Ultra-low temperature high-strength container steel plate and manufacturing method thereof

By adding specific elements and optimizing the process to the steel for low-temperature pressure vessels, the problem of unstable steel plate strength and weldability under ultra-low temperature conditions has been solved, and the production of high-strength and low-cost ultra-low temperature and high-strength vessel steel plates has been achieved to meet the requirements of ultra-low temperature and high pressure. performance requirements in the environment.

CN117004885BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310906845.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-24
Publication Date
2024-10-22
Estimated Expiration
2043-07-24

AI Technical Summary

Technical Problem

The low-temperature impact performance, strength and weldability of existing steel for cryogenic pressure vessels at the core and surface thickness locations under ultra-low temperature conditions are unstable, and the production cost is high.

Method used

Ultra-low temperature and high-strength container steel plates with specific composition are used, containing elements such as C, Si, Mn, Nb, Ni, V, Ca, Al, etc., through the smelting-continuous casting-heating-rolling-heat treatment process, using two-stage controlled rolling and normalizing + Tempering or normalizing weak cold and heat treatment to produce steel plates with a thickness range of ≤120mm, ensuring that the steel plates have good tensile strength and transverse impact energy under -70°C conditions.

Benefits of technology

It achieves high strength and good toughness properties of the steel plate under ultra-low temperature conditions, reduces production costs, and at the same time ensures the overall performance and welding performance of the steel plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117004885B_ABST
    Figure CN117004885B_ABST
Patent Text Reader

Abstract

The present invention provides an ultra-low temperature high-strength container steel plate and a manufacturing method thereof. The components of the steel plate are as follows by weight percentage: C: 0.1% to 0.12%, Si: 0.22% to 0.49%, Mn: 1.35% to 1.48%, P: ≤ 0.005%, S: ≤ 0.003%, Nb: 0.04% to 0.06%, Ni: 0.1% to 0.19%, V: 0.1% to 0.21%, Ca: 0.000 3%~0.005%, Als: 0.015%~0.035%, and the rest are Fe and unavoidable impurities; through smelting-continuous casting-heating-rolling-heat treatment, a two-stage controlled rolling method combined with normalizing + tempering and normalizing weak cold and hot treatment is adopted to produce container steel plates with a maximum thickness of 120mm. The structure of the produced steel plates is uniform throughout the entire thickness section, the steel plates have good strength and toughness matching at 1 / 4 and 1 / 2 thickness, and the steel plates have good welding performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of metal materials, and in particular relates to a production method of an ultra-low temperature high-strength container steel plate. Background Art

[0002] With the rapid development of my country's petrochemical industry, the liquefaction, separation and production, storage, transportation and application of liquefied gas have become quite common. In particular, liquefied petroleum gas, as a clean, convenient and thermally efficient energy source, has been widely used in the field of industrial and civilian fuels. Due to the many advantages of liquid gas and liquefied petroleum gas and the broad market prospects, the application of cryogenic pressure vessels, cryogenic spherical storage tanks and high-parameter cryogenic cylindrical containers in the fields of petroleum and chemical industry has been greatly promoted. However, since such cryogenic containers have the characteristics of low temperature and high pressure, higher performance and organizational requirements are also put forward for the steel used for cryogenic pressure vessels.

[0003] At present, the low-temperature steels commonly used in countries around the world are aluminum-killed C-Mn steel and Ni-containing low-temperature steel. Taking into account the technical and economic effects, process performance, and especially based on the safety of pressure vessels, there are two development directions for low-temperature pressure vessel low-alloy steel: one is to improve strength, and the other is to ensure good low-temperature toughness and welding performance. The current low-temperature steel is based on low-carbon steel to increase the strength of steel by increasing the Mn content, and appropriately reduce the carbon content to improve welding performance. While reducing the content of impurity elements such as S and P in steel and improving the purity of steel, Ni elements and micro-alloy elements such as Nb, V, and Ti are added at a rate of not more than 1% to achieve the purpose of solid solution strengthening and precipitation strengthening, thereby reducing the brittle transition temperature of steel. Therefore, compared with general low-carbon steel, this type of steel has better low-temperature toughness. Compared with the relevant standards in the United States and Europe, my country's GB 3531-2014 standard is more detailed, especially tightening the requirements for impact toughness, which can fully ensure the safety of low-temperature pressure vessels.

[0004] Low-temperature pressure vessel steel is required to have good low-temperature toughness and welding performance under low-temperature conditions, and should also have a certain strength level. Low-temperature pressure vessel steel used in the petrochemical field is fully capable of replacing similar foreign products, and the market demand is large. In view of this, it is urgent to develop ultra-low-temperature pressure vessel steel with high strength and toughness to meet market demand.

[0005] For full-thickness pressure vessel steel plates, in order to solve the problems of unstable low-temperature impact performance, unstable strength value and unstable weldability at the 1 / 2 thickness of the core and 1 / 4 of the surface under ultra-low temperature service temperature, it is urgent to develop a special low-cost production method for ultra-low temperature high-strength container steel plates.

[0006] The relevant technologies are as follows:

[0007] The steel plate disclosed in the patent document "A steel plate for ultra-low temperature container and its production method" (CN115558848A) is composed of the following weight percentage components: C 0.05-0.09%, Si 0.15-0.20%, Mn 0.90-1.30%, P≤0.008%, S≤0.002%, B≤0.005%, Cr 0.10-0.20%, Mo 0.10-0.18%, Nb 0.015-0.020%, Ni 0.20-0.35%, Ti 0.010-0.020%, Cu<0.3%, Zr≤0.05%, and the balance is Fe and unavoidable impurities. The above method can meet the needs of use in medium and low temperature and high pressure environments, but the addition of Zr element makes the production cost too high.

[0008] Patent document "A 9Ni marine low-temperature container steel plate with high flaw detection quality" (CN107604255A) discloses a low-temperature container steel plate with Fe as the base element and contains the following chemical components in mass percentage: C: 0.03-0.05%, Si: 0.10-0.14%, Mn: 0.50-0.80%, Ni: 8.7-9.7%, P: ≤0.008%, S: ≤0.002%, Cr: ≤0.25%, Mo: ≤0.08%, Cu: ≤0.35%, Alt: 0.020-0.035%, Nb: 0.01-0.02%, N: ≤60ppm, H: ≤1.2ppm, and unavoidable impurity elements. The steel plate thickness designed for production under the above composition is 6 to 50 mm. No research has been conducted on the production of large-thickness steel plates, and the addition of a large amount of alloying elements Ni and Cr also increases the production cost.

[0009] The chemical composition of the steel plate disclosed in the patent document "A Large Thickness Low Compression Ratio High Die Welding Low Temperature Container Steel Plate" (CN111349854A) is calculated by weight percentage, including C: 0.15-0.17%, Si: 0.30-0.40%, Mn: 1.25-1.35%, P≤0.008%, S≤0.002%, Ni: 0.28-0.32%, Nb: 0.013-0.019%, Alt: 0.035-0.065%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15≤0.42%, and the balance is Fe and unavoidable impurities. The above research designed a method for producing a steel plate with a thickness of 90mm. The thickness of the steel plate is single, and other thickness specifications have not been studied. In addition, the production method of quenching and heat treatment is more expensive than normalizing.

[0010] The steel plate disclosed in the patent document "A medium-thickness high-toughness high-mold welded low-temperature container steel plate and its production method" (CN111270142A) includes, by weight percentage, C: 0.15-0.17%, Si: 0.30-0.40%, Mn: 1.25-1.35%, P≤0.008%, S≤0.002%, Ni: 0.28-0.32%, Nb: 0.013-0.019%, Alt: 0.035-0.065%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15≤0.42%, and the remainder is Fe and inevitable impurities; the performance of the steel plate reaches: the tensile strength of 1 / 4 thickness and 1 / 2 thickness is ≥550MPa, and the lateral impact energy Akv at -45℃, 1 / 4 thickness and 1 / 2 thickness is ≥100J, and it has good strength and toughness properties. The thickness range of steel plates designed for production under the above composition is 20-60mm. The production of thicker steel plates has not been studied, the low-temperature impact margin is insufficient, and the low-temperature toughness at lower service temperatures has not been studied. Summary of the invention

[0011] The purpose of the present invention is to overcome the above-mentioned problems and shortcomings and to provide a method for producing an ultra-low temperature high-strength container steel plate. The tensile strength of the steel plate at 1 / 4 thickness and 1 / 2 thickness is ≥510MPa; under -70°C conditions, the transverse impact energy KV2 at 1 / 4 thickness and 1 / 2 thickness of the steel plate is ≥260J.

[0012] The object of the invention is achieved in this way:

[0013] The invention discloses an ultra-low temperature high-strength container steel plate, wherein the components of the steel plate are as follows by weight percentage: C: 0.1% to 0.12%, Si: 0.22% to 0.49%, Mn: 1.35% to 1.48%, P: ≤0.005%, S: ≤0.003%, Nb: 0.04% to 0.06%, Ni: 0.1% to 0.19%, V: 0.1% to 0.21%, Ca: 0.0003% to 0.005%, Als: 0.015% to 0.035%, and the rest are Fe and unavoidable impurities.

[0014] In the container steel plate, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15≤0.43%, Pcm={ω(C)+ω(Si) / 30+[ω(Mn)+ω(Cu)+ω(Cr)] / 20+ω(Ni) / 60+ω(Mo) / 15+ω(V) / 10+ω(B)}%≤0.23.

[0015] The Nb / V ratio in the steel plate is 0.2 to 0.6.

[0016] The microstructure of the steel plate is mainly ferrite + pearlite. The volume percentage of V / (C, N) in the microstructure of the steel plate is not more than 2%.

[0017] The thickness range of the steel plate is ≤120mm, the tensile strength at 1 / 4 thickness and 1 / 2 thickness of the steel plate is ≥510MPa; at -70℃, the transverse impact energy KV at 1 / 4 thickness and 1 / 2 thickness of the steel plate 2 ≥260J.

[0018] The reasons for the composition design of the present invention are as follows:

[0019] C often forms carbides with other alloying elements in steel to play a strengthening role. From the perspective of ensuring the strength of the steel plate, it is hoped that the C content is kept at a high level, but a high C content is prone to segregation in the steel, resulting in a significant decrease in the toughness and plasticity of the steel plate. Therefore, under the premise of ensuring the strength of the steel plate, the C content is controlled at 0.1-0.12%.

[0020] Si has deoxidation and desulfurization effects in steel and can improve the strength of steel plates through solid solution strengthening. Si is a cheap alloying element. Adding an appropriate amount of Si to steel can improve the hardness and strength of ferrite in steel. Si can improve the elastic limit, yield strength and yield ratio of steel as well as fatigue strength and fatigue ratio, and to a certain extent can improve strength and improve local corrosion resistance. However, if the Si content is too high, it will have a negative impact on the impact toughness of the heat-affected zone, so the Si content is limited to 0.22-0.49%.

[0021] Mn is a commonly used desulfurizer in steel, and Mn is easy to form MnS inclusions with S. The high-strength and low-toughness hard phases martensite and bainite produced by the segregation of Mn in steel will increase the cracking tendency after welding and have an adverse effect on low-temperature toughness. Therefore, the Mn content should not be too high. Taking into account the strength, toughness and welding performance of the steel plate, the Mn content is set in the range of 1.35-1.48% during the composition design.

[0022] P and S are embrittlement elements in steel and are also very easy to segregate, so the lower their content, the better. They also have a great damage to the low-temperature toughness of steel, but considering the operability of steelmaking, steelmaking cost and meeting the use requirements, the content of P and S is controlled below 0.005% and 0.003% respectively.

[0023] Nb exists in steel as a replacement solute atom, and is easy to combine with C / N, segregate on dislocation lines, and inhibit recrystallization. However, the complete solution temperature of Nb is relatively high, so it is advisable to add it together with V in an appropriate amount, and the ratio of the two is controlled within the range of 0.2 to 0.6. It can improve the strength of steel and improve the toughness of steel. Studies have shown that too high Nb will lose its strengthening effect on steel, so the Nb content is controlled at 1.35 to 1.58%.

[0024] Ni is a weak solid solution strengthening element, and its main function in steel is to increase the supercooling ability of austenite, thereby refining the structure and obtaining a strengthening effect, and has a good influence on impact toughness and brittle transition temperature. Therefore, in the present invention, the content of Ni is controlled to be 0.1-0.19%.

[0025] The V element is located on the left side of iron. The farther away from iron, the easier it is to form more stable carbides. These carbides are difficult to dissolve when heated, and can strongly hinder the growth of austenite grains. Therefore, alloy steel is not easy to overheat when heated for heat treatment, which is conducive to heat treatment operation and can improve the strength and toughness of steel. Secondly, it can fix the C and N elements in steel. By reasonably controlling the content of alloying element V and then accurately controlling the content of V / (C, N) in the alloy, the volume percentage of V / (C, N) in steel is controlled to be no more than 2%. In addition, during the rolling process, the steel plate rolled in the austenite region will produce a certain amount of deformation energy storage, and different degrees of deformation energy storage will have different degrees of influence on the dynamics of carbonitride precipitation in austenite. By increasing the deformation energy storage, the V-rich C and N particles are promoted to precipitate in the high temperature and low temperature stages of the austenite region, respectively, so as to better inhibit austenite recrystallization and prevent the growth of austenite grains. At the same time, the critical nucleation size of carbonitrides in the austenite region, especially in the high temperature region, is greatly reduced, the precipitation strengthening effect of carbonitrides is enhanced, and the strength of steel is increased while ensuring the grain size. Studies have shown that excessive V elements will cause abnormal grain growth, so the V content is controlled within the range of 0.1-0.21%.

[0026] Ca controls the morphology of sulfides in steel and has the effect of inhibiting the formation of MnS by forming CaS. In order to achieve this effect, the Ca content needs to be above 0.0003%. In addition, if the Ca content exceeds 0.005%, the size of the formed CaS is too large, the brittleness also increases, and it is easy to become the starting point of the fracture crack source. Therefore, Ca is limited to 0.0003-0.005%.

[0027] Als is a deoxidizing element in steel. It can effectively refine grains by forming AlN in steel. The appropriate content is 0.015-0.035%.

[0028] The second technical solution of the present invention is to provide a production method of ultra-low temperature high-strength container steel plate and its manufacturing method, through smelting-continuous casting-heating-rolling-heat treatment, adopting a two-stage controlled rolling method combined with normalizing + tempering and normalizing weak cold and hot treatment, to produce a container steel plate with a maximum thickness of 120mm, the structure of the entire thickness section of the produced steel plate is uniform, the steel plate has good strength and toughness matching at 1 / 4 and 1 / 2 thickness, and the steel plate has good welding performance. The specific production method is:

[0029] Smelting: It adopts converter smelting, VOD vacuum treatment and other processes.

[0030] Continuous casting: The key to the process is to control the casting temperature. The casting temperature of the molten steel in the tundish is ≤1506℃. Low-temperature casting is better to refine the original cast structure. In order to control the center segregation and looseness of the continuous casting billet, electromagnetic stirring or continuous casting billet light reduction process is adopted, in which the light reduction rate is controlled at 7% to 12%.

[0031] Heating: The continuous casting slab is sent to the heating furnace for heating. The slab is heated through the preheating section, heating section and soaking section before being taken out of the furnace. When the slab thickness is ≤220mm, the temperature range of the preheating section is 842-856℃; when the slab thickness is greater than 220mm, the temperature range of the preheating section is 756-827℃; the temperature range of the heating section of all thickness slabs is 1180-1250℃; the temperature range of the soaking section is 1250-1280℃. The soaking time of the slab is controlled at 1.2-2.6h. When the heating temperature is lower than 1250℃, the coarse precipitates in the continuous casting slab cannot be dissolved, the austenitization of the steel plate is incomplete, and the final rolling temperature of the first stage cannot be guaranteed; when the heating temperature is higher than 1280℃, it is easy to cause the fine precipitates in the continuous casting slab to dissolve again and cause excessive grain growth.

[0032] Rolling: The rolling process of continuous casting billet adopts two-stage controlled rolling process. The final rolling temperature of the first stage is ≥1026℃, and large deformation is used for rapid rolling in this stage, and the single-pass reduction rate is 8% to 11%, ensuring that the steel plate near the surface undergoes complete dynamic recrystallization; the second stage opening rolling temperature is ≤915℃, and small deformation is used for rapid rolling in this stage, and the single-pass reduction rate is 5% to 7%, ensuring that no recrystallization occurs near the surface of the steel plate.

[0033] Heat treatment: The rolled steel plates are treated with two processes: normalizing + tempering and normalizing weak cooling.

[0034] Among them, for steel plates with a thickness of no more than 60mm, excluding 60mm, the normalizing + tempering heat treatment method is adopted. The normalizing + tempering heat treatment process is as follows: the heating rate is controlled at 1.2-1.4min / mm, the normalizing temperature is 900-920℃, the time in the furnace is 1.9-2.1min / mm, the tempering temperature is 638-651℃, the time in the furnace is 3.1-3.5min / mm, and the plate is taken out of the furnace and air-cooled after reaching the temperature. The total time in the furnace is controlled below 5.5h.

[0035] For 60-120mm thick steel plates, the normalizing weak cold and heat treatment process is adopted. The normalizing weak cold and heat treatment process is that the heat treatment temperature is 860-880℃, the heating rate is 1.4-1.8min / mm, and the steel plates are taken out of the furnace for weak cooling after reaching the temperature, and the total time in the furnace is not more than 4h.

[0036] The beneficial effects of the present invention are:

[0037] In terms of steel grade composition design, the steel plate composition is simple and reasonable. To ensure the low temperature performance of the steel plate, the C and Mn contents in the steel are reasonably controlled to ensure that the segregation of the steel plate is light and the cross-section structure is uniform throughout the thickness; Ca is added to change the shape of inclusions in the steel; to ensure that the steel plate has good strength and toughness, alloy elements such as V, Nb, and Ni are added to the steel to refine the grains, and precipitation strengthening is used to ensure that the steel plate has good comprehensive performance after normalizing heat treatment.

[0038] In terms of manufacturing process, the present invention adopts a heat treatment method of staged rolling and normalizing + tempering and normalizing weak cooling to ensure that the finished steel plate has a uniform grain size and high strength in the entire thickness direction while also having excellent low-temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the metallographic microstructure diagram at 1 / 4 of the thickness of Example 1 of the present invention.

[0040] Figure 2 This is the metallographic microstructure diagram at 1 / 2 thickness of Example 1 of the present invention. DETAILED DESCRIPTION

[0041] The present invention will be further described below by way of examples.

[0042] The embodiment of the present invention carries out smelting-continuous casting-heating-rolling-heat treatment according to the component ratio of the technical solution;

[0043] Continuous casting: The molten steel casting temperature of the tundish is ≤1506℃, and electromagnetic stirring or continuous casting billet light pressing process is adopted.

[0044] The light reduction rate is controlled at 7% to 12%;

[0045] Heating: The continuous casting slab is sent to the heating furnace for heating. The slab is heated through the preheating section, heating section and soaking section before being taken out of the furnace. The temperature range of the slab heating section is 1180-1250℃, and the temperature range of the soaking section is 1250~1280℃. The soaking time of the slab is controlled at 1.2~2.6h;

[0046] Rolling: adopt two-stage controlled rolling process;

[0047] The first stage rolling single pass reduction rate is 8% to 11%, and the final rolling temperature is ≥1026℃; the second stage rolling temperature is ≤915℃, and the single pass reduction rate is 5% to 7%;

[0048] Heat treatment: After rolling, the steel plate is subjected to two processes: normalizing + tempering or normalizing weak cooling.

[0049] Furthermore, during the preheating section, when the slab thickness is ≤220mm, the preheating section temperature range is 842-856°C; when the slab thickness is greater than 220mm, excluding 220mm, the preheating section temperature range is 756-827°C.

[0050] Further; for steel plates with a thickness of ≤60mm, excluding 60mm, the normalizing + tempering heat treatment method is adopted. The specific process is: normalizing temperature 900~920℃, normalizing heating rate 1.2~1.4min / mm, furnace time 1.9~2.1min / mm; tempering temperature 638~651℃, furnace time 3.1~3.5min / mm, after reaching temperature, take out of the furnace and air cool, and the total furnace time is controlled below 5.5h.

[0051] Furthermore; for steel plates with a thickness of 60 to 120 mm, a normalizing weak cold heat treatment process is adopted. The specific process is: the heat treatment temperature is 860 to 880°C, the heating rate is 1.4 to 1.8 min / mm, and the steel is taken out of the furnace for weak cooling after reaching the temperature, and the total time in the furnace is not more than 4 hours.

[0052] The composition of the steel of the present invention is shown in Table 1. The main process parameters of continuous casting and heating of the steel of the present invention are shown in Table 2. The main process parameters of rolling of the steel of the present invention are shown in Table 3. The main process parameters of heat treatment of the steel of the present invention are shown in Table 4. The properties of the steel of the present invention are shown in Table 5. The grain size and non-metallic inclusion test results of the steel of the present invention are shown in Table 6.

[0053] Table 1 Composition of steel according to the present invention (wt%)

[0054]

[0055] Table 2 Main process parameters of continuous casting and heating of steel in the embodiment of the present invention

[0056]

[0057] Table 3 Main process parameters of steel rolling in the embodiment of the present invention

[0058]

[0059] Table 4 Main process parameters of heat treatment of steel in the embodiment of the present invention

[0060]

[0061] Table 5 Properties of steel according to the present invention

[0062]

[0063] Table 6 Grain size and non-metallic inclusion test results of the steel according to the present invention

[0064]

[0065] Note: T is the thickness of the steel plate

[0066] The present invention is applied to produce a high-strength container steel plate suitable for ultra-low temperature and high-pressure conditions, the steel plate thickness range is ≤120mm, the tensile strength at 1 / 4 thickness and 1 / 2 thickness of the steel plate is ≥510MPa; under -70°C conditions, the transverse impact energy KV2 at 1 / 4 thickness and 1 / 2 thickness of the steel plate is ≥260J, and the method for producing medium and thick plates with good strength and toughness properties is achieved, the steel plate has excellent comprehensive performance and low manufacturing cost.

[0067] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.

Claims

1. An ultra-low temperature high-strength container steel plate, characterized in that: The composition of the steel plate is as follows by weight percentage: C: 0.1% to 0.12%, Si: 0.22% to 0.49%, Mn: 1.35% to 1.48%, P: ≤ 0.005%, S: ≤ 0.003%, Nb: 0.04% to 0.06%, Ni: 0.1% to 0.19%, V: 0.1% to 0.21%, Ca: 0.0003% to 0.005%, Als: 0.015% to 0.035%, and the rest is Fe and unavoidable impurities; The Nb / V ratio in the steel plate is 0.2 to 0.6; The thickness of the steel plate is 68-120 mm, and the tensile strength at 1 / 4 and 1 / 2 thickness of the steel plate is ≥510 MPa; at -70°C, the transverse impact energy KV2 at 1 / 4 and 1 / 2 thickness of the steel plate is ≥260 J; The method for manufacturing an ultra-low temperature high-strength container steel plate comprises smelting-continuous casting-heating-rolling-heat treatment; Continuous casting: The molten steel casting temperature of the tundish is ≤1506℃, and electromagnetic stirring or continuous casting billet light reduction process is adopted, in which the light reduction rate is controlled at 7%~12%; Heating: The continuous casting slab is sent to the heating furnace for heating. The slab is heated through the preheating section, heating section and soaking section before being taken out of the furnace. The temperature range of the slab heating section is 1180-1250℃, and the temperature range of the soaking section is 1251~1280℃. The soaking time of the slab is controlled at 1.2~2.6h; Rolling: adopt two-stage controlled rolling process; The first stage rolling single pass reduction rate is 8%~11%, and the final rolling temperature is ≥1026℃; the second stage rolling temperature is 908~915℃, and the single pass reduction rate is 5%~7%; Heat treatment: For steel plates with a thickness of 68~120mm, the normalizing weak cold heat treatment process is adopted. The specific process is: the heat treatment temperature is 860~878℃, the heating rate is 1.4~1.8min / mm, and the plate is taken out of the furnace for weak cooling after reaching the temperature, and the total time in the furnace is not more than 4h.

2. The ultra-low temperature high strength container steel plate according to claim 1, characterized in that: In the steel plate, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15≤0.43%, Pcm={ω(C)+ω(Si) / 30+[ω(Mn)+ω(Cu) +ω(Cr)] / 20+ω(Ni) / 60 +ω(Mo) / 15 +ω(V) / 10 +ω(B)}%≤0.

23.

3. The ultra-low temperature high strength container steel plate according to claim 1, characterized in that: The microstructure of the steel plate is mainly ferrite+pearlite.

4. The ultra-low temperature high strength container steel plate according to claim 1, characterized in that: The volume percentage of V / (C, N) in the microstructure of the steel plate is not more than 2%.

5. The ultra-low temperature high strength container steel plate according to claim 1, characterized in that: When the slab thickness is greater than 220mm, excluding 220mm, the temperature range of the preheating section is 756~827℃.