Preparation method of narrow-band blue light Cu-Ga-S / ZnS nanocrystals
Cu-Ga-S/ZnS nanocrystals are prepared by the hot injection method and a ZnS shell is formed, which solves the problem of large full-width half-peak photoluminescence of copper-based I-III-VI nanocrystals and achieves narrow-band blue light emission. , suitable for electroluminescent devices with high color purity, and overcomes environmental and health hazards, and the materials are safe, cheap and easy to obtain.
Patent Information
- Application Number
- CN202310858144.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-07-13
AI Technical Summary
The application of existing copper-based I-III-VI semiconductor nanocrystals in the field of blue light is limited by the large half-maximum photoluminescence width, environmental and health hazards, and difficulty in achieving narrow-band emission.
The hot injection method is used to prepare Cu-Ga-S/ZnS nanocrystals. By forming a ZnS shell to coat the Cu-Ga-S quantum dots, a narrow band of photoluminescence peak at 470-480nm is achieved, and the full width at half maximum is less than 50nm.
It has achieved narrow-band luminescence of cadmium-free Cu-based I-III-VI quantum dots, with excellent crystallinity, dispersion and luminescence characteristics. It is suitable for electroluminescent devices with high color purity. The material is safe, cheap and easy to obtain. Suitable for industrial production.
Smart Images

Figure CN116891738B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of quantum dot synthesis, and in particular to a method for preparing a blue narrow-band Cu-Ga-S / ZnS luminescent quantum dot having a photoluminescence half-maximum full width of less than 50nm and a fluorescence luminescence peak at 470-480nm. Background Art
[0002] Light-emitting semiconductor nanocrystals (or quantum dots) are quasi-zero-dimensional nanomaterials, usually with all three dimensions between 1 and 10 nanometers. Nanocrystals exhibit unique physical and chemical properties due to their own quantum confinement effects and are widely used in the field of light-emitting devices.
[0003] The luminescent materials used in the electroluminescent devices of semiconductor quantum dots are mainly cadmium-based chalcogenide nanocrystals. However, heavy metal elements such as cadmium are harmful to the environment and human body. In comparison, I-III-VI semiconductor nanocrystals are more environmentally friendly and less harmful to the environment and human body.
[0004] Nanocrystalline materials used in electroluminescent devices need to have high color purity, that is, a narrow photoluminescence half-maximum full width. However, traditional copper-based I-III-VI semiconductor nanocrystals have a large number of defect states, and the hybridization of Cu compounds near the top of the valence band is more likely to split into multiple sub-bands. CGS quantum dots are more difficult to achieve narrow-band emission, and their photoluminescence half-maximum full width (FWHM) is generally large, which limits the application of copper-based I-III-VI semiconductor nanocrystals in the display field.
[0005] At present, the research on I-III-VI semiconductor nanocrystal light-emitting devices is mainly in the range of red to green light, because its Stokes shift is large, and there is less research in the blue light field, which is not conducive to the full-spectrum emission of I-III-VI semiconductor nanocrystals. Therefore, it is very necessary to develop an environmentally friendly and excellent optoelectronic performance blue light narrow-band semiconductor nanocrystal. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing Cu-Ga-S / ZnS-based blue light narrow-band nanocrystals, to achieve the synthesis of cadmium-free Cu-based I-III-VI group quantum dots with a photoluminescence full width at half maximum (FWHM) of less than 50 nm, to construct quantum dot light-emitting diodes to achieve narrow-spectrum electroluminescent devices with a full width at half maximum (FWHM) of less than 50 nm, so as to solve at least one technical problem existing in the above-mentioned background technology.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The invention provides a method for preparing narrow-band blue light Cu-Ga-S / ZnS nanocrystals, comprising: preparing narrow-band blue light Cu-Ga-S / ZnS nanocrystals based on a hot injection method, wherein the chemicals used in the preparation are metal salts of group IB and group IIIA and single substances and compounds of group VIA; the full width at half maximum of a photoluminescence spectrum is less than 50nm, and the photoluminescence peak is located at 470-480nm.
[0009] Further, the preparation steps include:
[0010] Weighing Cu source, Ga source, S source and solvent and mixing with ligand as nucleation precursor solution, vacuum degassing, stirring and dissolving, and then passing nitrogen to keep warm for use;
[0011] Weigh the Zn source and the solvent and mix them with the ligand as a zinc precursor solution, vacuum degas and stir to dissolve, then introduce nitrogen to keep warm for later use.
[0012] injecting a zinc precursor solution into a nucleation precursor solution, maintaining the temperature, and subsequently increasing the temperature and maintaining the temperature;
[0013] After the reaction product is cooled, isopropanol is added to the reaction product solution, centrifuged and the precipitate is separated, n-hexane is added to the precipitate to completely dissolve it, and then ethanol is added to completely precipitate it, and this is repeated several times to obtain narrow-band luminescent quantum dots.
[0014] Further, the Cu source, Ga source, S source, solvent and ligand are weighed, the Cu source is a Group IB metal salt including but not limited to cuprous chloride, cuprous bromide, cuprous iodide, cuprous acetate, cuprous acetylacetonate, and the Ga source is a Group IIIA metal salt including but not limited to gallium acetylacetonate and gallium chloride.
[0015] Further, the Cu source, Ga source, S source, solvent and ligand are weighed, and the ligand includes but is not limited to n-dodecanethiol and n-decanethiol.
[0016] Further, the Cu source, Ga source, S source, solvent and ligand are weighed, and the solvent includes but is not limited to oleic acid, oleylamine, octadecylamine and 1-octadecene.
[0017] Furthermore, the molar ratio of copper, gallium and sulfur precursors is 1:(30-40):(30-40); 6-8 mL of solvent is added for every 1 mmol of gallium source; 1.5-2 mL of ligand is added for every 1 mmol of gallium source; the vacuum degassing temperature is 80-120°C; the stirring time is 30-50 minutes; then the temperature is raised to 260°C-280°C at a rate of 10°C / min; and the insulation time is 10-20 minutes.
[0018] Furthermore, the weighed Zn source and solvent are mixed with the ligand, and the zinc source includes but is not limited to zinc stearate, anhydrous zinc acetate, and anhydrous zinc halide.
[0019] Furthermore, the weighed Zn source and solvent are mixed with the ligand, and the solvent includes but is not limited to oleic acid, oleylamine, octadecylamine, and 1-octadecene.
[0020] Furthermore, the ligand includes but is not limited to n-dodecanethiol and n-decanethiol; the volume ratio of the solvent to the ligand is (9-10):2; 0.5-0.7 mL of the ligand is added for every 1 mmol of zinc source; the heating temperature is 120-150° C.; and the insulation time is 30-40 min.
[0021] Furthermore, when the zinc precursor solution is injected into the nucleation precursor solution, the system is kept at 210°C to 230°C for 15 to 20 minutes; then the temperature is raised to 250°C at a rate of 10°C / min for 30 to 120 minutes.
[0022] The invention has the following beneficial effects: after the Cu-Ga-S nanocrystals are coated with a ZnS shell layer, a gradient-distributed zinc-rich alloy structure is formed on the surface of the quantum dots, an obvious narrow-band photoluminescence peak appears at 470-480nm, and the full width at half maximum is 36-46nm, achieving a narrow-band luminescence characteristic, and having the prospect of constructing an electroluminescent device; it has excellent crystallinity, dispersibility and luminescence characteristics, and can be used as a light-emitting layer to construct an electroluminescent diode, so as to obtain a cadmium-free QLED device with high color purity; the synthesis method is simple, the materials are cheap and easily available, the raw materials are non-toxic and harmless, the reaction time is short, and it is convenient for industrial mass production.
[0023] Additional advantages of the present invention will be more clearly given in the following description or learned through the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0025] Figure 1 These are the UV-visible fluorescence spectrum and UV-visible absorption spectrum of the Cu-Ga-S / ZnS nanocrystals prepared as described in the embodiments of the present invention.
[0026] Figure 2 This is the XRD diffraction spectrum of the Cu-Ga-S / ZnS nanocrystal product described in the embodiment of the present invention.
[0027] Figure 3 This is a transmission electron microscope photograph of the Cu-Ga-S / ZnS nanocrystal product described in the embodiment of the present invention. DETAILED DESCRIPTION
[0028] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below by the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention.
[0029] It should be understood by those skilled in the art that unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those skilled in the art to which this invention belongs.
[0030] It should also be understood that terms, such as those defined in commonly used dictionaries, should be understood to have a meaning consistent with that in the context of the prior art and will not be interpreted in an idealized or overly formal sense unless as defined herein.
[0031] Those skilled in the art will appreciate that, unless otherwise stated, the singular forms "a", "an", "said" and "the" used herein may also include plural forms. It should be further understood that the term "comprising" used in the specification of the present invention refers to the presence of the features, integers, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements and / or groups thereof.
[0032] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory.
[0033] To facilitate understanding of the present invention, the present invention is further explained below with reference to specific embodiments in conjunction with the accompanying drawings, and the specific embodiments do not constitute a limitation on the embodiments of the present invention.
[0034] Those skilled in the art should understand that the drawings are merely schematic diagrams of embodiments, and the components in the drawings are not necessarily necessary for implementing the present invention.
[0035] Example 1
[0036] In this embodiment 1, a method for synthesizing Cu-Ga-S / ZnS-based blue light narrow-band nanocrystals is provided to achieve the synthesis of cadmium-free Cu-based I-III-VI group quantum dots with a photoluminescence full width at half maximum (FWHM) of less than 50 nm, and to construct quantum dot light-emitting diodes to achieve narrow-spectrum electroluminescent devices with a full width at half maximum (FWHM) of less than 50 nm.
[0037] In this embodiment, the synthesis method of the Cu-Ga-S / ZnS-based blue light narrow band nanocrystals comprises the following steps:
[0038] Step 1: Weigh cuprous chloride, gallium chloride and sulfur powder, mix them evenly and dissolve them in a mixed solution of oleylamine, oleic acid, 1-octadecene and n-dodecyl mercaptan, and transfer them into a three-necked flask as a nucleation precursor solution.
[0039] The molar ratio of cuprous chloride, gallium chloride and sulfur powder is 1:40:40; the volume ratio of oleylamine, oleic acid, 1-octadecene and n-dodecyl mercaptan is 4:1:2:2; and the cuprous chloride concentration of the control system is 0.0025-0.003 mol / L.
[0040] Step 2: Weigh anhydrous zinc acetate and dissolve it in a mixed solution of oleylamine, oleic acid, 1-octadecene and n-dodecyl mercaptan, and transfer the mixture into a three-necked flask as a zinc precursor solution.
[0041] The volume ratio of oleylamine, oleic acid, 1-octadecene and n-dodecyl mercaptan is 2:1:6:2; the concentration of anhydrous zinc acetate in the control system is 0.36-0.37 mol / L. The molar ratio of gallium chloride in step 1 to anhydrous zinc acetate in step 2 is 1:4.
[0042] Step 3: Degas the nucleation precursor solution at 120°C for 20 min under magnetic stirring, introduce nitrogen protection, and heat to 270°C at a rate of 10°C / min and keep warm for 15 min.
[0043] Step 4: Degas the zinc precursor solution at 150°C for 40 min under magnetic stirring and then introduce nitrogen protection.
[0044] Step 5: Draw out the zinc precursor solution with a syringe and quickly inject it into the nucleation solution.
[0045] Step 6: After the injection is completed, keep warm at 230°C for 15 minutes.
[0046] Step 7: Heat to 250°C at a rate of 10°C / min and keep at this temperature for 45 minutes.
[0047] Step 8: After the reaction product in step 7 is cooled, add 3 times the volume of isopropanol to the reaction product solution to precipitate quantum dots, then centrifuge at 9000r / min for 5min, pour out the supernatant, and keep the precipitate. The obtained precipitate is dissolved with a small amount of n-hexane, and then add ethanol to precipitate completely. Centrifuge the precipitate more than three times to obtain narrow-band Cu-Ga-S / ZnS nanocrystals.
[0048] Example 2
[0049] In this embodiment 2, a method for preparing Cu-Ga-S / ZnS narrow-band luminescent nanocrystals is provided, comprising the following steps:
[0050] Weigh cuprous chloride, gallium chloride, and sulfur powder, dissolve them in a mixed solution of oleylamine, oleic acid, 1-octadecene, and n-dodecyl mercaptan, and transfer them into a three-necked flask as a nucleation precursor solution. The amount of cuprous chloride added is 0.05 mmol, the amount of gallium chloride added is 2 mmol, the amount of sulfur powder added is 2 mmol, the volume ratio of oleylamine, oleic acid, 1-octadecene, and n-dodecyl mercaptan is 4:1:2:2, and the total volume is 18 mL.
[0051] Weigh anhydrous zinc acetate and dissolve it in a mixed solution of oleylamine, oleic acid, 1-octadecene, and n-dodecyl mercaptan, and transfer it into a three-necked flask as a zinc precursor solution. The amount of anhydrous zinc acetate added is 8 mmol; the volume ratio of oleylamine, oleic acid, 1-octadecene, and n-dodecyl mercaptan is 2:1:6:2, and the total volume is 22 mL.
[0052] The nucleation precursor solution was degassed at 120°C for 20 min, nitrogen was introduced for protection, and the temperature was raised to 270°C at a rate of 10°C / min under magnetic stirring and kept for 15 min.
[0053] The zinc precursor solution was degassed at 150° C. for 40 min, nitrogen was introduced for protection, and the solution was kept warm under magnetic stirring for later use.
[0054] After the reaction of the nucleation precursor solution is completed, the zinc precursor solution is directly injected into the nucleation precursor solution by hot injection. After injection, the reaction is carried out at 230°C for 15 minutes. Then, the temperature is increased to 250°C at a rate of 10°C / min and kept at this temperature for 45 minutes.
[0055] After the reaction product is cooled, five times the volume of isopropanol is added to the reaction product solution to precipitate quantum dots, and then centrifuged at 9000r / min for 5 minutes. After the centrifugation is completed, the supernatant is poured out, leaving the precipitate, the obtained precipitate is dissolved with a small amount of n-hexane, and then ethanol is added until it is completely precipitated, and centrifuged at 9000r / min for 5 minutes to leave the precipitate, and the centrifugation is repeated 5 times to obtain Cu-Ga-S / ZnS nanocrystals with narrow-band luminescence characteristics.
[0056] like Figure 1As shown in the figure, the peak of Cu-Ga-S / ZnS nanocrystals is at 470nm, the full width at half maximum is 36nm, and it has good color purity. Figure 2 As shown in the figure, Cu-Ga-S / ZnS nanocrystals match the cubic ZnS and tetragonal CuGaS2 crystal phases. Figure 3 As shown, the Cu-Ga-S / ZnS nanocrystals have uniform size distribution, a size of 4.5 nm, and good crystallinity.
[0057] In summary, the method of nanocrystals described in the embodiment of the present invention effectively overcomes the disadvantage that the full width at half maximum (FWMH) of the photoluminescence spectrum of copper-based I-III-VI group nanocrystals is generally large, and obtains cadmium-free I-III-VI group semiconductor nanocrystals with a FWHM of less than 50nm. The growth process and photoluminescence performance of narrow-band luminescent quantum dots of copper-based I-III-VI group semiconductor nanocrystals are mainly studied by hot injection method. After the Cu-Ga-S nanocrystals are coated with ZnS shells, a gradient-distributed zinc-rich alloy structure is formed on the surface of the quantum dots, and an obvious narrow-band photoluminescence peak appears at 470-480nm, with a full width at half maximum of 36-46nm, achieving narrow-band luminescence characteristics, and having the prospect of constructing electroluminescent devices. The product was structurally analyzed using X-ray diffractometer (XRD), transmission electron microscope (TEM), ultraviolet-visible fluorescence spectrum (UV-Vis Spectra), etc., showing excellent crystallinity, dispersibility and luminescence characteristics. Using this material as the light-emitting layer to construct an electroluminescent diode, a cadmium-free QLED device with high color purity can be obtained. The synthesis method of this process is simple, the materials are cheap and easy to obtain, the raw materials are non-toxic and harmless, the reaction time is short, and it is easy to industrialize and mass produce.
[0058] Although the above describes the specific implementation mode of the present invention in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art without creative work on the basis of the technical solution disclosed in the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing narrow-band blue light Cu-Ga-S / ZnS nanocrystals, characterized in that: include: Preparation of narrow-band blue-light Cu-Ga-S / ZnS nanocrystals based on hot injection method; The full width at half maximum of the photoluminescence spectrum is less than 50 nm, and the photoluminescence peak is located at 470-480 nm; The steps for preparing the narrow-band blue light Cu-Ga-S / ZnS nanocrystals include: Weighing a Cu source, a Ga source, a S source and a solvent and mixing them with a ligand as a nucleation precursor solution, vacuum degassing, stirring and dissolving, and then introducing nitrogen to keep warm for standby use; wherein the ligand includes n-dodecyl mercaptan, n-decapryl mercaptan or n-octyl mercaptan; the solvent includes oleic acid, oleylamine or 1-octadecene; the molar ratio of copper, gallium and sulfur precursor is 1:(30-40):(30-40); Weigh a Zn source and a solvent and mix them with a ligand as a zinc precursor solution, vacuum degas and stir to dissolve, then introduce nitrogen to keep warm for standby use; wherein the ligand includes n-dodecyl mercaptan or n-decathic acid; the volume ratio of the solvent to the ligand is (9-10):2; 0.5-0.7 mL of the ligand is added for every 1 mmol of the zinc source; the heating temperature is 120-150° C.; and the insulation time is 30-40 min; injecting a zinc precursor solution into a nucleation precursor solution, maintaining the temperature, and subsequently increasing the temperature and maintaining the temperature; After the reaction product is cooled, isopropanol is added to the reaction product solution, centrifuged and the precipitate is separated, n-hexane is added to the precipitate to completely dissolve it, and then ethanol is added to completely precipitate it, and this is repeated several times to obtain narrow-band luminescent quantum dots.
2. The method for preparing narrow-band blue light Cu-Ga-S / ZnS nanocrystals according to claim 1, characterized in that: The Cu source, Ga source, S source, solvent and ligand are weighed, wherein the Cu source includes cuprous chloride, cuprous bromide, cuprous iodide, cuprous acetate or cuprous acetylacetonate, and the Ga source includes gallium acetylacetonate or gallium chloride.
3. The method for preparing narrow-band blue light Cu-Ga-S / ZnS nanocrystals according to claim 1, characterized in that: For every 1 mmol of gallium source, 6 to 8 mL of solvent is added; for every 1 mmol of gallium source, 1.5 to 2 mL of ligand is added; the vacuum degassing temperature is 80 to 120° C.; the stirring time is 30 to 50 minutes; then the temperature is raised to 260° C. to 280° C. at a speed of 10° C. / min; and the heat preservation time is 10 to 20 minutes.
4. The method for preparing narrow-band blue light Cu-Ga-S / ZnS nanocrystals according to claim 1, characterized in that: The weighed Zn source and solvent are mixed with the ligand, and the zinc source includes zinc stearate, anhydrous zinc acetate or anhydrous zinc halide.
5. The method for preparing narrow-band blue light Cu-Ga-S / ZnS nanocrystals according to claim 4, characterized in that: The weighed Zn source and solvent are mixed with the ligand, and the solvent includes oleic acid, oleylamine or 1-octadecene.
6. The method for preparing narrow-band blue light Cu-Ga-S / ZnS nanocrystals according to claim 1, characterized in that: When the zinc precursor solution is injected into the nucleation precursor solution, the system is kept at 210°C to 230°C for 15 to 20 minutes; then the temperature is raised to 250°C at a rate of 10°C / min for 30 to 120 minutes.
Citation Information
Patent Citations
CuGaS-ZnS core-shell structure quantum-dot material and preparation method thereof
CN107384371A
Core-shell structured quantum dots, preparation method thereof and polarizing film
CN109233802A