A method, device and medium for arc additive manufacturing of curved surface of robot roll forging die

Through the curved arc additive manufacturing method of the robot roll forging mold, the problems of poor surface quality and molten pool flow in the additive repair of the cylindrical curved surface of the roll forging mold are solved, achieving efficient and accurate additive repair, extending the life of the mold, and meeting the requirements meet the demand for high-quality, high-efficiency production.

CN116851871BActive Publication Date: 2024-10-11HUBEI LONGZHONG TECHNOLOGY DEVELOPMENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310968507.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-02
Publication Date
2024-10-11
Estimated Expiration
2043-08-02

AI Technical Summary

Technical Problem

The existing technology has poor surface quality, unreasonable material distribution and molten pool flow problems in the additive repair of cylindrical curved surfaces of roll forging dies, resulting in a low service life after repair and unable to meet the needs of high-quality and high-efficiency production.

Method used

The robot roll forging mold surface arc additive manufacturing method is used to obtain the three-dimensional STL model of the failed mold, determine the defective NURBS surface and additive entities, establish an offset surface group, conduct trajectory planning, generate arc additive trajectory files, and control the end of the welding gun. Attitude and position, combined with the angle of the rotary positioner, enable precise additive repair.

Benefits of technology

It improves the surface quality of additive repair, avoids molten pool flow problems, extends the service life of the roll forging mold, and meets the needs for high-quality and high-efficiency production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116851871B_ABST
    Figure CN116851871B_ABST
Patent Text Reader

Abstract

The present invention discloses a method, equipment and medium for manufacturing curved surface of a robot roll forging die by arc additive manufacturing, comprising the following steps: obtaining a scanning result of a failed roll forging die, obtaining a three-dimensional STL model of a defective surface of the failed roll forging die, and determining a defective NURBS surface, an additive entity, and an additive repair margin surface, obtaining a three-dimensional solid STL of a defective area to be repaired and determining an intersecting cutting surface group; performing trajectory planning on the intersecting cutting surface group and determining a trajectory file; generating a robot arc additive trajectory file based on the trajectory file, and determining the TCP posture and position of a robot welding gun end based on the robot arc additive trajectory file; determining the current angle of a rotary positioner, and calculating the rotation angle of the rotary positioner based on the robot arc additive trajectory file and the current angle of the positioner; and controlling the coordinated action of the robot welding gun and the positioner based on the TCP posture and position of the robot welding gun end and the rotation angle of the rotary positioner to complete the additive repair of the failed roll forging die.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of robot arc additive remanufacturing, and in particular to a robot roll forging die curved surface arc additive manufacturing method, equipment and medium. Background Art

[0002] Roll forging is a forming technology that deforms metal materials during rotation through a pair of rotating rollers equipped with circular roll forging dies to obtain various forgings or forging blanks. Compared with ordinary plane split die forging processes, roll forging processes have less relative sliding between metal and die, require smaller equipment tonnage, produce smoothly, have less vibration and noise, rotate continuously, have high production efficiency, and have low requirements for plant and foundation. A large number of forgings in the fields of automobiles, aerospace, engineering machinery, etc. are made or directly formed through roll forging processes, such as automobile front axles, crankshafts, connecting rods and other forgings. Roll forging dies are subjected to high temperatures, heavy loads, and friction of the blanks during service, and are prone to wear, deformation, and fatigue crack failure. In order to extend the life of the roll forging dies, they need to be frequently repaired and remanufactured.

[0003] The robot-automated repair and remanufacturing process based on arc additive manufacturing technology has been applied to ordinary plane parting molds, that is, the defective and ineffective areas of the forging mold are horizontally layered, and then the robot arc additive manufacturing technology is used to accumulate and add materials layer by layer from the bottom to the surface, and the repair and forming are automated, which has good shape and property repair effects. However, the roll forging mold is composed of two upper and lower rotating rolling molds, and the parting surface is a cylindrical surface. When horizontal layered additive remanufacturing is used, the surface surface is affected by the "step effect" and the forming accuracy is extremely poor, and it is impossible to form a gradient material structure of the base layer, transition layer, and cover layer that is evenly distributed along the depth direction, resulting in a low life of the roll forging die after repair, which cannot meet the high-quality and high-efficiency production of key components of key equipment in various industries. If the welding gun is directly controlled to add materials along the cylindrical surface, different welding postures such as upward and downward are prone to occur, and the molten pool fluid is prone to flow due to gravity, resulting in poor forming quality, and even the inability to complete the material accumulation additive repair and forming. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned technical deficiencies and provide a method, equipment and medium for arc additive manufacturing of curved surfaces of robot roll forging dies, so as to solve the technical problems of poor surface quality, unreasonable material distribution and flowing molten pool of curved surface forming in layered additive manufacturing during the repair of cylindrical roll forging dies in the prior art.

[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for arc additive manufacturing of a curved surface of a robot roll forging die, comprising the following steps:

[0007] Obtaining the scanning result of the failed roller forging die to obtain a three-dimensional STL model of the defective surface of the failed roller forging die;

[0008] Based on the three-dimensional STL model of the defective surface of the failed roll forging die, the defective NURBS surface, the additive solid and the additive repair margin surface are determined, and based on the defective NURBS surface, the additive solid and the additive repair margin surface, the three-dimensional solid STL of the defective area to be repaired is obtained;

[0009] After establishing the offset surface group of the failed roll forging die based on the three-dimensional solid STL of the defective area to be repaired, determining the intersecting cutting surface group based on the three-dimensional solid STL of the defective area to be repaired and the offset surface group;

[0010] Performing trajectory planning on the intersecting cutting surface group and determining a trajectory file;

[0011] After generating a robot arc additive trajectory file based on the trajectory file, determining the TCP posture and position of the robot welding gun end based on the robot arc additive trajectory file;

[0012] Determine the current angle of the rotary positioner on which the failed roll forging die is installed, and calculate the rotation angle of the rotary positioner based on the robot arc additive trajectory file and the current angle of the positioner;

[0013] Based on the TCP posture and position of the robot welding gun end and the rotation angle of the rotary positioner, the robot welding gun and the positioner are controlled to cooperate to complete the additive repair of the failed roll forging die.

[0014] In some embodiments, the method of determining the defective NURBS surface, the additive entity, and the additive repair margin based on the defective surface of the failed roll forging die, and obtaining the three-dimensional solid STL of the defective area to be repaired based on the defective NURBS surface, the additive entity, and the additive repair margin includes:

[0015] After aligning the three-dimensional STL model of the defective surface of the failed roll forging die with the precise CAD digital model coordinates, the three-dimensional STL model of the defective surface of the failed roll forging die is processed into a NURBS grid surface to obtain a defective NURBS surface;

[0016] Importing the defective NURBS surface and the precise CAD digital model into the three-dimensional modeling software to determine the entity of the additive area;

[0017] Obtaining a precise CAD surface of the forging die, and offsetting the precise CAD surface of the forging die outward to obtain an additive repair margin curved surface;

[0018] The additive area entity is subjected to Boolean subtraction with the defective NURBS surface and the additive repair margin surface to obtain a three-dimensional solid STL of the defective area to be repaired.

[0019] In some embodiments, after establishing the offset surface group of the failed roll forging die based on the three-dimensional solid STL of the defective area to be repaired, determining the intersecting cutting surface group based on the three-dimensional solid STL of the defective area to be repaired and the offset surface group includes:

[0020] Based on the three-dimensional solid STL of the defective area to be repaired, a cylindrical surface is drawn and the maximum radial depth of the three-dimensional solid of the defective area to be repaired is calculated;

[0021] Presetting the thickness of each layer during additive repair, based on the maximum depth and the thickness of each layer, offsetting the cylindrical surface inwards, and establishing an offset curved surface group of the failed roll forging die;

[0022] The offset curved surface group is intersected with the three-dimensional solid STL of the defective area to be repaired to obtain an intersecting cutting surface group of the failed roll forging die.

[0023] In some embodiments, the calculation formula for the intersecting cutting surface group is:

[0024] ∑' N+1 ={SF',SF1',SF2',SF3',…,SFN'},

[0025] ∑ N+1 ={SF,SF1,SF2,SF3,…,SFN},

[0026] N=D / H-1,

[0027] Among them, ∑' N+1 is the intersecting cutting face group, ∑ N+1 is the offset surface group, SF is the cylindrical surface, N is the number of times the cylindrical surface SF is offset inward, D is the maximum radial depth of the three-dimensional entity in the defect area to be repaired, and H is the thickness of each layer during layer-by-layer additive repair.

[0028] In some embodiments, performing trajectory planning on the intersecting cutting surface group and determining a trajectory file includes:

[0029] Performing trajectory planning on the intersecting cutting surface group to determine the trajectory mode, the distance between adjacent trajectories, the trajectory direction and the axis of each trajectory spot welding gun;

[0030] Based on the trajectory mode, adjacent trajectories, trajectory direction and the spot welding gun axis of each trajectory, a trajectory file is determined.

[0031] In some embodiments, the trajectory file includes at least the position and posture of each trajectory point, and the position and posture of the trajectory point are calculated as follows:

[0032] Pi=[xi,yi,zi],

[0033] Si=[xi,yi,zi,ui,0,wi],

[0034] Where Pi is the position of the trajectory point, xi is the coordinate of the ith trajectory point in the X direction, yi is the coordinate of the ith trajectory point in the Y direction, and zi is the coordinate of the ith trajectory point in the Z direction; Si is the posture of the ith trajectory point, ui is the X direction component, 0 is the Y direction component, and wi is the Z direction component.

[0035] In some embodiments, determining the TCP posture and position of the robot welding gun end based on the robot arc additive trajectory file includes:

[0036] Establishing a welding gun end TCP posture rotation matrix, and calculating the welding gun end TCP posture quaternion based on the welding gun end TCP posture rotation matrix;

[0037] Based on the position of the trajectory point and the TCP posture quaternion of the welding gun end, the target point of the robot arc additive trajectory is determined.

[0038] In some embodiments, the rotation angle calculation formula of the rotary positioner is:

[0039] β=α+|arctan2(yi / xi)|,

[0040] Among them, β is the rotation angle of the positioner, α is the current angle of the positioner, yi is the coordinate of the i-th track point in the Y direction, and xi is the coordinate of the i-th track point in the X direction.

[0041] In a second aspect, the present invention further provides an electronic device, comprising: a processor and a memory;

[0042] The memory stores a computer-readable program executable by the processor;

[0043] When the processor executes the computer-readable program, the steps in the robot roll forging die curved surface arc additive manufacturing method as described above are implemented.

[0044] In a third aspect, the present invention further provides a computer-readable storage medium storing one or more programs, which can be executed by one or more processors to implement the steps in the robotic roll forging die curved surface arc additive manufacturing method as described above.

[0045] Compared with the prior art, the arc additive manufacturing method, equipment and medium for the curved surface of the robot roll forging die provided by the present invention overcome the step effect of the traditional horizontal layered additive curved surface structure through the curved surface layering and curved surface trajectory planning additive, and improve the surface quality of additive repair. The failed roll forging die is installed on the rotary positioner, and the precise calculation of the rotary angle of the positioner during programming, the real-time adjustment of the positioner angle during additive, and the cooperation between the robot and the positioner system ensure that the molten pool is always in a horizontal position, avoiding the problem of unstable flow caused by gravity drag when the molten pool is located on an inclined surface or a vertical surface during traditional curved surface additive, thereby improving the forming quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is a flow chart of an embodiment of the arc additive manufacturing method for curved surface of a robot roll forging die provided by the present invention;

[0047] Figure 2 It is a schematic diagram of the geometric structure of a failed roll forging die and a defective area to be repaired in the arc additive manufacturing method for a curved surface of a robot roll forging die provided by the present invention;

[0048] Figure 3 It is a schematic diagram of an offset curved surface group of the arc additive manufacturing method for the curved surface of a robot roll forging die provided by the present invention;

[0049] Figure 4 It is a schematic diagram of the intersecting cutting surface group and the curved surface additive planning trajectory of the robot roll forging die curved surface arc additive manufacturing method provided by the present invention;

[0050] Figure 5 It is a schematic diagram of the operating environment of an embodiment of the robot roll forging die curved surface arc additive manufacturing program provided by the present invention. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0052] The present invention provides a method, device and medium for arc additive manufacturing of curved surface of a robot roll forging die, which can be used in a computer. The method, device or computer-readable storage medium involved in the present invention can be integrated with the above-mentioned device or can be relatively independent.

[0053] The present invention provides a method for arc additive manufacturing of a curved surface of a robot roll forging die, which can be executed by a computer, specifically by one or more processors of the computer. Figure 1 This is a flow chart of the arc additive manufacturing method for the curved surface of a robot roll forging die provided by an embodiment of the present invention. Figure 1 The arc additive manufacturing method for the curved surface of a robot roll forging die comprises the following steps:

[0054] S100, obtaining a scanning result of the failed roller forging die to obtain a three-dimensional STL model of a defective surface of the failed roller forging die;

[0055] S200, based on the three-dimensional STL model of the defective surface of the failed roller forging die, determining the defective NURBS surface, the additive solid and the additive repair margin surface, and obtaining the three-dimensional solid STL of the defective area to be repaired based on the defective NURBS surface, the additive solid and the additive repair margin surface;

[0056] S300, after establishing an offset surface group of the failed roll forging die based on the three-dimensional solid STL of the defective area to be repaired, determine an intersecting cutting surface group based on the three-dimensional solid STL of the defective area to be repaired and the offset surface group;

[0057] S400, determining a trajectory file by performing trajectory planning on the intersecting cutting surface group;

[0058] S500, after generating a robot arc additive trajectory file based on the trajectory file, determine the TCP posture and position of the robot welding gun end based on the robot arc additive trajectory file;

[0059] S600, determining the current angle of the rotary positioner on which the failed roll forging die is installed, and calculating the rotation angle of the rotary positioner based on the robot arc additive trajectory file and the current angle of the positioner;

[0060] S700, based on the TCP posture and position of the robot welding gun end and the rotation angle of the rotary positioner, control the coordinated action of the robot welding gun and the positioner to complete the additive repair of the failed roll forging die.

[0061] In this embodiment, first, a scanning result of the failed roller forging die is obtained to obtain a three-dimensional STL model of the defective surface of the failed roller forging die; based on the three-dimensional STL model of the defective surface of the failed roller forging die, a defective NURBS surface, an additive solid, and an additive repair margin surface are determined, and based on the defective NURBS surface, the additive solid, and the additive repair margin surface, a three-dimensional solid STL of the defective area to be repaired is obtained; based on the three-dimensional solid STL of the defective area to be repaired, an offset surface group of the failed roller forging die is established, and based on the three-dimensional solid STL of the defective area to be repaired and the offset surface group, an intersecting cutting surface group is determined; by intersecting the cutting surfaces The group performs trajectory planning and determines the trajectory file; secondly, based on the trajectory file, after generating the robot arc additive trajectory file, the TCP posture and position of the robot welding gun end are determined based on the robot arc additive trajectory file; the current angle of the rotary positioner on which the failed roller forging die is installed is determined, and the rotation angle of the rotary positioner is calculated based on the robot arc additive trajectory file and the current angle of the positioner; finally, based on the TCP posture and position of the robot welding gun end and the rotation angle of the rotary positioner, the robot welding gun and the positioner are controlled to coordinate to complete the additive repair of the failed roller forging die, thereby improving the additive repair forming quality.

[0062] In some embodiments, in step S100, after the roll forging die has been used for a certain number of times, when the working surface has precision tolerance or fatigue cracks due to wear or deformation, the surface failure layer is cleaned by carbon arc gouging or machining milling to remove 5 to 10 mm until there is no deep crack defect in the cavity, and the failed roll forging die is obtained. Figure 2 The failed roller forging die is scanned by a laser 3D scanner to obtain a 3D STL model of the defective surface of the failed roller forging die. Before scanning the defective surface of the roller forging die by a laser scanner, a white developer needs to be sprayed on the defective surface to avoid the problem of low point cloud recognition rate of the defective surface caused by the mirror reflection of the bright metal surface or the low light reflectivity of the black surface, and special scanning positioning points are randomly affixed to improve the scanning accuracy.

[0063] In some embodiments, in step S200, the three-dimensional STL model of the defective surface of the failed roll forging die is aligned with the precise CAD digital model coordinates through STL processing software, and the three-dimensional STL model of the defective surface of the failed roll forging die is processed into a NURBS grid surface to obtain a defective NURBS surface; the digital model alignment is performed using several planes and straight contour edges on the side of the roll forging die as a reference;

[0064] Import the defective NURBS surface and the precise CAD digital model into the 3D modeling software to determine the entity of the additive area;

[0065] Obtain the precise CAD surface of the forging die, and offset the precise CAD surface of the forging die outward by 3-5 mm to obtain the additive repair margin surface;

[0066] The additive area entity is subjected to Boolean subtraction with the defective NURBS surface and the additive repair margin surface to obtain the three-dimensional solid STL of the defective area to be repaired.

[0067] In some embodiments, in step S300, the maximum radial radius R1 of the three-dimensional entity of the defective area to be repaired of the roller forging die is taken as the radius, the center of the outer circle of the roller forging die is taken as the center of the circle, and the central axis of the outer circle of the roller forging die is taken as the axis, a cylindrical surface is drawn and the maximum radial depth of the three-dimensional entity of the defective area to be repaired is calculated;

[0068] When the additive repair is performed layer by layer, the thickness of each layer is H; the cylindrical surface is offset inward N times to establish the offset surface group of the failed roll forging die. Figure 3 ;

[0069] Intersect the offset surface group with the three-dimensional solid STL of the defective area to be repaired to obtain the intersecting cutting surface group of the failed roll forging die. Figure 4 ; The calculation formula for the intersecting cutting surface group is:

[0070] ∑' N+1 ={SF',SF1',SF2',SF3',…,SFN'},

[0071] Among them, ∑' N+1 is the intersecting cutting surface group, and the calculation formula for the offset surface group is:

[0072] ∑ N+1 ={SF,SF1,SF2,SF3,…,SFN},

[0073] Among them, ∑ N+1 is the offset surface group, SF is the cylindrical surface, N is the number of times the cylindrical surface SF is offset inward, and the calculation formula for the offset number N is:

[0074] N=D / H-1,

[0075] Among them, D is the maximum radial depth of the three-dimensional entity of the defect area to be repaired, and H is the thickness of each layer during the layer-by-layer additive repair.

[0076] In some embodiments, in step S400, a multi-axis surface finishing method in a three-dimensional software machining module is used to perform trajectory planning on the intersecting cutting surface group, see Figure 4; When planning the trajectory, the origin of the coordinate system is at the center of the outer circle of the roll forging die, the Z axis coincides with the outer circle axis of the roll forging die, and the X axis is in the plane of one end of the roll forging die; the trajectory mode is set to the curved surface reciprocating mode, the distance between adjacent trajectories is set to 4 to 7 mm, the trajectory direction is determined to be parallel or perpendicular to the outer circle axis of the roll forging die, and the axis of the welding gun at each trajectory point is determined to be perpendicular to the intersecting cutting surface, that is, the normal vector of each point on the surface is reversed, and the trajectory file is output, and the trajectory file at least includes the position and posture of each trajectory point, wherein the position of the trajectory point and the posture of the trajectory point are calculated as follows:

[0077] Pi=[xi,yi,zi],

[0078] Si=[xi,yi,zi,ui,0,wi],

[0079] Where Pi is the position of the trajectory point, xi is the coordinate of the ith trajectory point in the X direction, yi is the coordinate of the ith trajectory point in the Y direction, and zi is the coordinate of the ith trajectory point in the Z direction; Si is the posture of the ith trajectory point, ui is the X direction component, 0 is the Y direction component, and wi is the Z direction component.

[0080] In some embodiments, in step S500, based on the trajectory file, the program format of the selected robot is determined, and after the robot arc additive trajectory file is output, the TCP posture and position of the robot welding gun end are determined based on the robot arc additive trajectory file;

[0081] First, establish the welding gun end TCP posture rotation matrix, and the welding gun end TCP posture rotation matrix calculation formula is:

[0082] Ti=[wi,0,ui;0,1,0;-ui,0,wi],

[0083] Among them, Ti is the TCP posture rotation matrix of the welding gun end, wi is the Z direction component, ui is the X direction component, [0,1,0] is the Y direction component Yi; [wi,0,-ui] is the X direction component Xi, where Xi = Yi×Zi; [ui,0,wi] is the Z direction component Wi;

[0084] Secondly, the attitude quaternion is calculated based on the TCP attitude rotation matrix at the end of the welding gun. The attitude quaternion calculation formula is:

[0085]

[0086] q2=0,

[0087]

[0088] q4=0,

[0089] Qi=[q1,q2,q3,q4],

[0090] Among them, Qi is a quaternion, q1, q2, q3, q4 are the components of the quaternion;

[0091] Finally, based on the position and attitude quaternion of the trajectory point, the target point of the robot arc additive trajectory is determined. The calculation formula of the target point of the robot arc additive trajectory is:

[0092] PPi=[xi,yi,zi,q1,q2,q3,q4],

[0093] Among them, PPi is the target point of the robot arc additive trajectory.

[0094] The program formats of different robots are slightly different depending on the robot selected, but they all contain the TCP position and posture values ​​at the end of the robot welding gun.

[0095] In some embodiments, in step S600, the failed roll forging die to be repaired is installed on a rotary positioner, the outer axis of the roll forging die is kept coincident with the rotation axis of the positioner, the workpiece coordinate system of the robot arc welding additive system is calibrated by a three-point positioning method, and the Z axis of the workpiece coordinate system is ensured to coincide with the outer axis of the roll forging die, and the X axis is in the plane of one end of the roll forging die. The end face of the roll forging die on the positioner is manually controlled to rotate to a 90° vertical plane, and the current angle of the positioner on the robot teaching pendant is recorded. The rotation angle of the rotary positioner is calculated according to the coordinate value of the curved surface additive trajectory point and the current angle of the positioner. The rotation angle calculation formula of the rotary positioner is:

[0096] β=α+|arctan2(yi / xi)|,

[0097] Among them, β is the rotation angle of the positioner, α is the current angle of the positioner, yi is the coordinate of the ith trajectory point in the Y direction, and xi is the coordinate of the ith trajectory point in the X direction. The rotation angle of the positioner can ensure that the molten pool at the current additive position is always in a horizontal position, avoiding the problem of unstable flow caused by the gravity drag on the inclined or vertical surface during traditional curved additive manufacturing, thereby improving the forming quality.

[0098] The arc additive manufacturing of curved surface of robot roll forging die includes at least a six-degree-of-freedom arc welding robot, a one-degree-of-freedom rotation positioner, an arc welding power source, and a welding protection bottle assembly.

[0099] In some embodiments, in step S700, the failed roll forging die needs to be preheated in a heating furnace at a temperature of 500° C. for 5 hours before being installed on the positioner; the TCP position and posture of the robot welding gun end and the rotation angle of the rotary positioner are filled into the external axis control corresponding area of ​​the robot program instruction, and the generated robot program is imported into the robot controller;

[0100] The robot controller adjusts the welding power wire feeding speed, welding voltage, and robot welding speed to ensure that the single layer thickness is H during additive forming. After starting the robot welding program, the positioner rotates with the failed roller forging die. The robot controls the welding gun to move to the top of the failed roller forging die and starts additive forming. During the rotation of the positioner, the molten pool is always kept in a horizontal position.

[0101] After each layer of additive material is added, the robot is paused to check the thickness of the additive layer. The thickness of the additive layer should be consistent with the thickness of the curved layer. The inspection will be paused at the end of each layer of additive material. When the actual additive layer thickness is greater than the curved layer thickness, the robot welding speed will be appropriately increased during the additive process of the next layer; when the actual additive layer thickness is less than the curved layer thickness, the robot welding speed will be appropriately reduced during the additive process of the next layer. At the end of each layer of additive material, the weld layer will be manually struck with a hammer or pneumatic pick to clean the welding slag and reduce residual stress.

[0102] After the entire failed roll forging die additive repair and remanufacturing is completed, the room temperature is controlled first, and then it is transferred to a heating furnace for tempering heat treatment. The tempering temperature is 550 degrees Celsius and the insulation time is 7 hours. After the insulation is completed, the furnace is cooled to room temperature and removed. Subsequently, the cavity is precisely milled on a horizontal milling machine to remove the additive processing allowance, and finally the additive repair of the failed roll forging die is completed.

[0103] like Figure 5 As shown, based on the arc additive manufacturing method for curved surface of a robot roll forging die, the present invention also provides an electronic device, which can be a computing device such as a mobile terminal, a desktop computer, a notebook, a palm computer, and a server. The electronic device includes a processor 10, a memory 20, and a display 30. Figure 5 Only some components of the electronic device are shown, but it should be understood that it is not required to implement all of the components shown, and more or fewer components may be implemented instead.

[0104] In some embodiments, the memory 20 may be an internal storage unit of the electronic device, such as a hard disk or memory of the electronic device. In other embodiments, the memory 20 may also be an external storage device of the electronic device, such as a plug-in hard disk, a smart memory card (Smart Media Card, SMC), a secure digital (Secure Digital, SD) card, a flash card (Flash Card), etc. equipped on the electronic device. Further, the memory 20 may also include both an internal storage unit of the electronic device and an external storage device. The memory 20 is used to store application software and various types of data installed in the electronic device, such as program codes for installing the electronic device. The memory 20 may also be used to temporarily store data that has been output or is to be output. In one embodiment, a robot roll forging die curved surface arc additive manufacturing program 40 is stored on the memory 20, and the robot roll forging die curved surface arc additive manufacturing program 40 can be executed by the processor 10, thereby realizing the robot roll forging die curved surface arc additive manufacturing method of each embodiment of the present invention.

[0105] In some embodiments, the processor 10 may be a central processing unit (CPU), a microprocessor or other data processing chip, used to run program codes or process data stored in the memory 20, such as a robot roll forging die curved surface arc additive manufacturing method, etc.

[0106] In some embodiments, the display 30 may be an LED display, a liquid crystal display, a touch-sensitive liquid crystal display, an OLED (Organic Light-Emitting Diode) touch device, etc. The display 30 is used to display information on the arc additive manufacturing of the curved surface of the robot roll forging die and to display a visual user interface. The components 10-30 of the electronic device communicate with each other via a system bus.

[0107] In some embodiments, when the processor 10 executes the robotic roll forging die curved surface arc additive manufacturing program 40 in the memory 20, the various steps in the robotic roll forging die curved surface arc additive manufacturing method described in the above embodiments are implemented. Since the robotic roll forging die curved surface arc additive manufacturing method has been described in detail above, it will not be repeated here.

[0108] In summary, the robot roll forging die curved surface arc additive manufacturing method, equipment and medium provided by the present invention first obtain the scanning result of the failed roll forging die to obtain the three-dimensional STL model of the defective surface of the failed roll forging die; based on the three-dimensional STL model of the defective surface of the failed roll forging die, the defective NURBS surface, the additive entity and the additive repair residual surface are determined, and based on the defective NURBS surface, the additive entity and the additive repair residual surface, the three-dimensional solid STL of the defective area to be repaired is obtained; based on the three-dimensional solid STL of the defective area to be repaired, after establishing the offset surface group of the failed roll forging die, based on the three-dimensional solid STL of the defective area to be repaired and the offset surface group, the corresponding Intersecting cutting surface group; determining the trajectory file by performing trajectory planning on the intersecting cutting surface group; secondly, generating the robot arc additive trajectory file based on the trajectory file, determining the TCP posture and position of the robot welding gun end based on the robot arc additive trajectory file; determining the current angle of the rotary positioner on which the failed roller forging die is installed, and calculating the rotation angle of the rotary positioner based on the robot arc additive trajectory file and the current angle of the positioner; finally, based on the TCP posture and position of the robot welding gun end and the rotation angle of the rotary positioner, controlling the coordinated action of the robot welding gun and the positioner to complete the additive repair of the failed roller forging die; improving the additive repair forming quality.

[0109] Of course, those skilled in the art can understand that all or part of the processes in the above-mentioned embodiments can be implemented by instructing related hardware (such as a processor, a controller, etc.) through a computer program, and the program can be stored in a computer-readable storage medium, and the program can include the processes of the above-mentioned method embodiments when executed. The storage medium can be a memory, a disk, an optical disk, etc.

[0110] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for arc additive manufacturing of curved surface of a robot roll forging die, characterized in that: The steps include: Obtaining the scanning result of the failed roller forging die to obtain a three-dimensional STL model of the defective surface of the failed roller forging die; Based on the three-dimensional STL model of the defective surface of the failed roll forging die, the defective NURBS surface, the additive solid and the additive repair margin surface are determined, and based on the defective NURBS surface, the additive solid and the additive repair margin surface, the three-dimensional solid STL of the defective area to be repaired is obtained; After establishing the offset surface group of the failed roll forging die based on the three-dimensional solid STL of the defective area to be repaired, determining the intersecting cutting surface group based on the three-dimensional solid STL of the defective area to be repaired and the offset surface group; Performing trajectory planning on the intersecting cutting surface group and determining a trajectory file; After generating a robot arc additive trajectory file based on the trajectory file, determining the TCP posture and position of the robot welding gun end based on the robot arc additive trajectory file; Determine the current angle of the rotary positioner on which the failed roll forging die is installed, and calculate the rotation angle of the rotary positioner based on the robot arc additive trajectory file and the current angle of the positioner, wherein the rotation angle calculation formula of the rotary positioner is: β=α+|arctan2(yi / xi)|, Among them, β is the rotation angle of the positioner, α is the current angle of the positioner, yi is the coordinate of the i-th track point in the Y direction, and xi is the coordinate of the i-th track point in the X direction; Based on the TCP posture and position of the robot welding gun end and the rotation angle of the rotary positioner, the robot welding gun and the positioner are controlled to cooperate to complete the additive repair of the failed roll forging die.

2. The arc additive manufacturing method for curved surface of a robot roll forging die according to claim 1, characterized in that: The method of determining a defective NURBS surface, an additive entity, and an additive repair margin based on the defective NURBS surface, the additive entity, and the additive repair margin, and obtaining a three-dimensional solid STL of the defective area to be repaired based on the defective NURBS surface, the additive entity, and the additive repair margin, comprises: After aligning the three-dimensional STL model of the defective surface of the failed roll forging die with the precise CAD digital model coordinates, the three-dimensional STL model of the defective surface of the failed roll forging die is processed into a NURBS grid surface to obtain a defective NURBS surface; Importing the defective NURBS surface and the precise CAD digital model into the three-dimensional modeling software to determine the entity of the additive area; Obtaining a precise CAD surface of the forging die, and offsetting the precise CAD surface of the forging die outward to obtain an additive repair margin curved surface; The additive area entity is subjected to Boolean subtraction with the defective NURBS surface and the additive repair margin surface to obtain a three-dimensional solid STL of the defective area to be repaired.

3. The arc additive manufacturing method for curved surface of a robot roll forging die according to claim 2, characterized in that: After establishing the offset surface group of the failed roll forging die based on the three-dimensional solid STL of the defective area to be repaired, determining the intersecting cutting surface group based on the three-dimensional solid STL of the defective area to be repaired and the offset surface group, including: Based on the three-dimensional solid STL of the defective area to be repaired, a cylindrical surface is drawn and the maximum radial depth of the three-dimensional solid of the defective area to be repaired is calculated; Presetting the thickness of each layer during additive repair, based on the maximum depth and the thickness of each layer, offsetting the cylindrical surface inwards, and establishing an offset curved surface group of the failed roll forging die; The offset curved surface group is intersected with the three-dimensional solid STL of the defective area to be repaired to obtain an intersecting cutting surface group of the failed roll forging die.

4. The arc additive manufacturing method for curved surface of a robot roll forging die according to claim 3, characterized in that: The calculation formula for the intersecting cutting surface group is: ∑’ N+1 ={SF’,SF1’,SF2’,SF3’,…,SFN’}, ∑ N+1 ={SF,SF1,SF2,SF3,…,SFN}, N=D / H-1, Among them, ∑' N+1 is the intersecting cutting face group, ∑ N+1 is the offset surface group, SF is the cylindrical surface, N is the number of times the cylindrical surface SF is offset inward, D is the maximum radial depth of the three-dimensional entity in the defect area to be repaired, and H is the thickness of each layer during layer-by-layer additive repair.

5. The method for manufacturing curved surface of a robot roll forging die by arc additive manufacturing according to claim 3, characterized in that: The performing trajectory planning on the intersecting cutting surface group and determining the trajectory file comprises: Performing trajectory planning on the intersecting cutting surface group to determine the trajectory mode, the distance between adjacent trajectories, the trajectory direction and the axis of each trajectory spot welding gun; Based on the trajectory mode, adjacent trajectories, trajectory direction and the spot welding gun axis of each trajectory, a trajectory file is determined.

6. The arc additive manufacturing method for curved surface of a robot roll forging die according to claim 5, characterized in that: The trajectory file at least includes the position and posture of each trajectory point. The position and posture calculation formula of the trajectory point are as follows: Pi=[xi,yi,zi], Si=[xi,yi,zi,ui,0,wi], Where Pi is the position of the trajectory point, xi is the coordinate of the ith trajectory point in the X direction, yi is the coordinate of the ith trajectory point in the Y direction, and zi is the coordinate of the ith trajectory point in the Z direction; Si is the posture of the ith trajectory point, ui is the X direction component, 0 is the Y direction component, and wi is the Z direction component.

7. The arc additive manufacturing method for curved surface of a robot roll forging die according to claim 6, characterized in that: Determining the TCP posture and position of the robot welding gun end based on the robot arc additive trajectory file includes: Establishing a welding gun end TCP posture rotation matrix, and calculating the welding gun end TCP posture quaternion based on the welding gun end TCP posture rotation matrix; Based on the position of the trajectory point and the TCP posture quaternion of the welding gun end, the target point of the robot arc additive trajectory is determined.

8. An electronic device, characterized in that: include: Processor and memory; The memory stores a computer-readable program executable by the processor; When the processor executes the computer-readable program, the steps in the robot roll forging die curved surface arc additive manufacturing method as described in any one of claims 1 to 7 are implemented.

9. A computer-readable storage medium, characterized in that: The computer-readable storage medium stores one or more programs, and the one or more programs can be executed by one or more processors to implement the steps in the robot roll forging die curved surface arc additive manufacturing method as described in any one of claims 1-7.

Citation Information

Patent Citations

  • 3D printing method and system for complicated parts based on curved surface layering

    CN107187056A

  • Repairing system and repairing method for defects of complex curved parts

    CN108274187A

  • Arc fuse curved surface additive posture modeling method and control method

    CN111037054A

  • Direct layering method for laser additive repair

    CN111859577A

  • Shape following-up gradient additive remanufacturing method for complex surface of hot-forging die cavity