrolyte improves the ion conductivity and interfacial stability with lithium metal.
[0097] The present application also conducted cycling performance tests on the lithium metal batteries assembled in Example 1 and Comparative Example 2. Refer to Figure 16, which shows the cycling performance test of the lithium metal batteries assembled in Example 1 and Comparative Example 2 at room temperature and a 2C rate after 4900 cycles. Under the same conditions, the lithium metal battery assembled with the composite solid electrolyte prepared in Example 1 can stably cycle for 4900 cycles with a capacity retention rate of 60%, while the lithium metal battery assembled with the composite solid electrolyte without the addition of a ligand fails after about 1000 cycles, and the capacity retention rate decreases rapidly.
[0098] Refer to Figure 17, which shows the cycling performance test results of lithium metal batteries assembled in Example 1 and Comparative Example 2 at 45°C and a 2C rate for 1000 cycles. Under the same conditions, the lithium metal battery assembled with the composite solid electrolyte prepared in Example 1 can stably cycle for 1000 cycles with a capacity retention rate of 66.7%. However, the lithium metal battery assembled with the composite solid electrolyte without the addition of a complexing agent has a capacity retention rate of only 7.9% after about 1000 cycles, and the capacity retention rate decreases rapidly.
[0099] Referring to Figure 18 , Figure 18 shows the cycling performance of lithium metal batteries assembled in Example 1 and Comparative Example 2 at -20°C and a 0.1C rate for 200 cycles. Under the same conditions, the lithium metal battery assembled with the composite solid electrolyte prepared in Example 1 can stably cycle for 200 cycles with a capacity retention rate of approximately 95.2%. However, the lithium metal battery assembled with the composite solid electrolyte without the addition of a complexing agent only retained a capacity of 42.5% after approximately 200 cycles, and the capacity retention rate decreased rapidly.
[0100] Refer to Figure 19, which shows the cycling performance of the composite solid electrolyte prepared in Example 1 assembled into a soft-pack battery after 300 cycles at 25°C and 0.5C rate. After 300 cycles, the soft-pack battery's capacity retention was 87.1%. The above-mentioned test data of lithium metal batteries at different temperatures and after assembly into soft-pack batteries demonstrate that the introduction of a ligand into the composite solid electrolyte can increase the lithium ion transference number of lithium metal batteries, improving the ion transport capacity required for high-rate operation.
[0101] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent replacements of the technical solutions of the present invention should not depart from the spirit and scope of the technical solutions of the present invention.
Claims
1. A composite solid electrolyte, characterized in that: The invention comprises polyvinylidene fluoride, a lithium salt, an organic solvent and a ligand, wherein the ligand has a weaker coordination ability with the lithium ions in the lithium salt than the organic solvent, and the ligand comprises at least one of trifluoroacetamide, N-methyltrifluoroacetamide or N,N-dimethyltrifluoroacetamide.
2. The composite solid electrolyte according to claim 1, characterized in that The organic solvent includes one of N,N-dimethylformamide, acetamide or dimethyl sulfoxide.
3. The composite solid electrolyte according to claim 1, characterized in that The composite solid electrolyte also includes a fast ion conductor, and the fast ion conductor includes Li 1.4 Al 0.4 Ti 1.6 (PO4)3, Li7La3Zr2O 12 or Li 0.34 La 0.5 1TiO 2.94 One of them.
4. The composite solid electrolyte according to claim 1, characterized in that The molar ratio of the organic solvent to the complexing agent is 5:(1-5).
5. A method for preparing a composite solid electrolyte, characterized in that: The preparation method comprises: Mixing polyvinylidene fluoride and lithium salt, and dissolving them in an organic solvent to obtain a first solution; adding a ligand to the first solution and stirring uniformly to obtain a second solution, wherein the ligand has a weaker coordination ability with the lithium ions in the lithium salt than the organic solvent has with the lithium ions, and the ligand includes at least one of trifluoroacetamide, N-methyltrifluoroacetamide or N,N-dimethyltrifluoroacetamide; The second solution is dried to obtain a composite solid electrolyte.
6. The method for preparing the composite solid electrolyte according to claim 5, characterized in that: The molar ratio of the organic solvent to the complexing agent is 5:(1-5).
7. The method for preparing a composite solid electrolyte according to claim 5, characterized in that: The organic solvent includes one of N,N-dimethylformamide, acetamide or dimethyl sulfoxide.
8. The method for preparing a composite solid electrolyte according to claim 5, characterized in that: The second solution is also added with a fast ion conductor, the fast ion conductor includes Li 1.4 Al 0.4 Ti 1.6 (PO4)3, Li7La3Zr2O 12 or Li 0.34 La 0.5 1TiO 2.94 One of them.
9. The method for preparing a composite solid electrolyte according to claim 8, characterized in that: The fast ion conductor accounts for 5-20% of the mass percentage of the polyvinylidene fluoride.
10. A lithium metal battery, characterized in that: The method comprises the composite solid electrolyte as claimed in any one of claims 1 to 4.
Citation Information
Patent Citations
Solid polymer electrolyte and preparation method and application thereof
CN114678589A
Composite solid electrolyte, preparation method thereof and lithium metal battery
CN116454370A
Quasi-solid electrolyte and secondary battery
JP2022154743A
Composite electrolyte, method for manufacturing the same and battery
US20210328264A1
Cited By
Preparation method of efficient lithium ion battery electrolyte based on novel polymer
CN119133615A
A method for preparing a high-efficiency lithium-ion battery electrolyte based on a novel polymer
CN119133615B
Low-temperature solid polymer electrolyte, preparation method and battery
CN120657244A
PVDF (Polyvinylidene Fluoride)-based solid electrolyte based on ester hyperbranched polymer molecule modification and application of PVDF-based solid electrolyte
CN121484194A
Lithium ion conductive composite solid electrolyte comprising LATP nano fibers and method for producing the same
KR102980785B1