A nylon porous membrane for virus pre-filtration and its preparation method
By controlling parameters such as pore size, crystallinity, and hydrophobicity of nylon porous membranes, non-directional tortuous pathway nylon porous membranes were prepared, solving the problem of poor protein aggregate retention in the virus pre-filtration process of nylon membranes, and achieving efficient protein aggregate removal and improved membrane durability.
Patent Information
- Application Number
- CN202310910551.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-07-24
AI Technical Summary
In the pre-filtration process for viruses, existing nylon membranes have difficulty maintaining optimal levels of protein aggregate retention, adsorption capacity, and filtration efficiency, and are prone to membrane clogging, affecting the durability and efficiency of the filter.
By controlling parameters such as pore size, crystallinity, hydrophobicity, and crystal form of nylon porous membranes, nylon porous membranes with non-directional tortuous pathways were prepared, thereby improving their binding capacity and removal efficiency for protein aggregates.
It enhances the adsorption and retention effect of nylon membranes on protein aggregates, improves the removal rate of protein aggregates in the filtered biological feed liquid, reduces the risk of membrane clogging, and improves the service life and efficiency of the filter.
Smart Images

Figure CN116943428B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nylon membranes, and more specifically, to a porous nylon membrane for virus pre-filtration and a method for preparing the same. Background Technology
[0002] Protein solutions derived from plasma, cell cultures, tissue extracts, secretions, and synthetic proteins inevitably contain not only low-molecular-weight proteins such as required immunoglobulins (IgG) or monoclonal antibodies, but also high-molecular-weight proteins such as protein trimers or polymers. These high-molecular-weight protein aggregates are toxic and, when used in patient treatment, are easily perceived as foreign substances, triggering an immune system reaction; or causing abnormal cell function and death, affecting organ function and the central nervous system. Therefore, it is essential to remove these protein aggregates to avoid adverse reactions in patients.
[0003] Secondly, protein aggregates are typically larger than the pore size of the membrane used for virus removal filtration. Even when they enter the protein solution before virus removal filtration at the end of the purification process, although most protein aggregates have been removed in the previous purification steps, small protein molecules such as antibody proteins may still fold and aggregate in solution to form protein dimers, trimers, etc. These aggregates can easily clog the virus removal filter. Even at low aggregate concentrations of 0.01-0.1%, the virus removal filter will be rapidly clogged, resulting in a decrease in the virus removal filtration efficiency and a reduction in the durability of the virus removal filter.
[0004] Traditional methods for removing protein aggregates from protein solutions include gel chromatography, size exclusion chromatography, or ultrafiltration, all of which are relatively expensive.
[0005] Sartorius Inc.’s US Patent No. 10987629B2 discloses a method for removing biopolymer aggregates and small virus particles from a fluid. Step (a) involves filtering a fluid containing biopolymer aggregates and small virus particles through a porous polyamide shape body made of nylon-6. The porous polyamide shape body has internal and external surface regions and is configured such that all internal and external surface regions have the same chemical properties. Filtering the fluid containing biopolymer aggregates and small virus particles through the porous polyamide shape body allows the biopolymer aggregates to be selectively removed from the fluid by adsorption, while the small virus particles permeate through the shape body in the fluid in which the biopolymer aggregates have been removed.
[0006] The above method discloses that nylon-6 can adsorb and remove protein aggregates in fluids through its own chemical properties. The adsorption of protein aggregates by the nylon membrane is mainly manifested by hydrophobic interactions. Although nylon itself is a hydrophilic material, hydrophobic groups are exposed on the pore surface of the nylon membrane, which causes the nylon membrane to locally adsorb protein aggregates in the fluid during fluid filtration, thereby achieving the retention effect of protein aggregates.
[0007] However, the inventors of this invention have discovered that when nylon membranes are used for virus pre-filtration, improving the protein aggregate retention effect, adsorption capacity, and filtration efficiency of nylon membranes is a problem that urgently needs to be solved.
[0008] Although nylon membranes can adsorb impurities through hydrophobic adsorption, as disclosed in the aforementioned patent, not all nylon membranes can achieve the expected results when used for virus pre-filtration.
[0009] The adsorption and retention of protein aggregates by nylon membranes mainly occurs through hydrophobic interactions between the exposed hydrophobic groups on the pore surface of the nylon membrane and the protein aggregates in the filtered stream. While nylon membranes can retain protein aggregates larger than the pore size through a pore sieving mechanism, the filtered stream typically also contains very small protein dimers and trimers. These dimers and trimers are not easily retained by the pores and are primarily adsorbed and retained through hydrophobic interactions.
[0010] However, when the hydrophobic adsorption between the nylon membrane and the protein aggregates reaches saturation or the hydrophobic adsorption strength of the nylon membrane is low, impurities such as protein dimers and trimers in the filtered fluid passing through the nylon membrane can easily penetrate the nylon membrane and enter the downstream end of the filtered fluid, which can easily lead to an undesirable high concentration of impurities at the downstream end of the nylon membrane.
[0011] A key challenge is developing nylon membranes that can be better suited for virus pre-filtration. When conventional nylon membranes are used for virus pre-filtration, it is difficult to maintain optimal levels of protein aggregate adsorption capacity, efficiency, and rejection rate. Summary of the Invention
[0012] To address the problems existing in the prior art, the present invention aims to provide a nylon porous membrane for virus pre-filtration and its preparation method.
[0013] To achieve the above objectives, the present invention provides the following technical solution:
[0014] A nylon porous membrane for virus pre-filtration, wherein the nylon porous membrane has non-directional tortuous pathways, one side surface of the nylon porous membrane is a first side surface having a plurality of first pores, and the other side surface of the nylon porous membrane is a second side surface having a plurality of second pores.
[0015] The average pore size (PMI) of the nylon porous membrane is 0.05–1 μm.
[0016] The nylon porous membrane has a binding capacity of 30–100 μg / cm³ for IvIg protein at its isoelectric point. 2 ;
[0017] The saturated saline contact angle on the first side of the nylon porous membrane is 80-130°.
[0018] The crystallinity of the nylon porous membrane was measured by XRD, and the crystallinity of the nylon porous membrane was 40-90%.
[0019] This invention controls the binding amount of IvIg protein in the nylon membrane and the crystallinity of the nylon membrane within the range described in this invention, so as to obtain a nylon membrane with good binding ability to protein aggregates and high removal efficiency, while taking into account other properties of the nylon membrane, such as flux, flow rate, and loading capacity.
[0020] IvIg proteins, located at their isoelectric point, are electrically neutral. Since IvIg proteins themselves possess a degree of hydrophobicity, measuring the amount of IvIg protein bound to the nylon membrane can indicate the membrane's adsorption and retention efficiency for protein aggregates. The contact angle between the two surfaces of the nylon membrane represents the overall hydrophobicity range of the membrane. More specifically, the contact angle and the amount of IvIg protein bound together indirectly define the hydrophobic adsorption capacity of the nylon membrane for protein aggregates. The hydrophobic adsorption capacity of the nylon membrane should not be too low or too high. If the capacity is too low, impurities such as protein aggregates accumulate on the nylon membrane more quickly, potentially requiring frequent cleaning or replacement to maintain normal retention efficiency. If the capacity is too high, the accumulation of contaminants on the nylon membrane increases, easily leading to clogging and blockage, resulting in decreased treatment efficiency. Excessive membrane capacity also increases fluid resistance, increasing the operating pressure of the filtration system and thus increasing energy consumption.
[0021] The crystallinity of nylon membranes should not be too high or too low. Nylon is a semi-crystalline organic polymer, and its crystallization behavior has a significant impact on its performance. When used in the pre-filtration process for removing protein aggregates from biological feed solutions, the crystallinity of the nylon membrane has a crucial influence on the protein aggregate removal efficiency. Even if the protein aggregate adsorption capacity of the nylon membrane is within the aforementioned range, if the crystallinity is too low, the hydrophobic interaction strength of the nylon membrane pore surface may not be high enough when filtering protein aggregates. The hydrophobic interaction between the protein aggregates and some pore surface surfaces decreases, and under the continuous impact of the filtration flow, unstable protein aggregates will re-enter the filtration flow and enter the filtrate of the nylon membrane. This results in the protein aggregate content in the biological feed solution after filtration remaining at a level that is still sensitive for the virus removal filter, ultimately leading to clogging of the virus removal filter. Therefore, the crystallinity of the nylon membrane needs to be increased to an appropriate range. Higher crystallinity results in a more ordered arrangement of molecular chains in the pore structure of the nylon membrane, stronger intermolecular forces, and stronger hydrophobic interactions with protein aggregates. This increases the binding strength between protein aggregates and the nylon membrane pore surface, preventing protein aggregates from re-dissolving into the filtered stream. Secondly, if the crystallinity of the nylon membrane is too high, although the binding strength between the nylon membrane and protein aggregates can be increased significantly, the excessively strong hydrophobic interactions caused by high crystallinity can lead to the retention of some target products in the biological feed solution that do not need to be retained, such as antibody proteins, resulting in a decrease in the overall yield of the target product.
[0022] Furthermore, the contact angle of the saturated saline solution on the second side is 10–70°.
[0023] By adopting the above technical solution, the saturated saline contact angle of the second side (10–70°) can also indicate the relative hydrophobicity of the nylon membrane. Secondly, when the second side is used as the outlet surface and the first side as the inlet surface, the contact angle of the first side is significantly larger than that of the second side. Therefore, the end of the nylon membrane closer to the first side is more hydrophobic, while the end closer to the second side is less hydrophobic. This results in stronger hydrophobic adsorption and retention of protein aggregates at the end of the nylon membrane closer to the first side, allowing for the adsorption of more protein aggregates. The end closer to the second side primarily re-adsorbs protein aggregates that were missed or dropped at the end closer to the first side, thus ensuring that the protein aggregate content in the filtered liquid is reduced to a relatively low level.
[0024] Furthermore, the nylon porous membrane has a binding capacity of 40–60 μg / cm³ for IvIg protein at its isoelectric point. 2The contact angle of the first side of the nylon porous membrane is 90-110°; the contact angle of the second side is 20-55°.
[0025] When the amount of IvIg protein bound to the nylon membrane and the contact angles of the first and second sides are controlled within the above range, the nylon membrane has a better adsorption and retention effect on protein aggregates.
[0026] Furthermore, the nylon porous membrane contains α-crystal form, accounting for more than 95% of the total crystal form content.
[0027] Given a fixed degree of crystallinity, the crystal structure of the crystalline regions of nylon is significant in indicating the arrangement of nylon molecular chains. Different crystal forms of nylon can be obtained through various preparation methods, with common crystal forms including α-type, β-type, and γ-type. Among these, the α-type belongs to the monoclinic crystal system, possessing a compact structure and strong hydrogen bonding interactions between crystal chains. Compared to other crystal forms, the α-type can more effectively improve the orderliness between nylon membrane molecular chains, enhancing intermolecular forces and thus improving the adsorption effect of nylon membranes on protein aggregates.
[0028] Furthermore, it has diffraction angles 2θ1 and 2θ2 obtained from XRD analysis and testing, wherein the diffraction angle 2θ1 is in the range of 20° to 20.2° and the diffraction angle 2θ2 is in the range of 23.8° to 24.1°;
[0029] The ratio of the peak intensity I1 at diffraction angle 2θ1 to the peak intensity I2 at diffraction angle 2θ2 is in the range of 1 to 3.
[0030] The XRD pattern obtained after XRD analysis of the nylon membrane shows diffraction characteristic peaks of 2θ2 and 2θ1. The 2θ1 peak represents the van der Waals forces between the molecular chains in the nylon membrane, while the 2θ2 peak represents the strength of the hydrogen bonds between the molecular chains. Therefore, the ratio of their peak intensities indicates the proportion of hydrogen bonds between the molecular chains in the nylon membrane of this invention. A higher proportion of hydrogen bonds indicates stronger hydrophobic adsorption of the nylon membrane and higher adsorption efficiency for protein aggregates. The peak intensity ratio in the XRD pattern of the nylon membrane indicates the bonding situation within the nylon membrane.
[0031] Furthermore, the half-peak width at the diffraction angle 2θ2 is 1.5–2.5°.
[0032] The half-peak width (WHM) at a diffraction angle of 2θ2 is related to the size of the actual crystal structure within the nylon membrane; a larger WHM indicates a smaller crystal structure. This invention controls the size of the crystal structure within the nylon membrane to an appropriate size by controlling the WHM at 2θ2. The crystal structure size in the nylon membrane cannot be too small, as this would result in overly dense molecular chains, fewer exposed hydrophobic groups, and reduced hydrophobic interactions. Conversely, the crystal size should not be too large, as this would enhance the anisotropy of the nylon membrane, leading to internal heterogeneity. This heterogeneity would result in poorer adsorption and retention of protein aggregates by the nylon membrane.
[0033] Furthermore, the grain thickness of the α-crystals in the nylon porous membrane perpendicular to the 2θ2 crystal plane is...
[0034] The grain thickness of the crystal plane at the perpendicular 2θ2 diffraction angle of the α-crystalline structure in the nylon membrane can be calculated using the Scherrer formula. When the grain thickness of the crystal plane at the perpendicular 2θ2 diffraction angle of the α-crystalline structure in the nylon membrane is controlled within the range of this invention, the crystal structure size is at a suitable size, which can better utilize the hydrophobic adsorption capacity of the crystalline region in the nylon membrane. If the crystal structure size is too large, it can easily lead to a deterioration in the mechanical properties of the nylon membrane, such as toughness; if the crystal structure size is too small, it will cause the molecular chains in the crystalline region of the nylon membrane to be arranged too tightly, which will reduce the exposure of hydrophobic groups and thus reduce the hydrophobic adsorption capacity of the nylon membrane.
[0035] Furthermore, infrared absorption spectroscopy measurements were performed on the first and second sides of the nylon porous membrane using the ATR method to determine the relative crystallinity X1 of the first side of the nylon porous membrane and the relative crystallinity X2 of the second side of the nylon porous membrane.
[0036] Where X1 = A1 / A r X2 = A2 / A r ;
[0037] A1 indicates that the first side of the nylon membrane is at 960cm. -1 The peak area of the nearby peak; A2 indicates the second side of the nylon membrane at 960 cm⁻¹ -1 Peak area of nearby peaks; A r This indicates that the first side of the nylon membrane is at 1638 cm. -1 The peak area of the nearby peaks;
[0038] The ratio B of the relative crystallinity X1 of the first side of the nylon porous membrane to the relative crystallinity X2 of the second side is 0.7 to 0.97.
[0039] The relative crystallinity of the second side of the nylon membrane can be measured by the ATR method. This invention controls the crystallinity of the second side to be higher than that of the first side, so that the hydrophobic adsorption capacity of the nylon membrane near the second side is stronger. This is equivalent to controlling the adsorption capacity of the nylon membrane for protein aggregates to gradually increase in the thickness direction, so that the adsorption effect of the nylon membrane for protein aggregates is significantly improved.
[0040] Furthermore, the ratio of the average aperture of the first side to the average aperture of the second side is 1.1 to 1.6.
[0041] The average pore size of the first side of the nylon membrane of the present invention is slightly larger than that of the second side, which allows the nylon membrane to have a larger adsorption capacity at the end near the first side. Furthermore, the higher adsorption capacity at the front end of the nylon membrane improves the removal efficiency of protein aggregates at the rear end.
[0042] The average pore size of the first side and the pore size of the second side of the nylon in this invention can be obtained by measuring the average SEM pore size of the first side and the second side. The average SEM pore size of the first side and the second side can be obtained by characterizing the membrane structure using a scanning electron microscope, followed by measurement using computer software (such as Matlab, NIS-Elements, etc.) or manual measurement, and then performing corresponding calculations. During the membrane preparation process, in the direction perpendicular to the membrane thickness, its various characteristics, such as pore size distribution, are roughly uniform and basically consistent; therefore, the average pore size of the entire plane can be reflected by the average pore size of a certain area on the corresponding plane. In actual measurement, the membrane surface can be characterized first using an electron microscope to obtain the corresponding SEM image. Since the pores on the membrane surface are roughly uniform, a certain area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 25μm 2 (5μm by 5μm), the specific area size depends on the actual situation. Then, use appropriate computer software or manual measurement to determine the diameter of all holes on the area, and then calculate to obtain the average diameter of the holes on the surface. Of course, those skilled in the art can also obtain the above parameters through other measurement methods. The above measurement methods are for reference only.
[0043] Furthermore, the ratio of the average diameter of the nylon fibers on the first side and the second side is 0.7 to 0.97.
[0044] The nylon membrane of the present invention is composed of nylon fibers formed by phase separation of casting solution. The interior of the nylon membrane is more permeable, the connectivity between the pores inside the nylon membrane is better, the number of intersecting channels is more, and the number of closed pores is less, which effectively improves the filtration speed, membrane flux and loading capacity of the nylon membrane.
[0045] The average fiber diameter on the first side of the nylon membrane is slightly smaller than that on the second side, indicating that the nylon fibers on the first side of the nylon membrane are more fiberized, finer, and more likely to expose hydrophobic groups, which can improve the hydrophobic adsorption capacity of the nylon membrane for protein aggregates near the first side.
[0046] The ratio of the diameter of the nylon fibers on the first side and the second side of the nylon in this invention can be obtained by measuring the average diameter of the nylon fibers on the first side using SEM and the ratio of the average diameter of the nylon fibers on the second side using SEM. The average diameters of the nylon fibers on the first and second sides can be characterized by scanning electron microscopy (SEM) of the membrane structure, followed by measurement using computer software (such as Matlab, NIS-Elements, etc.) or manual calculation, and then the corresponding calculations are performed. During membrane fabrication, in the direction perpendicular to the membrane thickness, its various characteristics, such as fiber diameter distribution, are approximately uniform and consistent. Therefore, the average fiber diameter of a portion of the corresponding plane can reflect the overall average fiber diameter of that plane. In actual measurement, the membrane surface can be characterized using an electron microscope to obtain the corresponding SEM image. Since the fiber diameter on the membrane surface is approximately uniform, a certain area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 25μm 2 (5μm by 5μm), the specific area size depends on the actual situation, and then use the corresponding computer software or manually to measure the diameter of all fibers on the area, and then calculate to obtain the average diameter of the nylon fibers on the surface; of course, those skilled in the art can also obtain the above parameters through other measurement methods, and the above measurement methods are for reference only.
[0047] Furthermore, the specific surface area of the nylon porous membrane is not less than 18 m². 2 / g.
[0048] The specific surface area of the nylon membrane needs to be controlled to be no less than 18m². 2 / g, so that the nylon membrane has a sufficient surface area for the adsorption and retention of protein aggregates in the biological feed solution. When the specific surface area is too small, it is difficult to improve the hydrophobic adsorption capacity of the nylon membrane to a better level, because there are too few sites for exposed hydrophobic groups in the pores of the nylon membrane.
[0049] Furthermore, the tensile strength of the nylon porous membrane is 1–5 MPa.
[0050] The tensile strength of nylon membranes needs to meet the requirements of their application. Insufficient tensile strength can easily lead to membrane damage during filtration, while excessive tensile strength can negatively impact other mechanical properties. Tensile strength can be measured using a universal tensile testing machine.
[0051] A method for preparing a nylon porous membrane for virus pre-filtration includes the following steps:
[0052] S1: Prepare nylon casting solution and provide carrier; the viscosity of the nylon casting solution is controlled at 10,000 to 30,000 cP, and the molecular weight of nylon is controlled at 50,000 to 100,000.
[0053] S2: The nylon casting solution is brushed onto the surface of the carrier to form a coating film;
[0054] S3: Separate the coated film to form a semi-wet film; during the phase separation process, the phase separation time is set between 1s and 120s, and the temperature during phase separation is controlled between 25℃ and 40℃.
[0055] S4: Immerse the semi-wet film in the solution for at least 30 seconds, and control the solution temperature at 40-50°C. The solution includes at least one of an acid or an organic solvent, and a non-solvent, wherein the non-solvent content is not less than 80 wt%.
[0056] S5: The formed membrane is further cleaned and dried to form the finished membrane.
[0057] The temperature of the coagulation bath affects the phase separation rate of the nylon membrane. This invention controls the temperature in the coagulation bath to a relatively high level, and simultaneously controls the viscosity of the nylon membrane casting solution within a specified range. This results in better fiberization and higher crystallinity of the nylon fibers obtained through phase separation. Secondly, the proportion of non-solvents in this invention is also controlled within a relatively high range. A higher non-solvent content leads to a faster solvent extraction process in the coagulation bath, thus increasing the crystallinity of the nylon fibers formed through phase separation.
[0058] Secondly, this invention also achieves a nylon membrane with moderate pore density and good symmetry by controlling the molecular weight of the nylon added to the casting solution within a suitable range. Higher molecular weight nylon in the casting solution results in a higher pore density and smaller pores in the formed membrane structure, making it more difficult to maintain symmetry. Conversely, excessively low molecular weight nylon in the casting solution can easily lead to an inability to maintain the negative charge strength and crystallinity of the nylon membrane.
[0059] Furthermore, in step S4, the initial temperature of the semi-wet film differs from the initial temperature of the solution by 3 to 10°C.
[0060] In step S4, the initial temperature of the semi-wet membrane is kept at a certain temperature difference with the initial temperature of the solution. This allows the semi-wet membrane to heat up when it enters the coagulation bath, resulting in more uniform phase separation of the semi-wet membrane in the coagulation bath and a smaller difference between the membrane before and after the membrane.
[0061] Furthermore, in step S3, air blowing is performed simultaneously with phase separation, and the humidity of the blown air is controlled at 50-90%, and the temperature is controlled at 20-35°C.
[0062] Pre-phase separation allows the air side of the nylon membrane to have a tendency to pre-separate into depleted and rich phase regions. After entering the coagulation bath, the depleted and rich phase regions can be formed quickly, resulting in a more uniform formation and better fiberization. This allows the crystallinity of the second side of the nylon membrane to form the required difference between the first side and the second side.
[0063] Furthermore, the casting solution comprises the following components by mass percentage: 15%–35% nylon, 40%–85% polar solvent, and 0%–25% additives;
[0064] The polar solvent is selected from one or more of formic acid, hydrochloric acid, sulfuric acid, phosphoric acid, and trifluoroacetic acid;
[0065] The additive is selected from one or more of methanol, ethanol, water, citric acid, polyethylene glycol, and caprolactam;
[0066] Furthermore, the acid mentioned in step S4 includes one or more of formic acid, acetic acid, sulfuric acid, phosphoric acid, and hydrochloric acid; the organic solvent mentioned in step S4 includes one or more of alcohol, isopropanol, and glycerol.
[0067] In summary, the present invention has the following beneficial effects:
[0068] First, by controlling the amount of IvIg protein bound to the nylon membrane and the crystallinity of the nylon membrane, the hydrophobic adsorption capacity and hydrophobic adsorption strength of the nylon membrane are enhanced. As a result, when the biological feed liquid is filtered through the nylon membrane, the nylon membrane can effectively adsorb and retain impurities such as protein aggregates, thereby improving the removal rate of protein aggregates in the biological feed liquid after passing through the nylon membrane.
[0069] Secondly, the nylon membrane of the present invention also improves the removal efficiency of protein aggregates by controlling the crystal form and content of nylon to enhance the hydrophobic interaction of the nylon membrane with protein aggregates. Attached Figure Description
[0070] Figure 1 This is the XRD pattern obtained from the XRD test of the nylon film in Example 1;
[0071] Figure 2This is a 10000× SEM image of the second side of the nylon membrane in Example 1;
[0072] Figure 3 This is a 10000× SEM image of the first side of the nylon membrane in Example 1. Detailed Implementation
[0073] To better understand the above-mentioned objectives, features, and advantages of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be combined with each other.
[0074] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and therefore the scope of protection of the invention is not limited to the specific embodiments disclosed below.
[0075] Example
[0076] Example 1
[0077] A nylon porous membrane for virus pre-filtration has non-directional tortuous pathways inside. One side surface of the nylon porous membrane is a first side surface with a plurality of first pores, and the other side surface of the nylon porous membrane is a second side surface with a plurality of second pores.
[0078] A method for preparing a nylon porous membrane for virus pre-filtration includes the following steps:
[0079] S1: Prepare nylon casting solution and provide carrier;
[0080] The casting solution comprises the following components by weight percentage: 20% nylon-6, 65% polar solvent, and 15% additive; wherein, in this embodiment, the polar solvent is formic acid, but in another embodiment, the polar solvent may also be one or more of formic acid, hydrochloric acid, sulfuric acid, phosphoric acid, and trifluoroacetic acid. In this embodiment, the additive is methanol, but in another embodiment, the additive may also be one or more of methanol, ethanol, water, citric acid, polyethylene glycol, and caprolactam.
[0081] The viscosity of the casting solution is controlled between 10,000 and 30,000 cP, and the molecular weight of the nylon is controlled between 50,000 and 100,000. In this embodiment, the viscosity of the casting solution is controlled at 20,000 cP, and the molecular weight of the nylon is 50,000.
[0082] The carrier can be a plate-shaped material that supports a liquid film.
[0083] S2: Apply nylon casting solution to the surface of the carrier to form a coating film. The coating here refers to placing nylon casting solution on the surface and inside the carrier. The specific method can be to immerse the carrier in nylon casting solution, spray the nylon casting solution onto the surface of the carrier through a nozzle, brush the nylon casting solution onto the surface of the carrier, or use other coating methods.
[0084] S3: Pre-separate the coated film to form a semi-wet film; during the pre-separation process, the pre-separation time is set to 1 to 120 seconds, the temperature is 25 to 40 degrees Celsius, and air is blown while pre-separating, with the relative humidity of the blown air controlled at 50 to 90%.
[0085] In this embodiment, the pre-phase separation time is controlled at 10 seconds and the temperature is controlled at 40°C; and air blowing is performed simultaneously with the pre-phase separation, with the relative humidity of the blown air controlled at 80%.
[0086] S4: Immerse the semi-wet film in the solution, maintaining the solution temperature at 40–50°C. The initial temperature of the semi-wet film should differ from the initial temperature of the solution by 3–10°C, and this should be maintained for at least 30 seconds. The solution comprises the following components by weight percentage: formic acid 0–10%, alcohol 0–10%, and water 80%–100%. In this example, formic acid is 5%, alcohol is 10%, and water is 85%.
[0087] In this embodiment, the temperature of the solution is controlled at 40°C, and the initial temperature of the semi-wet film differs from the initial temperature of the solution by 6°C.
[0088] S5: The formed membrane is further cleaned and dried to form the finished membrane.
[0089] The process parameters for preparing nylon films in Examples 1 to 26 are different, as shown in Table 1 below.
[0090] Table 1
[0091]
[0092]
[0093] The nylon films prepared in Examples 1-10 were subjected to the following tests:
[0094] (1) The average pore size of the nylon membrane was obtained by measuring the pore size of the pore size meter.
[0095] (2) The amount of IvIg protein bound to the nylon membrane was detected by the following method:
[0096] use Intravenous immunoglobulin (pH 4) was used as the stock solution for IVIg protein. This stock solution was diluted with physiological saline to prepare a 0.5 g / L IVIg protein solution with a pH of 7 (the isoelectric point of the IVIg protein solution is 7). The sample was then held in a nylon membrane using a clamp, and the IVIg protein solution was supplied to the nylon membrane from one of the first side surfaces. The filtration rate was 120 L / min, and the filtration rate was 100 L / m³. 2 Then, the concentration c of the IvIg protein solution in the filtrate is measured.
[0097] (3) The crystallinity of the nylon film was obtained by XRD diffraction and then by MDI Jade 6 software analysis.
[0098] (4) The contact angle test used saturated saline solution as water droplets and was conducted using a fully automatic contact angle tester. The temperature during the test was room temperature (25℃).
[0099] Table 2
[0100]
[0101] Furthermore, XRD testing revealed that the XRD patterns of the nylon films prepared in Examples 1-10 (such as...) Figure 1 Only the α-type diffraction peak of Nylon-6 exists, and the crystal form is mainly α-type, with no other crystal forms.
[0102] The difference between Examples 11 and 12 and Example 1 is that the ratio of the peak intensity I1 at diffraction angle 2θ1 to the peak intensity I2 at diffraction angle 2θ2 in the XRD test of the nylon film is different.
[0103] The nylon films prepared in Examples 1 and 11-12 have diffraction angles 2θ1 and 2θ2 as determined by XRD analysis. Diffraction angle 2θ1 is in the range of 20° to 20.2°, and diffraction angle 2θ2 is in the range of 23.8° to 24.1°. The peak intensity at diffraction angle 2θ1 is I1, and the peak intensity at diffraction angle 2θ2 is I2.
[0104] Table 3
[0105]
[0106]
[0107] The difference between Examples 13 and 14 and Example 1 lies in the half-peak width (FWHM) of the 2θ2 diffraction angle of the nylon film. The FWHM of the 2θ2 diffraction angle of the nylon film was obtained by analyzing the XRD patterns using MDI Jade 6 software.
[0108] Table 4
[0109] Example Half-peak width (°) <![CDATA[Peak intensity ratio of I1 and I2]]> Example 1 1.8 1.6 Example 13 1.5 1.7 Example 14 2.5 1.6
[0110] The difference between Examples 15-16 and Example 1 lies in the grain thickness of the nylon film at the 2θ² diffraction angle, while other parameters are essentially the same. The grain thickness of the nylon film at the 2θ² diffraction angle is calculated using the Scherrer formula. Scherrer formula: D = Kγ / Bcosθ, where K is the Scherrer constant, D is the average thickness of the grain perpendicular to the crystal plane, B is the measured half-peak width or integral width of the diffraction peak in the sample, θ is the Bragg angle, and γ is the X-ray wavelength.
[0111] Table 5
[0112]
[0113] The difference between Examples 17-20 and Example 1 lies in the relative crystallinity ratio of the nylon film on the second side, while other parameters are basically similar. The relative crystallinity was measured by infrared absorption spectroscopy of the first and second sides of the porous substrate using the ATR method, where X1 = A1 / A r X2 = A2 / A r A1 indicates that the first side of the porous body is at 960cm. -1 The peak area of the nearby peak; A2 represents the second side surface of the porous body at 960 cm⁻¹ -1 Peak area of nearby peaks; A r This indicates that the first side of the porous body is at 1638 cm. -1 The peak area of the nearby peaks.
[0114] Table 6
[0115]
[0116] The difference between Examples 21-23 and Example 1 lies in the ratio of the average pore size of the second side of the nylon membrane. The average pore size of the first and second sides of the nylon membrane of this invention can be obtained by measuring the average SEM pore size of the first and second sides. The average SEM pore size of the first and second sides can be obtained by characterizing the membrane structure using a scanning electron microscope, followed by measurement using computer software (such as Matlab, NIS-Elements, etc.) or manual calculation. During membrane preparation, its characteristics, such as pore size distribution, are generally uniform and consistent along the direction perpendicular to the membrane thickness. Therefore, the average pore size of a portion of the corresponding plane can reflect the overall average pore size of that plane. In actual measurement, the membrane surface can be characterized using an electron microscope to obtain the corresponding SEM image. Since the pores on the membrane surface are generally uniform, a certain area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 25μm 2 (5μm by 5μm), the specific area size depends on the actual situation. Then, use appropriate computer software or manual measurement to determine the diameter of all holes on the area, and then calculate to obtain the average diameter of the holes on the surface. Of course, those skilled in the art can also obtain the above parameters through other measurement methods. The above measurement methods are for reference only.
[0117] Table 7
[0118]
[0119]
[0120] The difference between Examples 24-26 and Example 1 lies in the ratio of the nylon fiber diameters on the second side of the nylon membrane. The ratio of the nylon fiber diameters on the first and second sides of the nylon membrane of this invention can be obtained by measuring the average diameter of the nylon fibers on the first and second sides using SEM images. The average diameters of the nylon fibers on the first and second sides can be characterized using a scanning electron microscope (SEM) to model the membrane structure, followed by measurement using computer software (such as Matlab, NIS-Elements, etc.) or manual calculation, and then the corresponding calculations are performed. During membrane fabrication, in the direction perpendicular to the membrane thickness, its various characteristics, such as fiber diameter distribution, are approximately uniform and consistent. Therefore, the average fiber diameter of a portion of the corresponding plane can reflect the overall average fiber diameter of that plane. In actual measurement, the membrane surface can be characterized using an electron microscope to obtain the corresponding SEM image. Since the fiber diameter on the membrane surface is approximately uniform, a certain area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 25μm 2 (5μm by 5μm), the specific area size depends on the actual situation, and then use the corresponding computer software or manually to measure the diameter of all fibers on the area, and then calculate to obtain the average diameter of the nylon fibers on the surface; of course, those skilled in the art can also obtain the above parameters through other measurement methods, and the above measurement methods are for reference only.
[0121] Table 8
[0122]
[0123] Comparative Example
[0124]
[0125]
[0126] Performance testing:
[0127] (1) Protein aggregate retention performance test: Preparation of protein aggregate feed standard solution: IgG aggregate solution (SeraCare 5% human gamma globulin, purchased from SeraCare, Inc., CAT#HS-9000), phosphate buffer (10g / L Difeo FA buffer, pH 7.2, from Fisher Scientific, Cat#DF 2314150) and EDTA (10mmol / L calcium disodium ethylenediaminetetraate, from Sigma Aldrich, CAT#ED2SC) were mixed to obtain the initial feed solution. The initial feed solution was passed through a PLCXK membrane (PLCXK membrane is a cellulose ultrafiltration membrane with a nominal molecular weight of 1000kDaltons, available from Millipore, Bedford, Massachusetts) to remove 90% of the protein aggregates, resulting in a protein aggregate feed solution with a concentration of 10% of the original.
[0128] The effective filtration area assembled using the nylon membrane for virus pre-filtration in the various embodiments and comparative examples of this application is 4.5 × 10⁻⁶. -4 m 2 The filter selectively removes protein aggregates from the solution during constant flow (NFF) filtration. This is followed by sequential use of a Millipore filter with an effective filtration area of 3.5 cm², supplied by Millipore, Bedford, Massachusetts. 2 and 13.5cm 2 of The NFP filter performs a virus removal procedure, specifically when 3.5cm... 2 of After the NFP filter reaches its retention capacity, then use a 13.5cm filter. 2 of The NFP filter performs a virus removal step until the virus load is reached.
[0129] The effective filtration area is 3.5cm². 2 The virus filter's rejection capacity is measured in V. R V R A larger value indicates more stable protein aggregates adsorbed on the nylon membrane, resulting in lower dissolution at the rear end. A value of 13.5 cm was measured. 2 The virus filter's rejection capacity, Vmax, is used to measure the ability of the deep filter paperboard to remove protein aggregates; the stronger the removal capacity, the larger Vmax.
[0130] (2) The nylon membranes for virus pre-filtration from the various embodiments and comparative examples in this application were assembled into a filter to obtain a 4.5 × 10⁻⁶ membrane. -4 m 2Filters with effective filtration area; flow rates in various embodiments and comparative examples were measured when 50 ml of water passed through the filter at a constant pressure of 100 kPa and a temperature of 20°C.
[0131] Tests were conducted on Examples 1 to 7 and Comparative Examples 1 to 3, and the test results are shown in the table below:
[0132]
[0133] V R This indicates the protein aggregate content in the downstream feed solution during the initial filtration stage of the nylon membrane, while V R The larger the value, the stronger the adsorption capacity of the nylon membrane for protein aggregates in the feed solution, and the more stable the adsorption; while V R The smaller the value, the more likely the nylon membrane has cross-adsorption capacity for protein aggregates or poorer adsorption stability. max V represents the overall protein aggregate adsorption capacity of the nylon membrane. max A larger value indicates that the nylon membrane has a better adsorption and retention effect on protein aggregates in the biological feed solution, and also has a better adsorption loading capacity; while V max The smaller the value, the less likely the nylon membrane is to adsorb impurities such as protein aggregates in the biological feed solution. It is easy to reach the load saturation, causing the virus removal filter to become clogged quickly.
[0134] The test results in the table above show that the pore size of the nylon membrane, the amount of IvIg protein binding, the contact angle between the first and second sides, and the crystallinity of the nylon membrane itself (obtained by XRD testing) have a significant impact on the removal of protein aggregates from the biological feed solution by the nylon membrane. When the above parameters meet the requirements of this invention, the adsorption capacity of the nylon membrane for protein aggregates in the biological feed solution is significantly improved, and the adsorption loading and stability of the protein aggregates are also significantly optimized. A comparison between Examples 6-10 also shows that a larger difference in zeta potential between the first and second sides of the nylon membrane is not necessarily better. Within the preferred range of 8-25 mV, the nylon membrane exhibits superior adsorption capacity for protein aggregates.
[0135] Secondly, by comparing Example 4 with other examples, it can be seen that the contact angle of the second side cannot be too small. When the contact angle is too small, the adsorption effect of the protein aggregate near the second side is easily weakened, resulting in a poor overall retention and adsorption effect of the protein aggregate.
[0136] Tests were conducted on Examples 11 and 12, and the test results are shown in the table below:
[0137]
[0138] A comparison of the test results from Examples 11 and 12 shows that when the ratio of the peak intensities at the 2θ1 and 2θ2 diffraction angles of the prepared nylon membrane is between 1 and 3, the crystallization state within the nylon membrane is relatively more conducive to the hydrophobic adsorption of protein aggregates within the nylon membrane.
[0139] Tests were conducted on Examples 13 and 14, and the test results are shown in the table below:
[0140]
[0141] The comparison of the detection data in Examples 13 and 14 shows that the half-peak width at the 2θ2 diffraction angle of the nylon membrane has a certain influence on the specific crystallization of the crystalline region within the nylon membrane. This is because the half-peak width at the 2θ2 diffraction angle is related to the crystal structure size of the crystalline region of the nylon membrane, and a suitable crystal structure size can help the nylon membrane better generate hydrophobic adsorption for protein aggregates.
[0142] Tests were conducted on Examples 15 and 16, and the test results are shown in the table below:
[0143]
[0144]
[0145] The comparison of the test data from Examples 15 and 16 shows that when the grain thickness perpendicular to the crystal plane at the 2θ2 diffraction angle of the nylon membrane is within the range of the present invention, it can help the nylon membrane to better generate hydrophobic adsorption on protein aggregates.
[0146] Tests were conducted on Examples 17 to 20, and the test results are shown in the table below:
[0147]
[0148] The data in the table above shows that the relative crystallinity of the first and second sides of the nylon membrane together determines the overall crystallinity of the membrane. Nylon membranes with higher relative crystallinity on both the first and second sides exhibit higher adsorption effects on protein aggregates.
[0149] Secondly, compared with the relative crystallinity of the second side, when the ratio of the relative crystallinity of the first side to the relative crystallinity of the second side is controlled between 0.7 and 0.97, the adsorption intensity of the nylon membrane for protein aggregates in the gradient direction gradually increases, thereby significantly improving the adsorption effect of the nylon membrane on protein aggregates.
[0150] Tests were conducted on Examples 21 to 23, and the test results are shown in the table below:
[0151]
[0152] Analysis of the test results in the table above shows that the average pore size of the first side of the nylon membrane being slightly larger than that of the second side can improve the adsorption effect of the nylon membrane on protein aggregates to a certain extent.
[0153] Tests were conducted on Examples 24 to 26, and the test results are shown in the table below:
[0154]
[0155]
[0156] Analysis of the above test results shows that, compared with the average diameter of nylon fibers on the second side of the nylon membrane, the smaller the average diameter of nylon fibers on the first side of the nylon membrane, the better the hydrophobic adsorption capacity of the nylon membrane can be to a certain extent.
[0157] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A nylon porous membrane for virus pre-filtration, wherein the nylon porous membrane has non-directional tortuous pathways, one side surface of the nylon porous membrane is a first side surface having a plurality of first pores, and the other side surface of the nylon porous membrane is a second side surface having a plurality of second pores, characterized in that: The average pore size (PMI) of the nylon porous membrane is 0.05–1 μm. The nylon porous membrane has a binding capacity of 30–100 μg / cm³ for IvIg protein at its isoelectric point. 2 ; The saturated saline contact angle of the first side of the nylon porous membrane is 80-130°, and the saturated saline contact angle of the second side is 10-70°. The crystallinity of the nylon porous membrane was measured by XRD, and the crystallinity of the nylon porous membrane was 40-90%. The relative crystallinity X1 of the first side and the relative crystallinity X2 of the second side of the nylon porous membrane were measured by infrared absorption spectroscopy using the ATR method. Where X1 = A1 / A r X2 = A2 / A r ; A1 indicates that the first side of the nylon porous membrane is at 960cm. -1 The peak area of the nearby peak; A2 indicates the second side surface of the nylon porous membrane at 960 cm⁻¹ -1 Peak area of nearby peaks; A r This indicates that the first side of the nylon porous membrane is at 1638 cm. -1 The peak area of the nearby peaks; The ratio B of the relative crystallinity X1 of the first side of the nylon porous membrane to the relative crystallinity X2 of the second side is 0.7 to 0.
97. The ratio of the average aperture of the first side to the average aperture of the second side is 1.1 to 1.6; The ratio of the average diameter of the nylon fibers on the first side and the second side is 0.7 to 0.
97.
2. The nylon porous membrane for virus pre-filtration according to claim 1, characterized in that, The nylon porous membrane has a binding capacity of 40–60 μg / cm³ for IvIg protein at its isoelectric point. 2 The saturated saline contact angle of the first side of the nylon porous membrane is 90-110°; the saturated saline contact angle of the second side is 20-55°.
3. The nylon porous membrane for virus pre-filtration according to claim 1, characterized in that, The nylon porous membrane contains α-crystal form, accounting for more than 95% of the total crystal form content.
4. The nylon porous membrane for virus pre-filtration according to claim 1, characterized in that, It has diffraction angles 2θ1 and 2θ2 obtained from XRD analysis and testing, wherein the diffraction angle 2θ1 is in the range of 20° to 20.2° and the diffraction angle 2θ2 is in the range of 23.8° to 24.1°; The ratio of the peak intensity I1 at diffraction angle 2θ1 to the peak intensity I2 at diffraction angle 2θ2 is in the range of 1 to 3.
5. The nylon porous membrane for virus pre-filtration according to claim 4, characterized in that, The half-peak width at the diffraction angle 2θ2 is 1.5–2.5°.
6. The nylon porous membrane for virus pre-filtration according to claim 4, characterized in that, The grain thickness of the α crystals in the nylon porous membrane perpendicular to the 2θ2 crystal plane is 1.2–2.3 Å.
7. The nylon porous membrane for virus pre-filtration according to claim 1, characterized in that, The specific surface area of the nylon porous membrane is not less than 18m². 2 / g.
8. The nylon porous membrane for virus pre-filtration according to claim 1, characterized in that, The tensile strength of the nylon porous membrane is 1–5 MPa.
9. A method for preparing a nylon porous membrane for virus pre-filtration according to any one of claims 1 to 8, characterized in that, Includes the following steps: S1: Prepare nylon casting solution and provide carrier; control the viscosity of casting solution to 3000-30000 cP; S2: The nylon casting solution is brushed onto the surface of the carrier to form a coating film; S3: Pre-separate the coated film to form a semi-wet film; during the pre-separation process, the pre-separation time is set between 10s and 48s, and the temperature during the pre-separation is controlled between 25℃ and 40℃. S4: Immerse the semi-wet film in a coagulation bath at a temperature of 40–50°C for at least 30 seconds; the coagulation bath includes at least one of an acid or organic solvent, and a non-solvent, wherein the non-solvent content is not less than 80 wt%. S5: The formed membrane is further cleaned and dried to form the finished membrane; In step S3, air blowing is performed simultaneously with pre-phase separation, and the humidity of the blown air is controlled at 50-90% and the temperature is controlled at 25-35℃. Pre-phase separation creates a difference in crystallinity between the second side and the first side of the nylon film.
10. The method for preparing a nylon porous membrane for virus pre-filtration according to claim 9, characterized in that, In step S4, the initial temperature of the semi-wet film differs from the initial temperature of the coagulation bath by 3 to 10°C.
11. The method for preparing a nylon porous membrane for virus pre-filtration according to claim 9, characterized in that, The casting solution comprises the following components by weight percentage: 15%–35% nylon, 40%–85% polar solvent, and 0%–25% additives; The polar solvent is selected from one or more of formic acid, hydrochloric acid, sulfuric acid, phosphoric acid, and trifluoroacetic acid; The additive is selected from one or more of methanol, ethanol, water, citric acid, polyethylene glycol, and caprolactam.
12. The method for preparing a nylon porous membrane for virus pre-filtration according to claim 9, characterized in that, The acids mentioned in step S4 include one or more of formic acid, acetic acid, sulfuric acid, phosphoric acid, and hydrochloric acid; the organic solvents mentioned in step S4 include one or more of alcohol, isopropanol, and glycerol.
Citation Information
Patent Citations
Method for removing biopolymer aggregates and viruses from a fluid
US10987629B2
Nylon film, and preparation method and application thereof
CN111603948A